A method for preventing oxidation and nitridation of the surface of non-oriented high-silicon aluminum-silicon steel strip
By adding Cu and Sn or Sb to non-oriented high-silicon aluminum-silicon steel, the cleanliness and protective atmosphere of steel are controlled, and the problem of nitriding in the heat treatment of non-oriented high-silicon aluminum high-aluminum thin strips is solved, which improves product performance and reduces Production costs and safety risks.
Patent Information
- Application Number
- CN202411124979.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-16
AI Technical Summary
During the heat treatment process of unoriented high-silicon and high-aluminum thin belt products, conventional continuous annealing units cannot effectively prevent nitriding of the steel belt surface, resulting in a decrease in comprehensive performance indicators such as electromagnetic performance and strength, and the use of hydrogen increases production costs and safety risk.
Under the existing continuous annealing unit and protective atmosphere conditions, by adding 0.03% to 0.45% Cu and Sn or Sb of 0.3~1.5 times Cu to high-silicon aluminum-silicon steel, the cleanliness of steel and the dew point of the protective atmosphere ≤- At 30℃, the NOF open flame heating section and H2 content regulation are used to produce high-quality high-silicon aluminum-silicon steel thin strips to prevent nitriding.
It has achieved the production of high-quality high-silicon aluminum-silicon steel thin strips under existing equipment and process conditions, which has improved the electromagnetic and mechanical properties of the product, reduced the use of hydrogen, reduced production costs and improved the operation safety of the unit.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicon steel production, and in particular to a method for preventing oxidation and nitridation of the surface of a non-oriented high-silicon aluminum silicon steel thin strip. Background Art
[0002] With the development of frequency conversion technology and the requirements of low-carbon emission reduction, the development of high-speed high-power density motors such as new energy vehicle drive motors, drones and micro motors is changing with each passing day, and the demand for cold-rolled non-oriented electrical steel high-silicon high-aluminum thin strip products is also increasing. Taking non-oriented high-silicon aluminum thin strip products for new energy vehicle drive motors as an example, the domestic demand in 2023 has exceeded 900,000 tons, and the demand in the future will continue to rise sharply.
[0003] In order to meet the functional characteristics of high-frequency, high-speed and high-power density motors (mainly including low loss, high strength and high magnetic flux density) for new energy vehicle drive motors, high-grade thin strip products usually use Si≥3.0% and Als≥0.60% in the main alloy, and the product thickness specification is below 0.35mm (typical industrial product specifications are 0.30mm, 0.27mm, 0.25mm, 0.23mm, 0.20mm and 0.15mm), and the thickness specification of thin strip products required for new ultra-high speed motors is further reduced.
[0004] At present, the heat treatment of non-oriented silicon steel products usually adopts a multifunctional continuous annealing unit. In order to quickly raise the temperature of the steel strip, NOF open flame heating is often used (the surface of the steel strip is easily oxidized). Due to the limitations of the spacing between the conveyor rollers and the operating tension in the furnace, only thin strips with a thickness of 0.35mm to 0.25mm can be produced. The thinner the thickness, the more unstable the production operation, which directly affects the process stability control and product performance stability, and may even cause serious accidents such as broken strips and shutdowns.
[0005] Non-oriented high-silicon high-aluminum thin strip products are different from conventional non-oriented silicon steel (thickness specification is 0.65mm~0.35mm) products, so the original process equipment and process control for producing non-oriented silicon steel are used, which exposes many problems. In particular, in the finished product heat treatment process, if the conventional large-scale, specialized and multifunctional continuous annealing unit is used, and the process control cannot be adjusted according to the product characteristics and functional requirements, the purpose of producing high value-added competitive products with low cost and high efficiency cannot be achieved.
[0006] As non-oriented high-silicon and high-aluminum thin strip products further develop in the direction of thin specifications, the specific surface area of the steel strip increases, and the surface reaction activity is relatively improved. In addition, due to the increase in the content of high-silicon and high-aluminum elements in the main alloy of the product, under the conditions of traditional continuous annealing protective atmosphere (such as 80%N2+20%H2+dew point control under corresponding conditions), oxidation and nitridation are very likely to occur and an oxidation and nitridation layer inside and outside the matrix is formed, which deteriorates the comprehensive performance indicators of the product such as electromagnetic properties and product strength.
[0007] In order to solve the problem of oxidation and nitridation that is prone to occur during the heat treatment of high-silicon and high-aluminum thin strip products, the protective atmosphere needs to be adjusted during the continuous annealing production process, and the H2 content needs to be continuously increased, or even a full hydrogen atmosphere can be used. However, as the production scale increases, the supply of hydrogen, the matching of auxiliary power, the safety of the overall system operation, and the production cost of the product are all affected. Summary of the invention
[0008] The present invention provides a method for preventing oxidation and nitridation of the surface of a non-oriented high-silicon aluminum-silicon steel strip. Under the conditions of conventional production process equipment for high-grade non-oriented silicon steel products, on the basis of strict control of steel cleanliness, a variety of beneficial elements are added to exert synergistic effects. Under the conditions of existing continuous annealing treatment equipment capacity (the thickness specifications of the produced steel plates are limited due to the NOF open flame heating section) and protective atmosphere (H2 content control capability below 30%), high-quality high-silicon aluminum-silicon steel strip products are produced, which meets the high requirements of the new energy vehicle manufacturing industry for silicon steel strip products and further enhances the market competitiveness of the products.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions:
[0010] A method for preventing oxidation and nitridation of the surface of a non-oriented high-silicon aluminum-silicon steel strip, comprising taking the following measures:
[0011] 1) Add 0.03% to 0.45% Cu and 0.3 to 1.5 Cu Sn or Sb by mass percentage to non-oriented high silicon aluminum silicon steel;
[0012] 2) The production process of non-oriented high-silicon aluminum-silicon steel strip is smelting, continuous casting, ingot heating, hot rolling, cold rolling and continuous annealing; among them, the smelting process controls C≤0.0027%, S≤0.0015%, and N≤0.0016% by mass percentage; continuous annealing adopts a continuous annealing unit with a NOF open flame heating section, the H2 content in the protective atmosphere is 0~30%, and the dew point is ≤-30℃.
[0013] Furthermore, the chemical composition of the non-oriented high-silicon aluminum-silicon steel is, by mass percentage, Si: 3.1%-3.4%, Als: 0.6%-1.0%, Mn: 0.2%-0.4%, P≤0.007%, C≤0.0027%, S≤0.0015%, N≤0.0016%, Cu: 0.03%-0.45%, Sn+Sb: 0.3-1.5Cu, Ni≤0.2% or Ni+Cr≤0.2%, and the rest are Fe and unavoidable impurity elements.
[0014] Furthermore, in the continuous annealing process, the running speed of the cold-rolled steel strip is 90-110 m / min, the heating temperature of the NOF open flame heating section is 1050-1080°C, and the soaking temperature is 930-940°C.
[0015] Furthermore, the finished product thickness of the produced non-oriented high-silicon aluminum-silicon steel strip is 0.25 to 0.35 mm.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] 1) With the increasing market demand for high-silicon aluminum silicon steel thin strip products, the original production lines and production processes cannot meet the production and product quality requirements well. Various silicon steel production enterprises have invested in adding production lines or transforming the original continuous annealing production lines. The present invention is to improve the technology on the basis of the existing production line (continuous annealing unit with NOF open flame heating section) and production process, and produce thin strip products that meet the market requirements without increasing equipment investment and transformation costs;
[0018] 2) The implementation of the present invention is conducive to further improving the electromagnetic properties and mechanical properties of silicon steel strip products, and can be applied to low-loss, high-efficiency, and high-strength silicon steel products;
[0019] 3) After the implementation of the present invention, the hydrogen content can be further reduced in the production process of the original multifunctional continuous annealing unit, thereby reducing the production cost and improving the safety of the unit operation. DETAILED DESCRIPTION
[0020] The method for preventing oxidation and nitridation of the surface of a non-oriented high-silicon aluminum-silicon steel strip according to the present invention comprises taking the following measures:
[0021] 1) Add 0.03% to 0.45% Cu and 0.3 to 1.5 Cu Sn or Sb by mass percentage to non-oriented high silicon aluminum silicon steel;
[0022] 2) The production process of non-oriented high silicon aluminum silicon steel is smelting, continuous casting, ingot heating, hot rolling, cold rolling and continuous annealing; among them, the smelting process controls C≤0.0027%, S≤0.0015%, N≤0.0016% by mass percentage; continuous annealing adopts a continuous annealing unit with a NOF open flame heating section, the H2 content in the protective atmosphere is 0~30%, and the dew point is ≤-30℃.
[0023] Furthermore, the chemical composition of the non-oriented high-silicon aluminum-silicon steel is, by mass percentage, Si: 3.1%-3.4%, Als: 0.6%-1.0%, Mn: 0.2%-0.4%, P≤0.007%, C≤0.0027%, S≤0.0015%, N≤0.0016%, Cu: 0.03%-0.45%, Sn+Sb: 0.3-1.5Cu, Ni≤0.2% or Ni+Cr≤0.2%, and the rest are Fe and unavoidable impurity elements.
[0024] Furthermore, in the continuous annealing process, the running speed of the cold-rolled steel strip is 90-110 m / min, the heating temperature of the NOF open flame heating section is 1050-1080°C, and the soaking temperature is 930-940°C.
[0025] Furthermore, the finished product thickness of the produced non-oriented high-silicon aluminum-silicon steel strip is 0.25 to 0.35 mm.
[0026] In order to prevent the surface of non-oriented high-silicon aluminum-silicon steel strip from being oxidized and nitrided, the present invention adopts the following technical measures in terms of steel grade composition and production process design:
[0027] 1. Strictly control the cleanliness of steel; control C in steel ≤ 0.0027%, ensure that the product is not decarburized during the heat treatment process, reduce the involvement of oxidizing atmosphere in wet atmosphere (no humidification, dry atmosphere annealing, dew point ≤ -30℃), reduce the magnetic aging of the product, ensure that the product is made into functional components (such as motor stators and rotors) and operate stably under relatively high temperature (such as motor operating temperature rise) conditions for a long time, reduce the lattice distortion of recrystallization structure during heat treatment, and reduce the involvement of oxygen and nitrogen. Control S in steel ≤ 0.0015%, reduce sulfides and precipitates, reduce the lattice distortion of recrystallization structure during heat treatment, reduce the involvement of oxygen and nitrogen, reduce the impact of sulfur on electromagnetic properties, and reduce the "catalyst effect" of sulfur on the surface of thin strips. By reducing nitrides and precipitates, the lattice distortion of recrystallization structure is reduced, and the impact of nitrogen on electromagnetic properties is reduced.
[0028] 2. Add an appropriate amount of copper element and control the Cu content in the steel to 0.030% ~ 0.45%, so as to give full play to the corrosion resistance of copper element to iron-based materials; and in the heat treatment process, copper is enriched on the surface under the promotion of high silicon and high aluminum, which can reduce the oxidation and nitridation of the surface layer of the strip steel (containing iron, high silicon and aluminum) under the condition of large surface ratio.
[0029] 3. Add grain boundary segregation elements, that is, add Sn and / or Sb elements. These elements have similar functions and effects and can be added in combination or separately to control the total addition amount. Sn is used as an example for explanation below. The Sn content needs to be matched with the copper content, that is, the Sn content is controlled within the range of 0.3 to 1.5 times the Cu content. The grain boundary segregation characteristics of Sn are utilized to reduce the precipitates formed by residual harmful elements in the steel to pin the grain boundaries, improve the organization and texture, eliminate the adverse effects of copper and other added elements required for other processes on the magnetic properties; strengthen the grain boundaries, increase product strength and improve processability. In the present invention, another important function of Sn is to prevent copper from segregating and enriching at the grain boundaries. After copper is added to the steel of the present invention, copper is easy to aggregate at the grain boundaries, which can easily cause softening of the grain boundaries (melting of the high-temperature grain boundary copper-enriched zone) and copper brittleness and edge cracking during the production of hot-rolled steel strips.
[0030] In the present invention, the process control from continuous casting to cold rolling of non-oriented high-silicon aluminum-silicon steel thin strip products is the same as the conventional production process control. It only needs to implement the above measures on this basis, and under the process conditions of using the existing continuous annealing unit with a NOF open flame heating section and regulating the H2 content of the existing protective atmosphere within the range of 0 to 30%, and the dew point ≤-30°C, it is possible to produce thin strip products with a thickness of 0.25 to 0.35 mm. The product has excellent surface quality, no internal and external nitriding and oxidation defects, and excellent electromagnetic properties.
[0031] In order to more intuitively embody the present invention, the embodiments of the present invention are further described in conjunction with examples. The following examples are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any technical solution that can be obviously obtained by a person skilled in the art within the technical scope disclosed in the present invention, including simple changes or equivalent replacements, is within the protection scope of the present invention.
[0032]
Example 1
[0033] In this example, by using Comparative Example 1 and Example 1, a typical non-oriented high-silicon aluminum-silicon steel strip product 35NV1800 (low-loss type) is taken as an example to compare the chemical composition, production process and product performance of the product.
[0034] In Comparative Example 1, the chemical composition of the non-oriented high-silicon aluminum-silicon steel strip is, by mass percentage, C: 0.0027%, Si: 3.21%, Als: 0.68%, Mn: 0.351%, P: 0.009%, S: 0.0012%, N: 0.0017%, and the remainder is Fe and unavoidable impurity elements.
[0035] In Comparative Example 1, the molten steel is subjected to smelting, continuous casting, ingot heating, hot rolling and cold rolling to obtain a cold-rolled steel strip. The running speed of the cold-rolled steel strip in the continuous annealing production line is 100 m / min, the heating temperature of the NOF open flame heating section is 1050°C, the average heating temperature is 940°C, the H2 content in the protective atmosphere in the furnace is 20%, and the dew point is controlled at -10°C.
[0036] The finished product properties of the non-oriented high-silicon aluminum-silicon steel strip produced in Comparative Example 1 are: iron loss P10 / 400 is 17.3W / kg, magnetic induction B5000 is 1.67T, yield strength Rp0.2 is 390MPa, and the product surface is light gray and matte.
[0037] In Example 1, the chemical composition of the non-oriented high-silicon aluminum-silicon steel strip is, by mass percentage, Si: 3.19%, Als: 0.71%, Mn: 0.345%, P: 0.005%, C: 0.0021%, S: 0.0009%, N: 0.0013%, Cu: 0.11%, Sn: 0.035%, and the remainder is Fe and unavoidable impurity elements.
[0038] In Example 1, the molten steel is subjected to smelting, continuous casting, ingot heating, hot rolling and cold rolling to obtain a cold-rolled steel strip. The running speed of the cold-rolled steel strip in the continuous annealing production line is 100 m / min, the heating temperature of the NOF open flame heating section is 1050°C, the soaking temperature is 940°C, the H2 content in the protective atmosphere in the furnace is 20%, and the dew point is controlled at -30°C.
[0039] The finished product properties of the non-oriented high-silicon aluminum-silicon steel strip produced in Example 1 are: iron loss P10 / 400 is 16.5W / Kg, magnetic induction B5000 is 1.68T, yield strength Rp0.2 is 400MPa, the product surface is silvery white and bright, and there is no oxidation and nitridation layer.
[0040]
Example 2
[0041] In this example, by using Comparative Example 2 and Example 2, a typical non-oriented high-silicon aluminum-silicon steel strip product 35NVP1900 (high magnetic induction type) is taken as an example to compare the chemical composition, production process and product performance of the product.
[0042] In Comparative Example 2, the chemical composition of the non-oriented high-silicon aluminum-silicon steel strip is, by mass percentage, C: 0.0031%, Si: 3.25%, Als: 0.58%, Mn: 0.323%, P: 0.008%, S: 0.0013%, N: 0.0020%, and the remainder is Fe and unavoidable impurity elements.
[0043] In Comparative Example 2, the molten steel is subjected to smelting, continuous casting, ingot heating, hot rolling and cold rolling to obtain a cold-rolled steel strip. The running speed of the cold-rolled steel strip in the continuous annealing production line is 105 m / min, the heating temperature of the NOF open flame heating section is 1060°C, the average heating temperature is 930°C, the H2 content in the protective atmosphere in the furnace is 20%, and the dew point is controlled at -10°C.
[0044] The finished product properties of the non-oriented high-silicon aluminum-silicon steel strip produced in Comparative Example 2 are: iron loss P10 / 400 is 17.5 W / kg, magnetic induction B5000 is 1.68 T, yield strength Rp0.2 is 385 MPa, and the product surface is light gray and matte.
[0045] In Example 2, the chemical composition of the non-oriented high-silicon aluminum-silicon steel strip is, by mass percentage, Si: 3.15%, Als: 0.63%, Mn: 0.325%, P: 0.007%, C: 0.0018%, S: 0.0008%, N: 0.0012%, Cu: 0.045%, Sn: 0.055%, and the remainder is Fe and unavoidable impurity elements.
[0046] In Example 2, the molten steel is subjected to smelting, continuous casting, ingot heating, hot rolling and cold rolling to obtain a cold-rolled steel strip. The running speed of the cold-rolled steel strip in the continuous annealing production line is 105 m / min, the heating temperature of the NOF open flame heating section is 1060°C, the soaking temperature is 930°C, the H2 content in the protective atmosphere in the furnace is 15%, and the dew point is controlled at -35°C.
[0047] The finished product performance of the non-oriented high-silicon aluminum-silicon steel strip produced in Example 2 is: iron loss P10 / 400 is 16.5W / Kg, magnetic induction B5000 is 1.69T, yield strength Rp0.2 is 410MPa, the product surface is silvery white and bright, and there is no oxidation and nitridation layer.
[0048]
Example 3
[0049] In this example, by using Comparative Example 3 and Example 3, a typical non-oriented high-silicon aluminum-silicon steel strip product 30NVPS1500 (high magnetic induction and high strength type) is taken as an example to compare the chemical composition, production process and product performance of the product.
[0050] In Comparative Example 3, the chemical composition of the non-oriented high-silicon aluminum-silicon steel strip is, by mass percentage, C: 0.0032%, Si: 3.31%, Als: 0.88%, Mn: 0.227%, P: 0.006%, S: 0.0012%, N: 0.0017%, Ni: 0.120% (strengthening element), and the remainder is Fe and unavoidable impurity elements.
[0051] In Comparative Example 3, the molten steel is subjected to smelting, continuous casting, ingot heating, hot rolling and cold rolling to obtain a cold-rolled steel strip. The running speed of the cold-rolled steel strip in the continuous annealing production line is 95 m / min, the heating temperature of the NOF open flame heating section is 1080°C, the average heating temperature is 930°C, the H2 content in the protective atmosphere in the furnace is 20%, and the dew point is controlled at -10°C.
[0052] The finished product properties of the non-oriented high-silicon aluminum-silicon steel strip produced in Comparative Example 3 are: iron loss P10 / 400 is 14.15 W / kg, magnetic induction B5000 is 1.658 T, yield strength Rp0.2 is 445 MPa, and the product surface is dark gray and matte.
[0053] In Example 3, the chemical composition of the non-oriented high-silicon aluminum-silicon steel strip is, by mass percentage, Si: 3.29%, Als: 0.91%, Mn: 0.251%, P: 0.006%, C: 0.0022%, S: 0.0006%, N: 0.0011%, Cu: 0.135%, Sn: 0.145%, Ni: 0.118 (strengthening element), and the remainder is Fe and unavoidable impurity elements.
[0054] In Example 3, the molten steel is subjected to smelting, continuous casting, ingot heating, hot rolling and cold rolling to obtain a cold-rolled steel strip. The running speed of the cold-rolled steel strip in the continuous annealing production line is 95 m / min, the heating temperature of the NOF open flame heating section is 1075°C, the soaking temperature is 930°C, the H2 content in the protective atmosphere in the furnace is 15%, and the dew point is controlled at -35°C.
[0055] The finished product properties of the non-oriented high-silicon aluminum-silicon steel strip produced in Example 3 are: iron loss P10 / 400 is 13.71W / Kg, magnetic induction B5000 is 1.668T, yield strength Rp0.2 is 450MPa, the product surface is silvery white and bright, and there is no oxidation and nitridation layer.
[0056]
Example 4
[0057] In this example, by using Comparative Example 4 and Example 4, a typical non-oriented high-silicon aluminum-silicon steel strip product 25NVPS1300 (high magnetic induction and high strength type) is taken as an example to compare the chemical composition, production process and product performance of the product.
[0058] In Comparative Example 4, the chemical composition of the non-oriented high-silicon aluminum-silicon steel strip is, by mass percentage, C: 0.0028%, Si: 3.32%, Als: 0.85%, Mn: 0.247%, P: 0.006%, S: 0.0013%, N: 0.0018%, Ni+Cr: 0.160% (strengthening elements), and the balance is Fe and unavoidable impurity elements.
[0059] In Comparative Example 4, the molten steel is subjected to smelting, continuous casting, ingot heating, hot rolling and cold rolling to obtain a cold-rolled steel strip. The running speed of the cold-rolled steel strip in the continuous annealing production line is 90 m / min, the heating temperature of the NOF open flame heating section is 1055°C, the average heating temperature is 935°C, the H2 content in the protective atmosphere in the furnace is 30%, and the dew point is controlled at -30°C.
[0060] The finished product properties of the non-oriented high-silicon aluminum-silicon steel strip produced in Comparative Example 4 are: iron loss P10 / 400 is 12.85 W / kg, magnetic induction B5000 is 1.651 T, yield strength Rp0.2 is 450 MPa, and the product surface is dark gray and matte.
[0061] In Example 4, the chemical composition of the non-oriented high-silicon aluminum-silicon steel strip is, by mass percentage, Si: 3.31%, Als: 0.87%, Mn: 0.255%, P: 0.006%, C: 0.0018%, S: 0.0005%, N: 0.0012%, Cu: 0.25%, Sn: 0.115%, Ni+Cr: 0.170% (strengthening elements), and the balance is Fe and unavoidable impurity elements.
[0062] In Example 4, the molten steel is subjected to smelting, continuous casting, ingot heating, hot rolling and cold rolling to obtain a cold-rolled steel strip. The running speed of the cold-rolled steel strip in the continuous annealing production line is 90 m / min, the heating temperature of the NOF open flame heating section is 1055°C, the soaking temperature is 935°C, the H2 content in the protective atmosphere in the furnace is 20%, and the dew point is controlled at -30°C.
[0063] The finished product properties of the non-oriented high-silicon aluminum-silicon steel strip produced in Example 4 are: iron loss P10 / 400 is 12.51W / Kg, magnetic induction B5000 is 1.665T, yield strength Rp0.2 is 455MPa, the product surface is silvery white and bright, and there is no oxidation and nitridation layer.
[0064] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preventing oxidation and nitridation of the surface of non-oriented high-silicon aluminum-silicon steel strip, characterized in that: This includes taking the following measures: 1) The chemical composition of non-oriented high silicon aluminum silicon steel is Si: 3.29% ~ 3.4%, Als: 0.91% ~ 1.0%, Mn: 0.2% ~ 0.4%, P ≤ 0.007%, C ≤ 0.0027%, S ≤ 0.0015%, N ≤ 0.0016%, Cu: 0.11% ~ 0.45%, Sn + Sb: 0.3 ~ 1.5Cu, Ni 0.118% ~ 0.2% or Ni + Cr 0.17% ~ 0.2%, and the rest is Fe and unavoidable impurity elements; 2) The production process of non-oriented high-silicon aluminum-silicon steel strip is smelting, continuous casting, ingot heating, hot rolling, cold rolling and continuous annealing; among them, the smelting process controls C≤0.0027%, S≤0.0015%, and N≤0.0016% by mass percentage; the continuous annealing adopts a continuous annealing unit with a NOF open flame heating section, the H2 content in the protective atmosphere is 0-30%, and the dew point is ≤-30℃; in the continuous annealing process, the running speed of the cold-rolled steel strip is 90-110m / min, the heating temperature of the NOF open flame heating section is 1050-1080℃, and the soaking temperature is 930-940℃; The finished product thickness of the produced non-oriented high-silicon aluminum-silicon steel thin strip is 0.25-0.35 mm.