A method for recovering insulation and sealing of end joints of Paschen test magnets
By using multi-layer wrapping technology and heating curing treatment on the magnet end joints, the insulation and sealing treatment problems of exposed parts are solved, efficient insulation and sealing effects are achieved, and the safe operation and recovery of the magnet are ensured.
Patent Information
- Application Number
- CN202411114146.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-14
AI Technical Summary
When performing a Paxing test on the magnet end connector, how to insulate and seal the exposed parts without damaging the original insulation and magnet connectors and achieve recovery is a technical challenge.
Use G10 sleeve to cover the helium tube, use fine granular sandpaper to polish the insulating finishing area, and gradually wrap the polyimide belt, self-melting belt, resin, glass ribbon, polyethylene film and silicone belt to form a multi-layer insulation and sealing structure , and heat curing through heating belts to ensure insulation and sealing effect.
Effective insulation and sealing of the end joints of the magnets is achieved, ensuring safety and later recovery during the test process, and the use of materials is low and simple to operate, meeting the safe operation requirements of superconducting magnets.
Smart Images

Figure CN118645352B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of insulation and sealing recoverable treatment of magnet end joints, and in particular relates to an insulation and sealing recoverable treatment method for a Paschen test magnet end joint. Background Art
[0002] The Central Solenoid Model Coil (CSMC) is an important subunit of the superconducting magnet research system of the Critical Research Facility for Fusion Reactor Host (CRAFT). The CSMC consists of two Nb3Sn magnets and three NbTi magnets in series. Before assembly, each magnet needs to undergo a Paschen test, which requires applying a high voltage DC2kV_1min at four levels of vacuum pressure of 1\10\100\1000Pa, and the leakage current is less than 20uA. The Paschen test is used to verify whether the insulation and sealing of the magnet meet the requirements of the later experimental operation, and is a strict electrical performance test.
[0003] Since the joints at both ends of a single magnet are partially exposed outside the magnet insulation layer after vacuum pressure impregnation (VPI), they are used for subsequent connection with other magnets and current leads. Therefore, when a single magnet is subjected to Paschen test, the joints exposed outside the magnet insulation layer must be insulated and sealed. After the test, they need to be removed and restored. Therefore, how to insulate, seal and restore the end joints of the Paschen test magnet is particularly important. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for recoverable treatment of insulation and sealing of the end joint of a Paschen test magnet. The method is used to guide the insulation and sealing treatment of the exposed part of the end joint during the Paschen test of a single magnet in a CSMC device. The invention provides a recoverable treatment method without damaging the original insulation and magnet joint.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] A method for recovering the insulation and sealing of a Paschen test magnet end joint comprises the following steps:
[0007] Step 1: Use a G10 sleeve to cover the helium tube of the magnet end joint. The diameter of the G10 sleeve is flush with the armor on the lower end of the helium tube. The total length of the G10 sleeve is N.
[0008] Step 2: Use fine-grain sandpaper to polish the surface of the insulation finishing area;
[0009] Step 3: Use a 0.05 mm thick and 20 mm wide polyimide tape to wrap from the polished insulation tail area toward the helium tube and end at the N / 2 position of the G10 sleeve to form a polyimide layer;
[0010] Step 4, half-wrap with self-fusing tape to wrap the polyimide layer to form a self-fusing tape layer;
[0011] Step 5, evenly coating the upper surface of the self-fusing tape layer with resin to cover the self-fusing tape layer to form a resin coating layer;
[0012] Step 6: Use glass ribbon to half-wrap and wet-wrap, wrap the resin coating layer, and fill the irregular and complex structure positions with glass silk. Repeat this operation 9 times to form a glass ribbon wet-wrap layer;
[0013] Step 7, half-wrap the glass ribbon wet wrapping layer with polyethylene film to form a polyethylene film layer;
[0014] Step 8, dry wrapping with a 0.1 mm thick and 2 mm wide glass ribbon, half-folding once, and fully covering the polyethylene film layer to form a first glass ribbon dry wrapping layer;
[0015] Step 9, wrapping with silicone tape flatly to completely cover the first glass ribbon dry wrapping layer to form a silicone tape layer;
[0016] Step 10, dry wrap with a 0.1 mm thick and 2 mm wide glass ribbon, half-fold once, and fully cover the silicone tape layer to form a second glass ribbon dry wrapping layer;
[0017] Step 11: Wrap the second glass ribbon dry wrap layer with a heating tape to form a heating layer and heat it at a temperature of 65° C. for 8 hours.
[0018] Furthermore, the steps 3-4, 6-8 and 10 are half-fold wrapping processes, and steps 9 and 11 are flat wrapping processes.
[0019] The beneficial effects of the present invention are:
[0020] (1) The polyimide tape, self-fusing tape, polyethylene film, silicone tape, heating tape, etc. used in the treatment method of the present invention are all materials that are easily available on the market, have low costs, and have economic advantages.
[0021] (2) The treatment method of the present invention is simple, has good insulation and sealing effects on the metal segments at the exposed parts of the joints, is easy to operate, is easy for on-site construction personnel to understand, and has strong operability. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The present invention is a principle block diagram of a method for recoverable treatment of insulation and sealing of a Paschen test magnet end joint. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0024] like Figure 1 As shown, a principle block diagram of a method for recoverable insulation and sealing of a Paschen test magnet end joint of the present invention is provided. A G10 sleeve with a length of N is used to cover the helium tube of the end joint. The diameter of the G10 sleeve is just flush with the armor of the lower end surface of the helium tube, which is convenient for later insulation wrapping and sealing treatment; the surface of the insulation tail area is polished with sandpaper to increase the roughness, and a 0.05mm thick and 20mm wide polyimide tape is half-lapped and wrapped from the insulation tail area at the polishing position, and wrapped upward until N / 2 of the G10 sleeve to form a polyimide layer; a self-fusing tape is half-lapped and wrapped to wrap the polyimide layer to form a self-fusing tape layer; resin is applied to the upper surface of the self-fusing tape to cover the self-fusing tape layer to form a resin coating layer; a 0.05mm thick and 20mm wide polyimide tape is used to wrap the polyimide layer to form a self-fusing tape layer. 1mm, 15mm wide glass ribbon wet wrap half-lap, wrap the resin coating layer, fill the irregular complex structure position with glass silk, repeat this operation 9 times to form a 2mm thick glass ribbon wet wrapping layer; half-lap with polyethylene film, fully cover to form a polyethylene film layer; dry wrap with 0.1mm thick and 2mm wide glass ribbon, half-lap once, fully cover to form a glass ribbon dry wrapping layer; flat wrap with silicone tape, fully cover to form a silicone tape layer; dry wrap with 0.1mm thick and 2mm wide glass ribbon, half-lap once, fully cover to form a glass ribbon dry wrapping layer; finally, heat with a heating tape at 65℃ to accelerate the curing of the resin glue, and the heating time is 8hrs. This method is used to guide the insulation of the quench detection line of the superconducting magnet under vacuum pressure impregnation to avoid damage, and provide guarantee for the later Paschen test and safe operation of the magnet.
[0025] Furthermore, after sanding the insulation finishing area, the entire treated area surface is cleaned with alcohol to remove dust and impurities.
[0026] Furthermore, the G10 is a composite material made of glass fiber cloth and epoxy resin, and has good insulation performance and corrosion resistance and low temperature resistance.
[0027] Furthermore, the insulation finishing area has a "step" gradient, and this finishing method is used for overlapping of subsequent insulation wrapping to ensure the continuity of the insulation at the transition position.
[0028] Furthermore, the self-fusing tape is a kind of adhesive silicone tape that can withstand a temperature of 150°C. The self-fusing tape has strong adhesion and has a very good sealing effect, and is also convenient for later disassembly and restoration.
[0029] Furthermore, the resin is a special resin that can serve for a long time at low temperatures (-269°C), does not crack at low temperatures, and participates in the insulation component of superconducting magnets.
[0030] Furthermore, the glass ribbon wet wrapping is to immerse a 0.1 mm thick and 15 mm wide glass ribbon in the resin, take it out after it is completely moistened, and half-wrap it 10 times to form an insulating layer with a thickness of 2 mm.
[0031] Furthermore, the polyethylene film has no adhesion to the resin and can withstand a high temperature of 150° C. The polyethylene film tightly wraps the wet-wound insulation layer to prevent the resin of the glass ribbon from penetrating outward after wet-wounding and sticking to the next winding layer.
[0032] Furthermore, the silicone tape has a thickness of 1-2 mm and is used for isolating and transferring heat of the heating tape to ensure uniform heating. The glass tape is dry-wrapped twice. The first glass tape dry-wrapping is used for direct contact between the polyethylene film and the silicone tape to prevent the polyethylene film from being damaged and the resin from sticking to the silicone tape. The second glass tape dry-wrapping is used to avoid direct contact between the heating tape and the silicone tape. The ignition point of the glass tape is very high, which greatly reduces the risk of insulation burns caused by heating tape failure.
[0033] Furthermore, the heating belt is a glass fiber heating belt equipped with a temperature control device, the heating temperature is set to 65°C, the temperature of the entire heating process is controlled at 60-70°C, the heating time is 8 hours, and the heating purpose is to quickly cure the resin.
[0034] Example
[0035] The present invention treats 5 single magnets and 10 end joint positions of the CSMC device according to the processing method, and completes the Paschen test of the magnet at room temperature. The test results are shown in Table 1 (unit: nA). The leakage current is only at the nA level in the test DC2kV_1min, which is far lower than the design requirement of 20uA, meeting the experimental safety operation requirements, completing the key technical node tasks of the device, achieving good benefits, and providing guarantee for the safe and stable operation of superconducting magnets.
[0036] Table 1
[0037]
[0038] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for recovering the insulation and sealing of the end joint of a Paschen test magnet, characterized in that: The method comprises: Step 1, use a G10 sleeve to cover the helium tube of the end joint of the magnet, the diameter of the G10 sleeve is flush with the armor of the lower end surface of the helium tube, the total length of the G10 sleeve is N, and the G10 sleeve is a composite material synthesized from glass fiber cloth and epoxy resin; Step 2: Use fine-grain sandpaper to polish the surface of the insulation finishing area; Step 3: Use a 0.05 mm thick and 20 mm wide polyimide tape to wrap from the polished insulation tail area toward the helium tube and end at the N / 2 position of the G10 sleeve to form a polyimide layer; Step 4, half-wrap with self-fusing tape to wrap the polyimide layer to form a self-fusing tape layer; Step 5, evenly coating the upper surface of the self-fusing tape layer with resin to cover the self-fusing tape layer to form a resin coating layer, wherein the resin is a resin that has been in service for a long time at a low temperature of -269°C; Step 6, half-fold and wet-wrap with glass ribbon, wrap the resin coating layer, fill the irregular and complex structure position with glass silk, repeat the operation of step 6 9 times to form a glass ribbon wet-wrap layer, wherein the glass ribbon wet-wrap includes soaking a glass ribbon with a thickness of 0.1 mm and a width of 15 mm in the resin, taking it out after it is completely moistened, half-folding and wrapping 10 times, and forming an insulating layer with a thickness of 2 mm; Step 7, half-wrap the glass ribbon wet wrapping layer with polyethylene film to form a polyethylene film layer; Step 8, dry wrapping with a 0.1 mm thick and 2 mm wide glass ribbon, half-folding once, and fully covering the polyethylene film layer to form a first glass ribbon dry wrapping layer; Step 9, wrapping with silicone tape flatly to completely cover the first glass ribbon dry wrapping layer to form a silicone tape layer; Step 10, dry wrap with a 0.1 mm thick and 2 mm wide glass ribbon, half-fold once, and fully cover the silicone tape layer to form a second glass ribbon dry wrapping layer; Step 11: Wrap the second glass ribbon dry wrap layer with a heating tape to form a heating layer and heat it at a temperature of 65° C. for 8 hours.
2. A method for recovering insulation and sealing of a Paschen test magnet end joint according to claim 1, characterized in that: The steps 3-4, 6-8 and 10 are half-fold wrapping processes, and steps 9 and 11 are flat wrapping processes.
3. A method for recovering insulation and sealing of a Paschen test magnet end joint according to claim 1, characterized in that: The insulation finish region includes a step-like gradient.
4. A method for recovering insulation and sealing of a Paschen test magnet end joint according to claim 1, characterized in that: The self-fusing tape is a sticky silicone tape and is resistant to high temperatures of 150°C.
5. A method for recovering insulation and sealing of a Paschen test magnet end joint according to claim 1, characterized in that: The polyethylene film has no adhesion to the resin and is resistant to high temperatures of 150°C.
6. A method for recovering insulation and sealing of a Paschen test magnet end joint according to claim 1, characterized in that: The thickness of the silicone tape is 1-2 mm and is used for isolating and transferring heat of the heating tape; the dry wrapping of the first glass tape is used for direct contact between the polyethylene film and the silicone tape, and the dry wrapping of the second glass tape is used for avoiding direct contact between the heating tape and the silicone tape.
7. A method for recovering insulation and sealing of a Paschen test magnet end joint according to claim 1, characterized in that: The heating belt is a glass fiber heating belt and is equipped with a temperature control device.