A high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as negative electrode

By using composite materials of lithium vanadate/g-C3N4 and activated carbon or biomass carbon in lithium-ion capacitors, the cyclic stability and safety performance of the capacitor are solved, the capacity and rate performance are improved, the production cost is reduced, and the production cost is achieved High energy density and fast charging and discharging effects.

CN118645376BActive Publication Date: 2024-11-19GUORONG INTELLIGENT TECH (NANJING) CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411102875.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-19
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The problems of poor cycle stability, poor safety performance, high production cost and poor rate performance of lithium-ion capacitors limit their wide commercial application in practical applications.

Method used

Lithium vanadate/g-C3N4 is used as the negative electrode material, combined with activated carbon or biomass carbon as the positive electrode material, and organic solutions of lithium hexafluorophosphate, vinyl carbonate, diethyl carbonate and fluorovinyl carbonate are used as the electrolyte, and hydrothermal treatment and carbonization are used. Process and prepare negative electrode materials to improve the cyclic stability and capacity of the capacitor.

Benefits of technology

The cyclic stability and specific capacity of lithium ion capacitors are significantly improved, the accumulation and volume expansion problems of lithium vanadate are reduced, the safety performance and production efficiency of the capacitors are enhanced, and the effects of high energy density and fast charging and discharge are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118645376B_ABST
    Figure CN118645376B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of electrochemistry, and specifically relates to a high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as a negative electrode, comprising a positive electrode material, a negative electrode material and an electrolyte; wherein the negative electrode material is lithium vanadate / g-C3N4, the electrolyte is an organic electrolyte capable of conducting lithium ions, and the positive electrode material is a carbon material capable of reversible adsorption / desorption of anions in the organic electrolyte. The high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as a negative electrode provided by the present invention has a high capacity and good cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electrochemistry, and in particular relates to a high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as a negative electrode. Background Art

[0002] As a new energy storage technology, lithium-ion capacitors have attracted much attention in recent years and are gradually becoming practical. The emergence of this device stems from the continuous pursuit and improvement of traditional energy storage technology. Traditional batteries have many problems such as insufficient energy density, slow charging and discharging speed, and short cycle life, which limit their development in modern scientific and technological applications. The emergence of lithium-ion capacitors provides a new solution to these problems.

[0003] As people's demand for clean and renewable energy continues to increase, the research and development of lithium-ion capacitors has become a hot topic. It not only provides high energy density, but also has the advantages of fast charging and discharging, long cycle life, etc., which makes it have broad application prospects in electric vehicles, wearable devices, smart homes and other fields. In the field of electric vehicles, the high energy density and fast charging characteristics of lithium-ion capacitors can effectively improve the driving range and charging efficiency of electric vehicles, and promote the further development of the electric vehicle market.

[0004] However, lithium-ion capacitors still face some challenges. For example, their manufacturing cost is relatively high, which to some extent limits their large-scale commercialization process. At the same time, the safety and stability of lithium-ion capacitors are also key issues that need to be continuously strengthened, especially in high temperature environments or when they are damaged by external factors, safety accidents are prone to occur. The most important thing is that after long-term use, lithium-ion capacitors will have the problem of capacity attenuation, resulting in a decrease in their energy storage capacity. Therefore, the research and development of lithium-ion capacitors still needs to continuously invest energy and resources to solve the technical difficulties they face in practical applications and promote their wider commercial applications. Summary of the invention

[0005] The present invention mainly provides a high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as the negative electrode to solve the problems of poor cycle stability, poor safety performance, high production cost and poor rate performance of the above capacitors. The technical solution is as follows:

[0006] A high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as a negative electrode comprises a positive electrode, a negative electrode and an electrolyte capable of conducting lithium ions; the positive electrode adopts a carbon material capable of reversible adsorption and desorption of anions in an organic electrolyte as the positive electrode material; the negative electrode adopts lithium vanadate / g-C3N4 as the negative electrode material.

[0007] Furthermore, the carbon material is one or more of activated carbon or biochar.

[0008] Furthermore, the biomass charcoal is one or more of rice husk charcoal, wheat bran charcoal or peanut charcoal.

[0009] Furthermore, the electrolyte is an organic solution of lithium hexafluorophosphate, ethylene carbonate, diethyl carbonate and fluoroethylene carbonate.

[0010] Furthermore, the preparation of the negative electrode material comprises the following steps:

[0011] (1) dissolving ammonium metavanadate and lithium hydroxide in deionized water, and then adding g-C3N4 into the reaction system and mixing and dispersing the mixture thoroughly to obtain a dispersion;

[0012] (2) subjecting the obtained dispersion to hydrothermal treatment;

[0013] (3) After the hydrothermal treatment, the precipitate is collected by centrifugation, washed and dried to obtain the negative electrode material.

[0014] Furthermore, the molar ratio of the ammonium metavanadate to the lithium hydroxide is 1:(15-20); the mass of the g-C3N4 is 5%-20% of the total mass of the ammonium metavanadate and the lithium hydroxide.

[0015] Furthermore, the sufficient mixing and dispersion in step (1) is performed by first stirring for 0.5 to 2 hours and then ultrasonicating for 1 to 4 hours.

[0016] Furthermore, the temperature of the hydrothermal treatment in step (2) is 160-200° C., and the time is 2-4 hours.

[0017] Furthermore, the preparation of the biochar includes the following steps: crushing the biomass into powder, then adding the powder into a potassium hydroxide solution and stirring for 8 to 16 hours; after centrifugal drying, heating to 700 to 1000°C at a rate of 5°C / min in an argon atmosphere, keeping warm for 2 to 8 hours to obtain carbonized powder; treating the carbonized powder with hydrochloric acid for 12 to 18 hours, filtering, washing with water to neutrality, and drying to obtain biochar.

[0018] Further, the powder is added to a 0.5-2.0 M potassium hydroxide solution, and the pH value of the system is adjusted to 8-11; the carbonized powder is treated with 0.5-2.0 M hydrochloric acid, and the pH value of the system is adjusted to 3-4.

[0019] Based on the above scheme, the present invention has the following advantages:

[0020] The present invention adopts lithium vanadate / g-C3N4 as the negative electrode; the compound in which lithium ions can be reversibly embedded at a large current density is used as the negative electrode material, so it has very good stability and cycle performance.

[0021] The composite g-C3N4 in the negative electrode material of the present invention can reduce the accumulation of lithium vanadate and the volume expansion problem of lithium vanadate, thereby solving the problem of poor cycle stability of high-energy lithium-ion hybrid capacitors.

[0022] The lithium vanadate of the present invention is compounded with g-C3N4, and compared with the lithium vanadate not compounded with g-C3N4, the capacity of the obtained capacitor is significantly higher and the cycle stability is stronger.

[0023] The lithium vanadate / g-C3N4 composite negative electrode material of the present invention and biochar such as wheat bran charcoal and rice husk charcoal can synergistically improve the specific capacity and cycle stability of lithium ion capacitors. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a scanning electron microscope photograph of Example 1.

[0025] Figure 2 This is the X-ray diffraction pattern of Example 1.

[0026] Figure 3 This is a scanning electron microscope photograph of Example 2.

[0027] Figure 4 This is a scanning electron microscope photograph of Example 3.

[0028] Figure 5 It is the nitrogen adsorption-desorption curve of Example 3.

[0029] Figure 6 This is a scanning electron microscope photograph of Comparative Example 1.

[0030] Figure 7 Test case 1 at 1A g -1 Efficiency-specific capacity curve of cyclic charge and discharge under current density.

[0031] Figure 8 Test case 2 at 1A g -1 Efficiency-specific capacity curve of cyclic charge and discharge under current density.

[0032] Fig. 9 Test case 3 at 1A g -1 Efficiency-specific capacity curve of cyclic charge and discharge under current density.

[0033] Fig.10 Test case 4 at 1A g -1 Efficiency-specific capacity curve of cyclic charge and discharge under current density.

[0034] Fig.11 Test case 5 at 3A g -1 Efficiency-specific capacity curve of cyclic charge and discharge under current density.

[0035] Fig.12 Test case 6 at 3A g -1 Efficiency-specific capacity curve of cyclic charge and discharge under current density. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Example 1: 4 mmol of ammonium metavanadate and 70 mmol of lithium hydroxide were dissolved in 60 mL of deionized water, and then 100 mg of g-C3N4 was dispersed in the above solution by stirring and ultrasonication; the resulting mixture was transferred to an autoclave and hydrothermally treated at 180°C in a forced air oven for 2 hours; the hydrothermally treated solution was centrifuged and washed, and dried in a vacuum oven to obtain a lithium vanadate / g-C3N4 negative electrode material. The scanning electron microscope image of the product is shown in FIG. Figure 1 ,Depend on Figure 1 It can be seen that lithium vanadate is evenly anchored on the g-C3N4 sheet. The addition of g-C3N4 sheet can reduce the accumulation of lithium vanadate and the volume expansion problem of lithium vanadate, thereby solving the problem of poor cycle stability of high-energy lithium-ion hybrid capacitors. Figure 2 As shown, the results show that the spectrum of the product lithium vanadate / g-C3N4 composite material corresponds to the standard card of lithium vanadate, and there is no obvious impurity peak, indicating that the obtained sample is a pure phase without other impurities, and the addition of g-C3N4 does not affect the formation of lithium vanadate.

[0038] Example 2: The rice husk was placed in a drying oven overnight to remove moisture, and then ground into fine powder using a high-speed crusher; 5 g of rice husk powder was added to a 0.8 M potassium hydroxide solution so that the solution pH was 10-11, and rapidly stirred for 16 hours, and then the powder was centrifuged and dried, and heated to 900 °C in a tubular furnace in an argon atmosphere at a heating rate of 5 °C / min, and kept warm for 2 hours; then 0.8 M hydrochloric acid was added so that the solution pH was 3-4, and the powder was treated for 16 hours, filtered and washed with deionized water until neutral, and then dried in an oven at 100 °C to obtain a rice husk-derived rice husk carbon positive electrode material. The scanning electron microscope image of the rice husk-derived rice husk carbon is shown in Figure 2. Figure 3 , it can be seen from the figure that the product has a porous structure with high porosity.

[0039] Example 3: Place wheat bran in a drying oven overnight to remove moisture, then grind into fine powder using a high-speed stirrer; add 3 g of wheat bran powder to a 1M potassium hydroxide solution so that the solution has a pH value of 10-11, stir rapidly for 12 hours, centrifuge and dry, heat to 800°C in an argon atmosphere tube furnace at a heating rate of 5°C / min, keep warm for 7 hours, then treat with 1.5M hydrochloric acid for 13 hours so that the solution has a pH value of 3-4, filter and wash with deionized water until neutral, then dry in an oven at 80°C to obtain a wheat bran-derived wheat bran carbon positive electrode material. The scanning electron microscope image of wheat bran-derived wheat bran carbon is shown in Figure 2. Figure 4 As shown, it can be seen from the figure that the product has a porous structure and a large pore size. Figure 5 This is the nitrogen adsorption-desorption curve of wheat bran carbon positive electrode material derived from wheat bran. It can be seen from the figure that the obtained wheat bran carbon positive electrode material has a large specific surface area.

[0040] Comparative Example 1: 4 mmol of ammonium metavanadate and 70 mmol of lithium hydroxide were dissolved in 60 mL of deionized water, then transferred to an autoclave and hydrothermally treated at 180°C in a forced air oven for 2 h; the hydrothermally treated solution was centrifuged and washed, and dried in a vacuum oven to obtain a lithium vanadate negative electrode material. The scanning electron microscope image of lithium vanadate is shown in FIG. Figure 6 As shown, the obtained lithium vanadate particles are large in size and have serious agglomeration.

[0041] Electrochemical performance test: Preparation of positive electrode: accurately weigh the positive electrode material, conductive carbon black and polyvinylidene fluoride according to the mass fraction of 70%:20%:10%, use 1-methyl-2-pyrrolidone as solvent to evenly mix to make slurry, and evenly apply it on 19 mm aluminum foil. The coated electrode sheet is vacuum dried at 70 °C for 12 hours.

[0042] Preparation of negative electrode: accurately weigh the negative electrode material, conductive carbon black and polyvinylidene fluoride according to the mass fraction of 70%:20%:10%, mix them evenly with 1-methyl-2-pyrrolidone as solvent to make slurry, evenly apply it on 10 mm copper foil, and vacuum dry the coated electrode sheet at 70 °C for 12 h.

[0043] A polypropylene microporous membrane was used as the separator and 1 mol L -1 Lithium hexafluorophosphate / ethylene carbonate + diethyl carbonate (V EC :V DEC =1:1) + 5% fluoroethylene carbonate as the electrolyte, combined with the positive electrode and the negative electrode, and assembled into a button cell as an experimental battery in a glove box filled with high-purity argon.

[0044] Test Example 1: Using Example 1 as the negative electrode material and activated carbon as the positive electrode material, a button battery was assembled and tested at 1A g -1 The cycling performance of the device was measured at a current density of 20 cycles. Figure 7 As shown in Figure 2, the sample still maintains 226 mAh g after 20 cycles. -1 The capacity of the capacitor indicates that the capacitor made of the lithium vanadate / g-C3N4 negative electrode material of the present invention has a high capacity, and the capacity retention rate is close to 100%, and has excellent cycle stability.

[0045] Test Example 2: Comparative Example 1 was used as the negative electrode material and activated carbon was used as the positive electrode material to assemble a button battery and test its -1 The cycling performance of the device was measured at a current density of 20 cycles. Figure 8 As shown, the sample has only 120 mAh g after 20 cycles. -1 The capacity of the capacitor in Test Example 2 made of lithium vanadate negative electrode material has a lower specific capacity than that in Test Example 1.

[0046] Test Example 3: Example 1 was used as the negative electrode material and Example 2 was used as the positive electrode material to assemble a button battery and test its -1 The cycling performance of the battery was measured at a current density of 200 cycles. Fig. 9 As shown in Figure 2, the sample still maintains 317 mAh g after 200 cycles. -1 The capacity of the capacitor is high and has excellent cycle stability. The capacity attenuation is small when rice husk carbon is used as the positive electrode material. The performance improvement effect of rice husk carbon on the capacitor is significantly better than that of test example 1 using ordinary activated carbon.

[0047] Test Example 4: Comparative Example 1 was used as the negative electrode material and Example 2 was used as the positive electrode material to assemble a button battery and test its -1 The cycling performance of the battery was measured at a current density of 200 cycles. Fig.10 As shown in Figure 2, the sample only has 97 mAh g after 200 cycles. -1 The capacity has poor cycle stability compared to Test Example 3.

[0048] Compared with Test Example 2, the cycle performance of the capacitor using rice husk carbon has been improved, but the improvement is not obvious. The comparison of Test Example 3 and Test Example 4, combined with Test Example 1 and Test Example 2, which only compare lithium vanadate / g-C3N4 and lithium vanadate, shows that the use of rice husk carbon and lithium vanadate / g-C3N4 together can significantly improve the capacity and cycle performance of the capacitor. This improvement effect is difficult to achieve by using rice husk carbon or lithium vanadate / g-C3N4 alone. The rice husk carbon positive electrode material and the lithium vanadate / g-C3N4 negative electrode material have a synergistic effect.

[0049] Test Example 5: Example 1 was used as the negative electrode material and Example 3 was used as the positive electrode material to assemble a button battery and test its -1 The cycling performance of the battery was measured at a current density of 100 cycles. Fig.11 As shown in Figure 2, the sample still maintains 195.8 mAh g after 100 cycles. -1 The capacity of the battery is high and has excellent cycle stability. Under the premise of using the lithium vanadate / g-C3N4 negative electrode material of Example 1, wheat bran carbon is used as the positive electrode. -1 Even after 100 cycles at high current, it can still maintain nearly 200mAh g -1 The capacity of the battery is much higher than that of Test Example 1 which uses activated carbon as the positive electrode. The cycle performance is significantly improved.

[0050] Test Example 6: Comparative Example 1 was used as the negative electrode material and Example 3 was used as the positive electrode material to assemble a button battery and test its -1 The cycling performance of the battery was measured at a current density of 100 cycles. Fig.12 As shown in Figure 2, the sample only has 112 mAh g after 100 cycles. -1 The capacity has poor cycle stability compared to Test Example 5.

[0051] Under the premise of a higher current density, compared with Test Example 2 using activated carbon as the positive electrode, Test Example 6 has better cycle stability, but the improvement is not obvious. Combined with the comparison of Test Example 1 and Test Example 2, from the comparison of the above Test Example 5 and Test Example 6, it can be seen that the improvement effect of wheat bran carbon positive electrode material and lithium vanadate / g-C3N4 negative electrode material on capacitor performance is greater than the improvement effect produced by the application of a single electrode material, and the wheat bran carbon positive electrode material and lithium vanadate / g-C3N4 negative electrode material can synergistically enhance the performance.

[0052] It can be seen from the above test examples that the first cycle charge and discharge attenuation of the capacitor made of the lithium vanadate / g-C3N4 negative electrode material of Example 1 of the present invention is significantly less than that of lithium vanadate, and the overall specific capacity attenuation is also significantly smaller, the capacity is higher, and the cycle stability is also better. The cycle stability of the capacitor using biomass charcoal such as rice husk charcoal and wheat bran charcoal is also stronger, but the cycle stability and specific capacity of the capacitor using only lithium vanadate / g-C3N4 negative electrode material or biomass charcoal positive electrode material are not as good as test examples 3 and 5 using both lithium vanadate / g-C3N4 negative electrode material and biomass charcoal positive electrode material. In particular, the specific capacity of test examples 3 and 5 has a trend of slowly rising as the cycle proceeds, and the synergistic effect of lithium vanadate / g-C3N4 negative electrode material and biomass charcoal positive electrode material is very obvious.

[0053] For those skilled in the art, various other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all of these changes and deformations should fall within the protection scope of the claims of the present invention.

Claims

1. A high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as a negative electrode, characterized in that: It includes a positive electrode, a negative electrode and an electrolyte capable of conducting lithium ions; the positive electrode uses a carbon material that can undergo reversible adsorption and desorption of anions in an organic electrolyte as the positive electrode material; the negative electrode uses lithium vanadate / g-C3N4 as the negative electrode material.

2. The high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as the negative electrode according to claim 1, characterized in that The carbon material is one or more of activated carbon and biochar.

3. The high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as the negative electrode according to claim 2, characterized in that The biomass charcoal is one or more of rice husk charcoal, wheat bran charcoal or peanut charcoal.

4. The high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as a negative electrode according to claim 1, characterized in that The electrolyte is an organic solution of lithium hexafluorophosphate, ethylene carbonate, diethyl carbonate and fluoroethylene carbonate.

5. The high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as a negative electrode according to claim 1, characterized in that The preparation of the negative electrode material comprises the following steps: (1) Dissolve ammonium metavanadate and lithium hydroxide in deionized water, then add g-C3N4 into the reaction system and mix and disperse thoroughly to obtain a dispersion; (2) subjecting the obtained dispersion to hydrothermal treatment; (3) After hydrothermal treatment, the precipitate is collected by centrifugation, washed and dried to obtain the negative electrode material.

6. The high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as a negative electrode according to claim 5, characterized in that The molar ratio of the ammonium metavanadate to the lithium hydroxide is 1:(15-20); the mass of the g-C3N4 is 5%-20% of the total mass of the ammonium metavanadate and the lithium hydroxide.

7. The high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as a negative electrode according to claim 5, characterized in that The thorough mixing and dispersion in step (1) is performed by first stirring for 0.5 to 2 hours and then ultrasonicating for 1 to 4 hours.

8. The high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as a negative electrode according to claim 5, characterized in that The temperature of the hydrothermal treatment in step (2) is 160-200°C and the time is 2-4 hours.

9. The high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as a negative electrode according to claim 2, characterized in that The preparation of the biochar comprises the following steps: crushing the biomass into powder, then adding the powder into a potassium hydroxide solution and stirring for 8 to 16 hours; after centrifugal drying, heating the biomass to 700 to 1000° C. at a rate of 5° C. / min in an argon atmosphere and keeping the temperature for 2 to 8 hours to obtain a carbonized powder; treating the carbonized powder with hydrochloric acid for 12 to 18 hours, filtering, washing with water until neutral, and drying to obtain the biochar.

10. The high-energy lithium-ion hybrid capacitor with lithium vanadate / g-C3N4 as a negative electrode according to claim 9, characterized in that The powder is added to a 0.5-2.0M potassium hydroxide solution, and the pH value of the system is adjusted to 8-11; the carbonized powder is treated with 0.5-2.0M hydrochloric acid, and the pH value of the system is adjusted to 3-4.

Citation Information

Cited By

  • Electrochemical device based on CaV2O6 / CaSiO3 / g-C3N4 nanocomposite

    US12518933B1