A lithium metal composite negative electrode and preparation method thereof, and a lithium ion battery

By using a composite negative electrode with three-dimensional skeleton material and doped inorganic solid electrolyte in lithium-ion batteries, the volume expansion problem caused by the activeness and chemical instability of the lithium metal negative electrode is solved, and the circulation and rate performance of the battery is improved, ensuring that Battery safety.

CN118645589BActive Publication Date: 2024-11-15SHENZHEN BTR NEW ENERGY TECH RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411083258.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-15
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The lithium metal negative electrode causes volume expansion and dendritic growth due to its activity and chemical instability, destroying the interface of the negative electrode solid electrolyte and affecting the commercial application of lithium-ion batteries.

Method used

The composite negative electrode of a three-dimensional framework material and a doped inorganic solid electrolyte are used to form a protective layer of ion-conducting channels on the surface of the three-dimensional framework material, and the direct contact between lithium metal and the electrolyte is suppressed, thereby improving the cycling and rate performance of the battery.

Benefits of technology

Effectively inhibit the volume expansion of lithium metal, improve the circulation performance, rate performance and safety of the battery, and achieve uniform dispersion through the high ionic conductivity and mechanical stability of the inorganic solid electrolyte to avoid the occurrence of side reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118645589B_ABST
    Figure CN118645589B_ABST
Patent Text Reader

Abstract

The present application provides a lithium metal composite negative electrode and a preparation method thereof, and a lithium ion battery, which relates to the field of new energy technology. The rich pore structure of the three-dimensional skeleton material of the lithium metal composite negative electrode provides sufficient space for lithium metal deposition, avoiding the volume expansion of lithium metal during the charging and discharging process; due to the Ti in the inorganic solid electrolyte 4+ When in contact with lithium metal, it is easily reduced to Ti 3+ This reduction reaction will lead to the formation of a protective layer at the interface between lithium metal and the three-dimensional skeleton material. Since the inorganic solid electrolyte has high ionic conductivity, good mechanical stability and wide temperature adaptability, it can be evenly dispersed on the surface of the three-dimensional skeleton material, resulting in the protective layer formed by the reaction with lithium metal coating the surface of the three-dimensional skeleton material. In the presence of electrolyte, it can be regarded as a percolation network with high ionic conductivity, which can avoid direct contact between lithium metal and electrolyte and inhibit the occurrence of side reactions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of new energy technology, and in particular to a lithium metal composite negative electrode and a preparation method thereof, and a lithium ion battery. Background Art

[0002] Lithium metal anodes are expected to become the ultimate choice for lithium-ion battery anodes due to their high theoretical capacity. However, lithium metal is more active and chemically unstable. Its unlimited volume expansion and dendrite growth lead to repeated rupture and recombination of the anode solid electrolyte interface layer, which greatly affects the commercial application of lithium metal anodes.

[0003] In the prior art, SEI can be directly or indirectly generated on the surface of lithium metal by using solid electrolyte or artificial SEI. This SEI not only has good mechanical strength, but also can inhibit the continuous reaction between electrolyte and lithium metal. However, the use of polymer solid electrolyte or its use as a protective layer may cause uneven reaction and low ion conductivity, which will reduce the charging and discharging efficiency of the battery, and may also cause uneven SEI film, and finally cause uneven lithium deposition. Summary of the invention

[0004] The purpose of the present application is to provide a lithium metal composite negative electrode and a preparation method thereof, and a lithium ion battery, aiming to solve the problems existing in the existing lithium metal negative electrode.

[0005] To achieve the above objectives, the present application provides a lithium metal composite negative electrode in the first aspect, see Figure 1 , Figure 1 The schematic diagram of the structure of the lithium metal composite negative electrode of the present application includes:

[0006] current collector;

[0007] A three-dimensional skeleton material coated on the surface of the current collector, wherein the three-dimensional skeleton material is a porous structure, a conductive agent exists in the pores of the three-dimensional skeleton material, and an inorganic solid electrolyte is doped in the three-dimensional skeleton material, wherein the inorganic solid electrolyte contains a titanium element with a valence of tetravalent or higher;

[0008] Lithium metal is composited on the surface of the three-dimensional skeleton material.

[0009] Preferably, the inorganic solid electrolyte includes one or both of LLTO and LATP, wherein LLTO is a lithium lanthanum titanium oxide material having a chemical formula of Li 3x La 2 / 3-x TiO3, LATP is a lithium aluminum titanium phosphate material, and its chemical formula is Li 1.3 Al 0.3 Ti 1.7 (PO4)3.

[0010] Preferably, the particle size D50 of the inorganic solid electrolyte is 100 nm to 2 μm, for example, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1 μm, 1.5 μm or 2 μm. More preferably, the particle size D50 of the inorganic solid electrolyte is 200 nm to 600 nm.

[0011] Preferably, the ionic conductivity σ of the three-dimensional framework material doped with the inorganic solid electrolyte is 10 -5 S / cm~10 -3 S / cm.

[0012] Preferably, the mass ratio of the inorganic solid electrolyte to the three-dimensional skeleton material is 1:1 to 1:15, for example, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14 or 1:15. More preferably, the mass ratio of the inorganic solid electrolyte to the three-dimensional skeleton material is 1:3 to 1:15.

[0013] The uniformity of the protective layer with ion-conducting channels formed by the reaction of the three-dimensional skeleton material doped with inorganic solid electrolyte and lithium metal is related to the particle size and addition amount of the inorganic solid electrolyte. The larger the particle size and the smaller the addition amount, the more uneven the protective layer formed, resulting in uneven lithium deposition and affecting the coulombic efficiency.

[0014] Preferably, the particle size D50 of the three-dimensional skeleton material is 0.5 μm to 60 μm, for example, it can be 0.5 μm, 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm or 60 μm.

[0015] Preferably, the thickness change Δd of the three-dimensional skeleton material before and after being doped with the inorganic solid electrolyte is 100 nm to 2 μm;

[0016] Preferably, the coating thickness of the three-dimensional skeleton material is 30 μm to 60 μm, for example, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm or 60 μm.

[0017] Preferably, the pore volume of the three-dimensional framework material is 0.001 cm 3 / g ~0.2cm 3 / g.

[0018] Preferably, the specific surface area of ​​the three-dimensional skeleton material is 10 to 1000 m 2 / g, for example, 10m 2 / g, 50m2 / g、100m 2 / g, 200m 2 / g、300m 2 / g, 400m 2 / g、500m 2 / g、600m 2 / g、700m 2 / g、800m 2 / g、900m 2 / g or 1000m 2 / g.

[0019] Preferably, the three-dimensional skeleton material is an organic polymer, and the organic polymer includes any one of polyaniline, polypyrrole, polythiophene, polyacetylene, phenolic resin, formaldehyde resin, epoxy resin, melamine resin, furfural resin, and polyester resin.

[0020] Preferably, the three-dimensional skeleton material is subjected to a BET test, and the average pore size is 3 to 500 nm.

[0021] Preferably, the thickness of the lithium metal composite negative electrode is 34 μm to 86 μm.

[0022] Preferably, the content of the conductive agent in the three-dimensional skeleton material is 1% to 30% of the mass of the three-dimensional skeleton material, for example, 1%, 5%, 10%, 15%, 20%, 25% or 30%.

[0023] Preferably, the conductive agent includes one or more of SP, graphite, acetylene black, carbon nanotubes, graphene, and Ketjen black.

[0024] Preferably, the particle size of the conductive agent is 1 nm to 100 nm.

[0025] Preferably, there is also a lithium-philic substance in the pores of the three-dimensional skeleton material, and the content of the lithium-philic substance in the three-dimensional skeleton material is 1% to 10% of the mass of the three-dimensional skeleton material, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%.

[0026] Preferably, the lithiophilic substance includes one or more of carbon fiber, carbon nanotube, graphene, Ag, Au, Si, ZnO, Al, Mg, and Ti.

[0027] Preferably, the particle size of the lithiophilic substance is 10 nm to 500 nm.

[0028] The second aspect of the present application also provides a method for preparing the above-mentioned lithium metal composite negative electrode, comprising:

[0029] Mixing a three-dimensional skeleton material and an inorganic solid electrolyte, wherein the three-dimensional skeleton material is a porous structure with a conductive agent in the pores, and the inorganic solid electrolyte contains titanium, to obtain a three-dimensional skeleton material doped with the inorganic solid electrolyte;

[0030] The three-dimensional skeleton material doped with an inorganic solid electrolyte, a binder, a conductive agent, and a solvent are mixed to obtain a slurry, the slurry is coated on a current collector, and after drying, a three-dimensional skeleton material current collector doped with an inorganic solid electrolyte is obtained;

[0031] The three-dimensional skeleton material current collector doped with the inorganic solid electrolyte is composited with lithium metal to obtain a lithium metal composite negative electrode.

[0032] Preferably, the method for preparing the three-dimensional skeleton material comprises:

[0033] Adding monomer 1 and monomer 2 into water to mix and dissolve, adding a catalyst to adjust the pH, and reacting to obtain a polymer material;

[0034] The polymer material, the conductive agent and the dispersant are mixed with water, or the polymer material, the conductive agent, the lithium-philic substance and the dispersant are mixed with water to react to obtain a three-dimensional skeleton material.

[0035] Preferably, the monomer 1 includes one or more of cresol, nonylphenol, urea, melamine, phenol, aralkylphenol, furfuryl alcohol, acrylic acid, and phthalic acid.

[0036] Preferably, the monomer 2 comprises one or more of formaldehyde, pentamethylenediamine, propylene, acrylonitrile, methacrylic acid, acetaldehyde, and vinyl alcohol.

[0037] Preferably, the mass ratio of the monomer 1 to the monomer 2 is 0.1:1-3:1, for example, it can be 0.1:1, 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1 or 3:1; the mass ratio of the water to the monomer 1 is 5-100, for example, it can be 5, 10, 15, 20, 30, 40, 50, 60, 70, 80, 90 or 100.

[0038] Preferably, the catalyst is selected from one or more of hydrochloric acid, formic acid, ammonia water, sulfuric acid, oxalic acid, carbonic acid, citric acid and acetic acid.

[0039] Preferably, the pH range is 1-7, and the pH may be 1, 2, 3, 4, 5, 6 or 7, for example.

[0040] Preferably, the amount of the conductive agent is 1% to 30% of the mass of the polymer material, for example, 1%, 5%, 10%, 15%, 20%, 25% or 30%.

[0041] Preferably, the amount of the lithium-philic substance is 1% to 10% of the mass of the polymer material, for example, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%.

[0042] Preferably, the mass ratio of the water to the polymer material is 2-10, for example, 2, 3, 4, 5, 6, 7, 8, 9 or 10.

[0043] Preferably, the dispersant is selected from any one of polyacrylate, polyvinyl ester, sodium tripolyphosphate, sodium pyrophosphate, sodium citrate, cellulose, polyvinyl pyrrolidone, polyvinyl alcohol, polycarboxylic acid, and ethanol.

[0044] Preferably, the stirring time for mixing the polymer materials in the preparation of the three-dimensional skeleton material is 10-60 min, for example, 10 min, 20 min, 30 min, 40 min, 50 min or 60 min.

[0045] Preferably, the mass ratio of the inorganic solid electrolyte to the three-dimensional skeleton material is 1:1-1:15.

[0046] Preferably, the inorganic solid electrolyte and the three-dimensional framework material are mixed with water, so that the inorganic solid electrolyte is doped in the form of a slurry, and the amount of water is 3 to 10 times the mass of the three-dimensional framework material, for example, it can be 3, 4, 5, 6, 7, 8, 9 or 10. It is understandable that when the inorganic solid electrolyte and the three-dimensional framework material are directly mixed, the inorganic solid electrolyte is doped in the form of a powder.

[0047] Preferably, the mass proportion of the three-dimensional skeleton material doped with the inorganic solid electrolyte in the slurry is 70% to 90%, for example, 70%, 75%, 80%, 85%, 90% or 95%, and the mass proportion of the binder in the slurry is 5% to 10%, for example, 5%, 6%, 7%, 8%, 9% or 10%.

[0048] Wherein, the mixing method of the three-dimensional skeleton material and the inorganic solid electrolyte includes any one of direct mixing, VC mixing, wet mixing, and ball milling.

[0049] Preferably, the binder is any one or more of polyvinylidene fluoride, polyacrylic acid, polyamide, LA133, polyvinyl alcohol, polyethyleneimine, polyimide, polyethylene, SBR (styrene-butadiene latex), and sodium carboxymethyl cellulose.

[0050] Preferably, the conductive agent is selected from any one or more of SP (conductive carbon black), graphite, acetylene black, carbon nanotubes, graphene, and Ketjen black.

[0051] Preferably, the solvent is any one of NMP (N-methylpyrrolidone), DMF (N,N-dimethylformamide), and water.

[0052] Preferably, the compounding method includes any one of cold rolling, hot rolling, rolling and extrusion.

[0053] The third aspect of the present application also provides a lithium-ion battery, comprising the above-mentioned lithium metal composite negative electrode.

[0054] Compared with the prior art, the beneficial effects of this application include:

[0055] The lithium metal composite negative electrode provided by the present application includes a current collector, a three-dimensional skeleton material and lithium metal sequentially coated on the current collector, wherein the rich pore structure of the three-dimensional skeleton material provides sufficient space for lithium metal deposition, thereby avoiding the volume expansion of lithium metal during the charge and discharge process; the inorganic solid electrolyte doped in the three-dimensional skeleton material is mainly distributed in the external pores of the three-dimensional skeleton material, and the Ti in the inorganic solid electrolyte is mainly distributed in the external pores of the three-dimensional skeleton material. 4+ When in contact with lithium metal, it is easily reduced to Ti 3+ , so it will consume a part of the active lithium; this reduction reaction will lead to the formation of a protective layer at the interface between lithium metal and the three-dimensional skeleton material. Since the inorganic solid electrolyte has high ionic conductivity, good mechanical stability and wide temperature adaptability, it can be evenly dispersed on the surface of the three-dimensional skeleton material, resulting in the protective layer formed by the reaction with lithium metal coating the surface of the three-dimensional skeleton material. In the presence of electrolyte, it can be regarded as a percolation network with high ionic conductivity, which can avoid direct contact between lithium metal and electrolyte and inhibit the occurrence of side reactions; in addition, due to the presence of inorganic solid electrolyte, the particles of the three-dimensional skeleton material also have good ionic conductivity, which can achieve faster lithium ion transmission and has a significant effect on improving the rate performance of the battery. In summary, the construction of a composite electrode of a three-dimensional skeleton material and an inorganic solid electrolyte is effective in inhibiting the volume expansion of lithium metal and improving the cycle performance, rate performance and safety of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0057] Figure 1 This is a schematic diagram of the structure of the lithium metal composite negative electrode of the present application;

[0058] Figure 2 The first cycle charge and discharge curves of the half-cells of Example 1, Comparative Example 2 and Comparative Example 4;

[0059] Figure 3 This is a SEM image of the polymer material of Example 2;

[0060] Figure 4 The first cycle charge and discharge curves of the half-cells of Example 2, Example 3 and Example 4;

[0061] Figure 5 A full battery cycle comparison of Example 3 and Comparative Example 6;

[0062] Figure 6 is a SEM image of the surface of the pole piece of Example 4;

[0063] Figure 7 The cross-sectional SEM and EDS characterization of the Ti element of the three-dimensional framework material doped with the inorganic solid electrolyte of Example 4;

[0064] Figure 8 The full battery cycle comparison of Example 5, Comparative Example 2 and Comparative Example 4;

[0065] Fig. 9 This is the SEM image of the cross-section of the mesoporous carbon of Comparative Example 5. DETAILED DESCRIPTION

[0066] As used herein:

[0067] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0068] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0069] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0070] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0071] Example 1

[0072] Dissolve 64g urea and 48g formaldehyde in 2L water and stir until completely dissolved, then add a certain amount of hydrochloric acid to adjust the pH to 4; stir the mixed solution evenly and let it stand for 24h, filter and wash until neutral, and dry to obtain the polymer material. Dissolve 30g polymer material and 2g graphene material in 100mL water, add a small amount of ethanol and stir for a certain period of time, then filter the mixed solution and dry to obtain the three-dimensional skeleton material.

[0073] Mix 20g of three-dimensional skeleton material with 20g of LATP with a particle size of 600nm, 5g of conductive carbon black, and 100g of 5% LA133, and add appropriate amount of water and stir to form a uniform slurry. Then use a scraper to coat the slurry on the copper foil, wait for it to dry and then roll it. The total thickness of the electrode after rolling is measured by a micrometer and is 34μm. Finally, the electrode is cut into a 16mm diameter electrode as the positive electrode, a 1mm ultra-thin lithium sheet as the negative electrode, and 1M LiTFSI+DOL / DME (v / v=1:1) +2wt% LiNO3 as the electrolyte to assemble a button half-cell, and the charge and discharge test is carried out on it. The charge and discharge results of the first cycle are as follows: Figure 2 shown.

[0074] Example 2

[0075] 90g urea and 30g formaldehyde were dissolved in 1L water and stirred until completely dissolved, and then a certain amount of hydrochloric acid was added to adjust the pH to 6; the mixed solution was stirred evenly and then allowed to stand for 24h, filtered and washed until neutral, and dried to obtain a polymer material, whose SEM is as follows Figure 3 30g of polymer material and 2g of graphene material were dissolved in 100mL, and a small amount of ethanol was added and stirred for a certain period of time, and then the mixed solution was filtered and dried to obtain a three-dimensional skeleton material.

[0076] 20 g of three-dimensional framework material and 2.85 g of LATP with a particle size of 300 nm were added to 50 mL of water and stirred for 1 h, then filtered and dried to obtain the three-dimensional framework material doped with inorganic solid electrolyte. The ionic conductivity of the material was measured by electrochemical impedance spectroscopy to be 5.2×10 -4S / cm. Add 2.8g SP, 140g sodium carboxymethyl cellulose, 5.7g 50% SBR and appropriate amount of water to the three-dimensional skeleton material and stir until the slurry is completely dispersed. Then use a scraper to coat the slurry on the copper foil, roll it after it dries, and cut it into pole pieces with a diameter of 16mm. Use the pole piece as the positive electrode, 1mm ultra-thin lithium sheet as the negative electrode, 1M LiTFSI+DOL / DME (v / v=1:1) +2wt% LiNO3 as the electrolyte to assemble a button half-cell, and perform charge and discharge tests on it. The charge and discharge results of the first cycle are as follows Figure 4 shown.

[0077] Example 3

[0078] Dissolve 80g urea and 48g formaldehyde in 1L water and stir until completely dissolved, then add a certain amount of hydrochloric acid to adjust the pH to 3; stir the mixed solution evenly and let it stand for 24h, filter and wash until neutral, and dry to obtain the polymer material. Dissolve 50g polymer material and 2.5g carbon nanotubes in 100mL, add a small amount of ethanol and stir for a certain period of time, then filter the mixed solution and dry to obtain the three-dimensional skeleton material.

[0079] 30g of three-dimensional framework material and 2g of LATP with a particle size of 300nm were stirred in a VC mixer for 1h to obtain a three-dimensional framework material doped with an inorganic solid electrolyte. The ionic conductivity of the material was 2.58×10 -4 S / cm. Add 4g SP, 80g 5% LA133 and appropriate amount of water to the three-dimensional skeleton material and stir until the slurry is completely dispersed. Then use a scraper to coat the slurry on the copper foil, wait for it to dry, roll it, and cut it into pole pieces with a diameter of 16mm. Use the pole piece as the positive electrode and the 1mm ultra-thin lithium sheet as the negative electrode to assemble a button half-cell; for the full battery, the pole piece is cut into a disc with a diameter of 12mm as the negative electrode, and NCM with a diameter of 8.4mm is used as the positive electrode. The electrolyte is 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3. It is subjected to charge and discharge tests. The cycle results of the full battery are shown as follows. Figure 5 As shown, the first cycle charge and discharge curve of the half-battery is as follows Figure 4 shown.

[0080] Example 4

[0081] Dissolve 72g urea and 72g formaldehyde in 1L water and stir until completely dissolved, then add a certain amount of acetic acid to adjust the pH to 2; stir the mixed solution evenly and let it stand for 24h, filter and wash until neutral, and dry to obtain the polymer material. Dissolve 50g polymer material, 2.5g carbon nanotubes, and 5g ZnO in 100mL and stir for a certain period of time, then filter the mixed solution and dry to obtain the three-dimensional skeleton material.

[0082] 25g of three-dimensional framework material and 8.3g of LATP with a particle size of 300nm were added to 50mL of water and stirred for 1h, then filtered and dried to obtain the three-dimensional framework material doped with inorganic solid electrolyte. The ionic conductivity of the material was 7.36×10 -4 S / cm. The particle size of LATP on the surface of the skeleton material was measured by SEM, and it was found that its particle size was mainly distributed between 250-350nm, indicating that doping LATP by the above method does not change its morphology. 4g SP and a certain amount of polyvinylidene fluoride were added to the three-dimensional skeleton material, and an appropriate amount of DMF was added and stirred until the slurry was completely dispersed. The slurry was then coated on a copper foil with a scraper, rolled after it was dried, and cut into pole pieces with a diameter of 16mm. A button half-cell was assembled with the pole piece as the positive electrode, a 1mm ultra-thin lithium sheet as the negative electrode, and 1MLiTFSI+DOL / DME (v / v=1:1) +2wt% LiNO3 as the electrolyte; the button full cell was made in the same way as in Example 3, and the two batteries were charged and discharged. Figure 4 Comparison results of first cycle charge and discharge of half cells prepared in Example 2, Example 3 and Example 4. Figure 6 This is a SEM image of the electrode surface; Figure 7 This is a cross-sectional SEM image of a three-dimensional framework material doped with an inorganic solid electrolyte ( Figure 7 The upper part) and the EDS characterization results of Ti element at the horizontal line in the SEM image ( Figure 7 The results show that in addition to being distributed on the surface of the three-dimensional framework material, some LATP also enters the pores of the framework material during the mixing process.

[0083] Example 5

[0084] The three-dimensional skeleton material was prepared in the same manner as in Example 4.

[0085] 30g of three-dimensional skeleton material and 2g of LATP with a particle size of 600nm were added to 50mL of water and stirred for 1h, then filtered and dried to obtain a three-dimensional skeleton material doped with an inorganic solid electrolyte. 4g of SP and a certain amount of polyvinylidene fluoride were added to the three-dimensional skeleton material, and an appropriate amount of DMF was added and stirred until the slurry was completely dispersed. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece, and cut into a pole piece with a diameter of 12mm as the negative electrode, and a NCM with a diameter of 8.4mm was used as the positive electrode, and 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 was used as the electrolyte to assemble a button-type full battery, and the charge and discharge test was performed on it.

[0086] Example 6

[0087] The three-dimensional skeleton material was prepared in the same manner as in Example 3.

[0088] 30g of three-dimensional skeleton material and 2g of LLTO with a particle size of 500nm were added to 50mL of water and stirred for 1h, then filtered and dried to obtain a three-dimensional skeleton material doped with an inorganic solid electrolyte. 4g of SP, 80g of 5% LA133 and an appropriate amount of water were added to the three-dimensional skeleton material and stirred until the slurry was completely dispersed. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 46μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, 1M LiTFSI+DOL / DME (v / v=1:1)+2wt%LiNO3 as the electrolyte, and the charge and discharge test was performed on it.

[0089] Comparative Example 1

[0090] Dissolve 126g of melamine and 45g of formaldehyde in 1L of water and stir until completely dissolved, then add a certain amount of acetic acid to adjust the pH to 3; stir the mixed solution evenly and let it stand for 24h, filter and wash until neutral, and dry to obtain the polymer material. Dissolve 50g of polymer material, 2.5g of carbon nanotubes, and 5g of ZnO in 100mL and stir for a certain period of time, then filter the mixed solution and dry to obtain the three-dimensional skeleton material.

[0091] 20g of three-dimensional skeleton material and 2.8g of Al2O3 were stirred in a VC mixer for 1h to obtain a three-dimensional skeleton material doped with a solid electrolyte. 2.8g of SP, 140g of sodium carboxymethyl cellulose, 5.7g of 50% SBR and an appropriate amount of water were added to the three-dimensional skeleton material and stirred until the slurry was completely dispersed. Then the slurry was coated on the copper foil with a scraper. After it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece and cut into a pole piece with a diameter of 12mm as the negative electrode, and a NCM with a diameter of 8.4mm was used as the positive electrode. 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 was used as the electrolyte to assemble a button-type full battery, and the charge and discharge test was performed on it.

[0092] Comparative Example 2

[0093] The three-dimensional skeleton material was prepared in the same manner as in Example 3.

[0094] Mix 32g of three-dimensional skeleton material, 4g of SP, 80g of 5% LA133 and appropriate amount of water and stir until the slurry is completely dispersed. Then use a scraper to coat the slurry on copper foil, roll it after it dries, and cut it into pole pieces with a diameter of 16mm. Use the pole piece as the positive electrode, 1mm ultra-thin lithium sheet as the negative electrode, and 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte to assemble a button half-cell; the button full cell is made in the same way as in Example 3, and the two batteries are charged and discharged. The first cycle charge and discharge curve of the half-cell is shown in Figure 2 As shown, the full battery cycle comparison is Figure 8 shown.

[0095] Comparative Example 3

[0096] The three-dimensional skeleton material was prepared in the same manner as in Comparative Example 1.

[0097] 32g of three-dimensional skeleton material, 4g of SP, 80g of 5% LA133 and appropriate amount of water were mixed and stirred until the slurry was completely dispersed. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece, and a NMP solution containing 5% LATP (300nm) was dripped on the composite lithium pole piece, and baked at 80℃ on a heating plate to evaporate the solvent. After the pole piece was dried, it was cut into a pole piece with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, 1MLiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.

[0098] Comparative Example 4

[0099] The three-dimensional skeleton material was prepared in the same manner as in Example 4.

[0100] 31.6g of three-dimensional skeleton material and 0.4g of LATP with a particle size of 600nm were added to 50mL of water and stirred for 1h, then filtered and dried to obtain a three-dimensional skeleton material doped with an inorganic solid electrolyte. 4g of SP and a certain amount of polyvinylidene fluoride were added to the three-dimensional skeleton material, and an appropriate amount of DMF was added and stirred until the slurry was completely dispersed. The slurry was then coated on a copper foil with a scraper, rolled after it was dried, and cut into pole pieces with a diameter of 16mm. A button half-cell was assembled with the pole piece as the positive electrode, a 1mm ultra-thin lithium sheet as the negative electrode, and 1MLiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte; the button full cell was made in the same way as in Example 3, and both batteries were subjected to charge and discharge tests. Among them, the first cycle charge and discharge curves of the half-cells of Example 1, Comparative Example 2, and Comparative Example 4 are shown in the following figure. Figure 2As shown, the cycle comparison of the full battery in Example 5, Comparative Example 2 and Comparative Example 4 is as follows Figure 8 shown.

[0101] Comparative Example 5

[0102] 30 g of porous carbon material with mesoporous structure (cross section SEM as shown in Fig. 9 The 3D skeleton material was obtained by dissolving 1.5 g of SP, 0.6 g of ZnO and an appropriate amount of polyvinyl pyrrolidone in 100 mL of water, and then separated, washed and dried to obtain a 3D skeleton material. The specific surface area of ​​the 3D skeleton material measured by BET was 555.5 m 2 / g.

[0103] 20g of three-dimensional skeleton material was mixed with 20g of LLZTO with a particle size of 300nm, 5g of carbon nanotubes, and 100g of 5% LA133, and an appropriate amount of water was added to stir to form a uniform slurry. The slurry was then coated on copper foil with a scraper, and rolled after drying. The total thickness of the pole piece after rolling was measured by a micrometer to be 34μm. Finally, the pole piece was cut into a pole piece with a diameter of 16mm as the positive electrode, a 1mm ultra-thin lithium sheet as the negative electrode, and 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte to assemble a button half-cell, and the charge and discharge test was performed on it.

[0104] Comparative Example 6

[0105] The three-dimensional skeleton material was prepared in the same manner as in Example 3.

[0106] 30g of three-dimensional skeleton material and 2g of LLZTO with a particle size of 300nm were added to 50mL of water and stirred for 1h, then filtered and dried to obtain a three-dimensional skeleton material doped with an inorganic solid electrolyte. 4g of SP, 80g of 5% LA133 and an appropriate amount of water were added to the three-dimensional skeleton material and stirred until the slurry was completely dispersed. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the electrode. The total thickness of the electrode was measured by a micrometer to be 46μm. The electrode was cut into discs with a diameter of 12mm as the negative electrode, and NCM with a diameter of 8.4mm was used as the positive electrode, and 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 was used as the electrolyte to assemble a button-type full battery, which was subjected to charge and discharge tests. The results are as follows Figure 5 shown.

[0107] Performance Testing

[0108] The inorganic solid electrolyte doped three-dimensional skeleton materials obtained in the above embodiments and comparative examples were tested for specific surface area and pore size distribution using a Gaobo BK300C specific surface area meter and an American Mack TriStar-3030 pore size analyzer; the particle size range of the samples was tested using a Malvern 3000 laser particle size analyzer; the surface, cross-section SEM and element distribution of the samples were tested using a Zeiss SEM 460 thermal field emission scanning electron microscope and an Oxford Ultim Max170 energy spectrometer; the ionic conductivity of the samples was tested using a German Cond3310 conductivity meter; the thickness of the electrode before and after the deposition of metallic lithium was measured using a micrometer, and the expansion rate was calculated.

[0109] After the batteries were prepared, the electrochemical performance tests were carried out. The electrochemical performance tests of the samples were carried out using a Blue Power M340A test cabinet, and the battery assembly was carried out in a German Braun glove box.

[0110] The button half-cell is prepared by a method known in the art: a three-dimensional skeleton material electrode doped with an inorganic solid electrolyte is used as the working electrode, a metal lithium sheet (1mm) is used as the counter electrode, 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 is used as the electrolyte, Celgrad2400 is used as the diaphragm, and the shell is a 2032 button battery shell to assemble the button half-cell. The test conditions are: at room temperature, the first week adopts a charge and discharge system of first 0.1C constant rate discharge, then 0.1C constant rate charge to 1.2V, and then 0.5C cycle. Among them, the deposition capacity of lithium is 4mAh.

[0111] The specific button-type full battery is prepared by a method known in the art: lithium iron phosphate or NCM polycrystalline is used as the positive electrode, an inorganic solid electrolyte doped three-dimensional skeleton material pole piece is used as the negative electrode, 1M LiTFSI+DOL / DME (v / v=1:1)+2wt%LiNO3 is used as the electrolyte, Celgard2400 is used as the diaphragm, and the shell adopts a 2032 button-type battery shell to assemble the button-type full battery. The test conditions are: at room temperature, first use a 0.05C constant rate charge and discharge for two weeks, the voltage range is 2.75-4.2V, and then use a 1C / 5C charge and discharge system for cycling. The designed gram capacity of the inorganic solid electrolyte doped three-dimensional skeleton material pole piece in all embodiments and comparative examples is greater than 2000mAh / g.

[0112] The test results are shown in Table 1. Figure 2 , Figure 4 and Figure 5 It can be seen that in Examples 2 to 4, as well as in Example 1, Comparative Example 2 and Comparative Example 4, as the amount of LATP added increases, the initial efficiency of the half-cell decreases significantly. This is because LATP undergoes a redox reaction when in contact with lithium metal, and the metal Li converts Ti in LATP to 4+Reduction to Ti 3+ , resulting in the consumption of some active lithium, and the more LATP content, the more active lithium is consumed in the first cycle, so the first efficiency is reduced compared to before addition. However, in the full battery, since such side reactions will generate a stable interface and good ion conductivity SEI between the electrolyte and the negative electrode in the early stage of activation, the side reactions between the electrolyte and lithium metal are reduced in the later cycle process, resulting in an increase in cycle life, such as Figure 5 The full battery cycle results of Example 3 and Figure 8 Full battery cycle results of Comparative Example 2.

[0113] The present application adjusts the morphology of the three-dimensional skeleton material by adjusting the mass ratio of monomer one to monomer two, wherein when the mass ratio of monomer one to monomer two is greater than 2:1, the obtained three-dimensional skeleton material has an irregular morphology. It can be seen from Examples 2, 3 and 4 that when the three-dimensional skeleton material changes from an irregular shape to a spherical shape, only the change in the LATP content affects the first effect, capacity retention rate and expansion rate, which has little to do with the structure of the three-dimensional skeleton material itself, and has similar effects on polymer skeleton materials with regular and irregular structures and porous carbon materials. Testing the expansion rate of the electrode after the cycle shows that the amount of LATP added is not the more the better. When the amount of LATP added to the slurry is 10% or 20%, it may be because too much LATP is prone to agglomeration during the pulping and coating process, resulting in uneven lithium deposition at the initial stage of battery activation, thereby accelerating the growth of dendrites and affecting the cycle.

[0114] However, by comparing Example 1, Example 3, Example 6, Comparative Example 5 and Comparative Example 6, it is found that when the solid electrolyte added is LLTO, it has an electrochemical effect similar to LATP, and when 300nm LLZTO accounting for 50% of the mass in the slurry is added to Comparative Example 5, there is no obvious effect on the first efficiency of the half-cell, which shows that LLZTO does not react with lithium to consume active lithium after addition, so the coulomb efficiency is close to that before addition. However, the capacity retention rate of the full battery (Comparative Example 6) with LLZTO added deteriorates, which may be because LLZTO itself does not react with lithium, but in the process of pulping and coating, LLZTO will contact with moisture, carbon dioxide and other substances in the air, resulting in the interface deterioration of the pole piece after the composite lithium and the addition of electrolyte, which may cause problems such as poor interface contact and increased impedance, and ultimately induce the growth of lithium dendrites, thereby affecting the cycle.

[0115] By comparing Example 3 and Example 5, it can be found that when the amount of LATP added is the same but the particle size is different, the effect on the initial efficiency of the battery is not obvious, but it will affect the battery cycle. By comparison, it is found that the capacity retention rate under large particle size will decrease. This may be because the large particle size causes the transmission distance between ions to become longer and the transmission channels to become fewer, thereby reducing the ion mobility and affecting the rate performance and cycle stability of the battery (the particle distribution diagram in the pole piece is shown in Figure 1 as shown).

[0116] In addition, Example 3 and Comparative Example 3 use different feeding methods to coat LATP. The results show that when LATP is directly coated on the surface of the pole piece, it can be completely in contact with lithium metal to form a stable SEI, but there is no LATP between the particles of the three-dimensional skeleton material, resulting in the skeleton material ion conductivity not being improved, which will cause the battery to be easily polarized at high charge and discharge rates, and in the cycle process, due to uneven ion transmission, uneven lithium deposition may be formed on the surface of the pole piece, affecting the cycle performance and safety of the battery. By first mixing LATP and the three-dimensional skeleton material evenly by VC mixing or wet mixing, it is possible to avoid the absence of solid electrolyte filling between the three-dimensional skeleton material particles ( Figure 6 As shown), the overall ion conductivity of the composite electrode is improved. Figure 6 The circled part of LATP, Figure 6 For the LATP on the surface of a three-dimensional skeleton material particle, it can be deduced that when there are many three-dimensional skeleton material particles, there will also be LATP between the particles.

[0117] In order to compare whether other electrolyte materials will produce similar effects to LATP, and whether the test system will also affect the cycle performance of the battery, we also conducted an experiment for Comparative Example 1. The results showed that compared with LATP, the full battery with the addition of Al2O3 electrolyte did not show a significant improvement in life. It can be seen that the type and amount of solid electrolyte added, as well as the combination of solid electrolyte and three-dimensional skeleton material, all have a certain impact on the cycle performance.

[0118] Table 1 Electrochemical properties of batteries prepared in Examples and Comparative Examples and expansion ratio of pole pieces after cycling

[0119]

[0120] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

[0121] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A lithium metal composite negative electrode, characterized in that: include: current collector; A three-dimensional skeleton material coated on the surface of the current collector, wherein the particle size D50 of the three-dimensional skeleton material is 0.5 μm to 60 μm, the three-dimensional skeleton material is an organic polymer, the three-dimensional skeleton material is a porous structure, and a conductive agent exists in the pores thereof, and an inorganic solid electrolyte is doped in the external pores of the three-dimensional skeleton material, and the inorganic solid electrolyte contains a titanium element with a valence of tetravalent or higher; the inorganic solid electrolyte is one or two of LLTO and LATP; the particle size D50 of the inorganic solid electrolyte is 200 nm to 600 nm; the mass ratio of the inorganic solid electrolyte to the three-dimensional skeleton material is 1:3 to 1:15; Lithium metal is composited on the surface of the three-dimensional skeleton material.

2. The lithium metal composite negative electrode according to claim 1, characterized in that The ionic conductivity σ of the three-dimensional framework material doped with the inorganic solid electrolyte is 10 -5 S / cm~10 -3 S / cm.

3. The lithium metal composite negative electrode according to any one of claims 1 to 2, characterized in that: At least one of the following conditions is met: (1) The thickness change Δd of the three-dimensional skeleton material before and after being doped with the inorganic solid electrolyte is 100 nm to 2 μm; (2) The coating thickness of the three-dimensional skeleton material is 30 μm to 60 μm; (3) The pore volume of the three-dimensional framework material is 0.001 cm 3 / g ~0.2cm 3 / g; (4) The specific surface area of ​​the three-dimensional skeleton material is 10 to 1000 m 2 / g; (5) The organic polymer includes any one of polyaniline, polypyrrole, polythiophene, polyacetylene, phenolic resin, formaldehyde resin, epoxy resin, melamine resin, furfural resin and polyester resin; (6) performing a BET test on the three-dimensional framework material, and the average pore size is 3-500 nm; (7) The thickness of the lithium metal composite negative electrode is 34 μm to 86 μm.

4. The lithium metal composite negative electrode according to claim 3, characterized in that: At least one of the following conditions is met: a. The content of the conductive agent in the three-dimensional skeleton material is 1% to 30% of the mass of the three-dimensional skeleton material; b. The conductive agent includes one or more of SP, graphite, acetylene black, carbon nanotubes, graphene, and Ketjen black; c. The particle size of the conductive agent is 1nm~100nm; There is also a lithium-philic substance in the pores of the three-dimensional skeleton material, and the three-dimensional skeleton material satisfies at least one of the following conditions: d. The content of the lithium-philic substance in the three-dimensional framework material is 1% to 10% of the mass of the three-dimensional framework material; e. The lithium-philic material includes one or more of carbon fiber, carbon nanotubes, graphene, Ag, Au, Si, ZnO, Al, Mg, and Ti; f. The particle size of the lithiophilic substance is 10 nm to 500 nm.

5. A method for preparing a lithium metal composite negative electrode according to any one of claims 1 to 4, characterized in that: include: Mixing a three-dimensional skeleton material and an inorganic solid electrolyte, wherein the three-dimensional skeleton material is a porous structure with a conductive agent in the pores, and the inorganic solid electrolyte contains titanium, to obtain a three-dimensional skeleton material doped with the inorganic solid electrolyte; The three-dimensional skeleton material doped with an inorganic solid electrolyte, a binder, a conductive agent, and a solvent are mixed to obtain a slurry, the slurry is coated on a current collector, and after drying, a three-dimensional skeleton material current collector doped with an inorganic solid electrolyte is obtained; The three-dimensional skeleton material current collector doped with the inorganic solid electrolyte is composited with lithium metal to obtain a lithium metal composite negative electrode.

6. The preparation method according to claim 5, characterized in that: The preparation method of the three-dimensional skeleton material comprises: Adding monomer 1 and monomer 2 into water to mix and dissolve, adding a catalyst to adjust the pH, and reacting to obtain a polymer material; The polymer material, the conductive agent and the dispersant are mixed with water, or the polymer material, the conductive agent, the lithium-philic substance and the dispersant are mixed with water to react to obtain a three-dimensional skeleton material; The preparation method of the three-dimensional skeleton material meets at least one of the following conditions: I. The monomer includes one or more of cresol, nonylphenol, urea, melamine, phenol, aralkylphenol, furfuryl alcohol, acrylic acid, and phthalic acid; II. The monomer II includes one or more of formaldehyde, pentamethylenediamine, propylene, acrylonitrile, methacrylic acid, acetaldehyde, and vinyl alcohol; III. The mass ratio of the monomer 1 to the monomer 2 is 0.1:1~3:1; the mass ratio of the water to the monomer 1 is 5~100; IV. The catalyst is selected from one or more of hydrochloric acid, formic acid, ammonia, sulfuric acid, oxalic acid, carbonic acid, citric acid, and acetic acid; V. the pH range is 1 to 7; VI. The amount of the conductive agent is 1% to 30% of the mass of the polymer material; VII. The amount of the lithium-philic substance is 1% to 10% of the mass of the polymer material; VIII. The mass ratio of the water to the polymer material is 2 to 10; Ⅸ. The dispersant is selected from any one of polyacrylate, polyvinyl ester, sodium tripolyphosphate, sodium pyrophosphate, sodium citrate, cellulose, polyvinyl pyrrolidone, polyvinyl alcohol, polycarboxylic acid and ethanol; X. The stirring time for mixing the polymer materials in the preparation of the three-dimensional skeleton material is 10-60 minutes.

7. The preparation method according to claim 5, characterized in that: The preparation method satisfies at least one of the following conditions: i. The mass ratio of the inorganic solid electrolyte to the three-dimensional framework material is 1:3~1:15; ii. The inorganic solid electrolyte and the three-dimensional framework material are mixed with water, wherein the amount of water is 3 to 10 times the mass of the three-dimensional framework material; iii. The mass proportion of the three-dimensional skeleton material doped with the inorganic solid electrolyte in the slurry is 70% to 90%, and the mass proportion of the binder in the slurry is 5% to 10%.

8. The preparation method according to any one of claims 5 to 7, characterized in that: At least one of the following conditions is met: ① The mixing method of the three-dimensional skeleton material and the inorganic solid electrolyte includes any one of direct mixing, VC mixing, wet mixing, and ball milling; ② The binder is any one or more of polyvinylidene fluoride, polyacrylic acid, polyamide, LA133, polyvinyl alcohol, polyethyleneimine, polyimide, polyethylene, SBR, and sodium carboxymethyl cellulose; ③ The conductive agent is selected from any one or more of SP, graphite, acetylene black, carbon nanotubes, graphene, and Ketjen black; ④ The solvent is any one of NMP, DMF, and water; ⑤ The composite method includes any one of cold rolling, hot rolling, rolling and extrusion.

9. A lithium ion battery, characterized in that: The invention comprises the lithium metal composite negative electrode as described in any one of claims 1 to 4.