A photocatalytic hydrogen production nanomaterial and preparation method thereof

By synthesizing nanotitanium dioxide at low temperature in porous gel support and combining it with molybdenum sulfide, the problem of low efficiency of titanium dioxide in sunlight is solved, and the photocatalytic hydrogen production efficiency is significantly improved.

CN118649693BActive Publication Date: 2024-11-15INNER MONGOLIA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411118313.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-15
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Titanium dioxide is low in efficiency as a photocatalyst under sunlight, and uneven dispersion after doping leads to a reduction in catalytic active sites and a reduction in hydrogen production efficiency.

Method used

Nanotitanium dioxide was synthesized at low temperature using a porous gel support, combined with molybdenum sulfide, uniformly distributed through cetyltrimethylammonium and glucose additives, and high-temperature reaction was carried out using thioacetamide and siligotungstic acid to form photocatalytic hydrogen production Nanomaterial MOS2@TiO2.

Benefits of technology

The uniform distribution of nanotitanium dioxide in the gel is achieved, the catalytic active sites are improved, and the photocatalytic hydrogen production efficiency is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118649693B_ABST
    Figure CN118649693B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of photocatalytic nanomaterials, and in particular to a photocatalytic hydrogen production nanomaterial and a preparation method thereof, wherein the preparation method adopts the following steps: S1, mixing deionized water and isopropanol, adjusting the pH and dropping titanium tetrachloride, placing a porous gel in the mixed solution and soaking for 0.5-2h, adjusting the pH to 8-9, heating and heat preservation to obtain a porous gel loaded with nano titanium dioxide; S2, dissolving sodium molybdate in a mixed solution of hexadecyltrimethylammonium, glucose and deionized water, adjusting the pH to 9-11, placing the porous gel loaded with nano titanium dioxide prepared in step S1 in the aforementioned mixed solution and soaking for 2-4h to obtain a mixture; S3, placing the mixture in step S2 in a reactor, adding thioacetamide and silicotungstic acid thereto and heating and reacting to obtain a product. The titanium dioxide and molybdenum sulfide prepared by the present invention are evenly combined, have many catalytic active sites, and have high hydrogen production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photocatalytic nanomaterials, and in particular to a photocatalytic hydrogen production nanomaterial and a preparation method thereof. Background Art

[0002] The semiconductor material titanium dioxide can completely degrade organic matter in the environment into water and carbon dioxide under ultraviolet light. It has the advantages of stable chemical properties, good acid and alkali resistance, non-toxicity, low cost, and good catalytic performance. It is the most widely used photocatalyst. However, because titanium dioxide is a wide-bandgap semiconductor, it has a low visible light response and can only absorb 3% of ultraviolet light in sunlight. In addition, the recombination probability of photogenerated electrons and holes in titanium dioxide is relatively high, which greatly limits the photocatalytic efficiency of titanium dioxide under sunlight.

[0003] Therefore, in order to solve these problems of nano titanium dioxide, titanium dioxide is doped, such as copper, gold, molybdenum and other elements, to improve the catalytic effect of titanium dioxide. However, when preparing nano titanium dioxide doped with other elements, the dispersion is uneven, it is easy to agglomerate, and the catalytic active sites are reduced, resulting in a decrease in the hydrogen production efficiency of the prepared nanomaterial. To this end, in view of the problems raised in the above background technology, those skilled in the art have proposed a photocatalytic hydrogen production nanomaterial and a preparation method thereof. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a photocatalytic hydrogen production nanomaterial and a preparation method thereof to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing a photocatalytic hydrogen-producing nanomaterial comprises the following steps:

[0007] S1. Deionized water and isopropanol are mixed, and 37%wt concentrated hydrochloric acid is added dropwise to adjust the pH to 1-3 to obtain a mixed solution, 1 mol / L titanium tetrachloride solution is slowly added dropwise to the mixed solution, an ice bath is maintained during the addition process, and then the porous gel is placed in the mixed solution and soaked for 0.5-2 hours, and then 25% ammonia water is continuously added dropwise to the mixed solution, the pH is adjusted to 8-9, and the solution is heated to 55-65°C and kept warm for 1-3 hours, and then the solution is allowed to stand at room temperature for 10-15 hours to obtain a porous gel loaded with nano-titanium dioxide;

[0008] S2, dissolving sodium molybdate in a mixed solution of hexadecyltrimethylammonium, glucose and deionized water, adding 5 mol / L sodium hydroxide solution to adjust the pH to 9-11, and placing the porous gel loaded with nano-titanium dioxide prepared in step S1 into the mixed solution and soaking for 2-4 hours to obtain a mixture;

[0009] S3, putting the mixture in step S2 into a reactor, adding thioacetamide and silicotungstic acid thereto, heating to 150-250°C, reacting for 12-24 hours, after the reaction is completed, filtering out the product and washing it with deionized water, calcining it at 400-600°C for 2-5 hours under a nitrogen atmosphere, and obtaining a photocatalytic hydrogen production nanomaterial (M O S2@TiO2).

[0010] Furthermore, the porous gel in step S1 is prepared by the following method:

[0011] S101: adding EDTA, ethylene oxide and agar into deionized water at 95° C., stirring and mixing until completely dissolved, to obtain a gel solution;

[0012] S102: The gel solution prepared in step S101 is placed in a freezer at -25 to -35°C for 3 to 4 hours to obtain a porous gel.

[0013] Furthermore, in step S101, the mass ratio of EDTA, ethylene oxide, agar and deionized water is 1:(0.2-0.4):(2-3):(20-24).

[0014] Furthermore, in step S1, the mass ratio of titanium tetrachloride, deionized water and isopropanol is 1:(25-35):(5-7).

[0015] Furthermore, in step S2, the mass ratio of sodium molybdate, hexadecyltrimethylammonium, glucose and deionized water is 1:(0.5-1):(1-3):(90-140).

[0016] Furthermore, the mass ratio of the titanium tetrachloride solution used in step S1 to the sodium molybdate used in step S2 is 1:(0.3-0.6).

[0017] Furthermore, the mass ratio of thioacetamide and silicotungstic acid in step S3 to sodium molybdate in step S2 is 1:(0.5-2):1.

[0018] A photocatalytic hydrogen production nano material is prepared according to the photocatalytic hydrogen production nano material preparation method.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The present invention synthesizes nano titanium dioxide at a relatively low temperature, and the process of synthesizing nano titanium dioxide is completed in the gel. The nano titanium dioxide is evenly distributed in the gel. With the addition of hexadecyltrimethylammonium and glucose, nano molybdenum sulfide can be synthesized on the titanium dioxide in the gel, and the synthesis process is simple.

[0021] 2. The present invention prepares nano-catalytic hydrogen production materials by synthesizing titanium dioxide and molybdenum sulfide. Titanium dioxide and molybdenum sulfide are evenly combined and have many catalytic active sites. The prepared nano-hydrogen production material has a strong photocatalytic effect and is suitable for promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a process flow chart of the photocatalytic hydrogen production nanomaterial prepared in the present invention;

[0023] Figure 2 is a process flow chart for preparing porous gel in the present invention;

[0024] Figure 3 The photocatalytic hydrogen production nanomaterial (M) prepared in Example 1 of the present invention O XRD pattern of S2@TiO2);

[0025] Figure 4 This is the SEM image of nano-titanium dioxide;

[0026] Figure 5 This is the SEM image of nano-molybdenum sulfide;

[0027] Figure 6 The photocatalytic hydrogen production nanomaterial (M) prepared in Example 1 of the present invention O SEM image of S2@TiO2). DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] See also Figure 1-6 , the present invention provides a technical solution:

[0030] Example 1

[0031] A method for preparing a photocatalytic hydrogen-producing nanomaterial comprises the following steps:

[0032] S1. 156 g of deionized water and 31.2 g of isopropanol were mixed, and concentrated hydrochloric acid with a mass fraction of 37% was added dropwise to adjust the pH to 1.5 to obtain a mixed solution, 5.2 g of a titanium tetrachloride solution with a concentration of 1 mol / L was slowly added dropwise to the mixed solution, and an ice bath was maintained during the dropping process. Then 15 g of the porous gel was placed in the mixed solution and soaked for 1.4 h, and then 25% ammonia water was continuously added dropwise to the mixed solution, and the pH was adjusted to 8. The solution was heated to 60° C. and kept warm for 2.5 h, and then continued to stand at room temperature for 14 h to obtain a porous gel loaded with nano-titanium dioxide;

[0033] S2, dissolving 2.1 g of sodium molybdate in a mixed solution of 1.9 g of hexadecyltrimethylammonium, 4.3 g of glucose and 225 g of deionized water, adding 5 mol / L of sodium hydroxide solution to adjust the pH to 10, and placing the porous gel loaded with nano-titanium dioxide prepared in step S1 into the aforementioned mixed solution and soaking for 3 h to obtain a mixture;

[0034] S3, putting the mixture in step S2 into a reactor, adding 2.1 g of thioacetamide and 3.2 g of silicotungstic acid, heating to 220° C., reacting for 18 h, filtering out the product after the reaction is completed, washing with deionized water, and calcining at 550° C. for 4.5 h under a nitrogen atmosphere to obtain a photocatalytic hydrogen production nanomaterial;

[0035] The porous gel is prepared by the following method:

[0036] S101: Add 6.2 g EDTA, 1.8 g ethylene oxide and 17.5 g agar into 134 g deionized water at 95° C., and stir to mix until completely dissolved to obtain a gel solution;

[0037] S102: The gel solution prepared in step S101 is placed in a freezer at -32°C for 3.6 hours to obtain a porous gel.

[0038] Figure 3 The XRD pattern of the photocatalytic hydrogen production material prepared in Example 1 is shown in FIG. O S2@TiO2 was successfully synthesized. Figure 6 The middle is M O SEM image of S2@TiO2, TiO2 and M O S2 is evenly combined and the hydrogen production efficiency is improved.

[0039] Example 2

[0040] A method for preparing a photocatalytic hydrogen-producing nanomaterial comprises the following steps:

[0041] S1. Mix 203 g of deionized water and 40.6 g of isopropanol, and add concentrated hydrochloric acid with a mass fraction of 37% to obtain a mixed solution, slowly add 5.8 g of a titanium tetrachloride solution with a concentration of 1 mol / L to the mixed solution, keep an ice bath during the dropping process, and then put 16 g of the porous gel into the mixed solution and soak for 2 hours, then continue to add ammonia water with a mass fraction of 25% to the mixed solution, adjust the pH to 9, heat to 65°C and keep warm for 1 hour, and then continue to stand at room temperature for 15 hours to obtain a porous gel loaded with nano-titanium dioxide;

[0042] S2, dissolving 3.5 g of sodium molybdate into a mixed solution of 3.5 g of hexadecyltrimethylammonium, 10.5 g of glucose and 490 g of deionized water, adding 5 mol / L of sodium hydroxide solution to adjust the pH to 11, and placing the porous gel loaded with nano-titanium dioxide prepared in step S1 into the aforementioned mixed solution and soaking for 4 hours to obtain a mixture;

[0043] S3, putting the mixture in step S2 into a reactor, adding 3.5 g of thioacetamide and 6.0 g of silicotungstic acid thereto, heating to 250° C., reacting for 24 h, after the reaction is completed, filtering out the product and washing it with deionized water, and calcining it at 600° C. for 5 h under a nitrogen atmosphere to obtain a photocatalytic hydrogen production nanomaterial;

[0044] The porous gel is prepared by the following method:

[0045] S101: Add 4.6 g EDTA, 1.84 g ethylene oxide and 13.8 g agar into 110 g deionized water at 95° C., and stir to mix until completely dissolved to obtain a gel solution;

[0046] S102: The gel solution prepared in step S101 is placed in a freezer at -35°C for 4 hours to obtain a porous gel.

[0047] Example 3

[0048] A method for preparing a photocatalytic hydrogen-producing nanomaterial comprises the following steps:

[0049] S1. 160 g of deionized water and 32 g of isopropanol were mixed, and concentrated hydrochloric acid with a mass fraction of 37% was added dropwise to adjust the pH to 1 to obtain a mixed solution, 6.4 g of a titanium tetrachloride solution with a concentration of 1 mol / L was slowly added dropwise to the mixed solution, and an ice bath was maintained during the dropping process. Then 14 g of the porous gel was placed in the mixed solution and soaked for 0.5 h, and then 25% ammonia water was continuously added dropwise to the mixed solution, and the pH was adjusted to 8. The solution was heated to 55° C. and kept warm for 3 h, and then continued to stand at room temperature for 10 h to obtain a porous gel loaded with nano-titanium dioxide;

[0050] S2, dissolving 1.9 g of sodium molybdate in a mixed solution of 0.95 g of hexadecyltrimethylammonium, 1.9 g of glucose and 171 g of deionized water, adding 5 mol / L of sodium hydroxide solution to adjust the pH to 9, and placing the porous gel loaded with nano-titanium dioxide prepared in step S1 into the aforementioned mixed solution and soaking for 2 h to obtain a mixture;

[0051] S3, putting the mixture in step S2 into a reactor, adding 1.9 g of thioacetamide and 0.8 g of silicotungstic acid thereto, heating to 150° C., reacting for 12 h, after the reaction is completed, filtering out the product and washing it with deionized water, and calcining it at 400° C. for 2 h under a nitrogen atmosphere to obtain a photocatalytic hydrogen production nanomaterial;

[0052] The porous gel is prepared by the following method:

[0053] S101: Add 5.8 g EDTA, 1.16 g ethylene oxide and 11.6 g agar into 116 g deionized water at 95° C., and stir to mix until completely dissolved to obtain a gel solution;

[0054] S102: The gel solution prepared in step S101 is placed in a freezer at -25°C for 3 hours to obtain a porous gel.

[0055] Example 4

[0056] A method for preparing a photocatalytic hydrogen-producing nanomaterial comprises the following steps:

[0057] S1. Mix 202 g of deionized water and 38.4 g of isopropanol, and add concentrated hydrochloric acid with a mass fraction of 37% to adjust the pH to 2 to obtain a mixed solution, slowly add 6.6 g of a titanium tetrachloride solution with a concentration of 1 mol / L to the mixed solution, keep an ice bath during the dropping process, and then put 18 g of the porous gel into the mixed solution and soak for 1.5 h, and then continue to add ammonia water with a mass fraction of 25% to the mixed solution, adjust the pH to 8.5, heat to 58°C and keep warm for 2.3 h, and then continue to stand at room temperature for 12 h to obtain a porous gel loaded with nano-titanium dioxide;

[0058] S2, dissolving 3.2 g of sodium molybdate into a mixed solution of 2.3 g of hexadecyltrimethylammonium, 6.3 g of glucose and 345 g of deionized water, adding 5 mol / L of sodium hydroxide solution to adjust the pH to 10, and placing the porous gel loaded with nano-titanium dioxide prepared in step S1 into the aforementioned mixed solution and soaking for 2.8 h to obtain a mixture;

[0059] S3, putting the mixture in step S2 into a reactor, adding 3.2 g of thioacetamide and 2.9 g of silicotungstic acid thereto, heating to 240° C., reacting for 22 h, after the reaction is completed, filtering out the product and washing it with deionized water, and calcining it at 500° C. for 3.6 h under a nitrogen atmosphere to obtain a photocatalytic hydrogen production nanomaterial;

[0060] The porous gel is prepared by the following method:

[0061] S101: Add 5.4 g EDTA, 1.84 g ethylene oxide and 12.3 g agar into 118 g deionized water at 95° C., and stir to mix until completely dissolved to obtain a gel solution;

[0062] S102: The gel solution prepared in step S101 is placed in a freezer at -30°C for 3.5 hours to obtain a porous gel.

[0063] Comparative Example 1

[0064] Comparative Example 1 is relative to Example 1, in which step S101 is omitted, thereby eliminating the addition of EDTA, and the remaining steps are exactly the same as those of Example 1.

[0065] Comparative Example 2

[0066] Comparative Example 2 is relative to Example 1, in which step S2 is omitted, thereby eliminating the addition of hexadecyltrimethylammonium and glucose, and the remaining steps are exactly the same as those of Example 1.

[0067] Comparative Example 3

[0068] Compared with Comparative Example 1, Comparative Example 3 also omitted step S2, thereby eliminating the addition of hexadecyltrimethylammonium and glucose, and the remaining steps are exactly the same as those of Comparative Example 1.

[0069] Comparative Example 4

[0070] Compared with Example 1, Comparative Example 4 eliminated the use of porous gel as a carrier to synthesize the composite material, and also eliminated the addition of hexadecyltrimethylammonium and glucose, and synthesized directly in the solution. The specific operation steps are as follows:

[0071] S1. 156 g of deionized water and 31.2 g of isopropanol were mixed, and concentrated hydrochloric acid with a mass fraction of 37% was added dropwise to adjust the pH to 1.5 to obtain a mixed solution, 5.2 g of a titanium tetrachloride solution with a concentration of 1 mol / L was slowly added dropwise to the mixed solution, and an ice bath was maintained during the dropping process. Then, 25% ammonia water was continued to be added dropwise to the mixed solution, and the pH was adjusted to 8. The solution was heated to 60° C. and kept warm for 2.5 h, and then allowed to stand at room temperature for 14 h to obtain a titanium dioxide sol;

[0072] S2, dissolving 2.1 g of sodium molybdate into the gel in step S1, adding 5 mol / L sodium hydroxide solution to adjust the pH to 10, to obtain a mixed sol;

[0073] S3. Put the mixture in step S2 into a reactor, add 2.1 g of thioacetamide and 3.2 g of silicotungstic acid, heat to 220°C, and react for 18 hours. After the reaction is completed, filter out the product and wash it with deionized water, and calcine it at 550°C for 4.5 hours under a nitrogen atmosphere to obtain a photocatalytic hydrogen production nanomaterial.

[0074] Through the above-mentioned Examples 1-4 and Comparative Examples 1-4, eight different photocatalytic hydrogen production nanomaterials were obtained, and hydrogen production efficiency experiments were conducted on different photocatalytic hydrogen production nanomaterials. The specific experiment was to take 20 mg of the photocatalytic hydrogen production nanomaterials prepared in Examples 1-4 and Comparative Examples 1-4, respectively, and ultrasonically disperse them into different portions of a mixed solution of deionized water, methanol and acetone, wherein the volume ratios of deionized water, methanol and acetone were 90 ml, 30 ml and 30 ml, respectively, and use a 350W xenon lamp as a light source for continuous irradiation for 5 hours, and determine the average hydrogen production efficiency per hour by gas chromatography. The specific test results are shown in Table 1 below:

[0075] Table 1: Hydrogen production efficiency of photocatalytic hydrogen production nanomaterials in various embodiments

[0076]

[0077] It can be seen from the data of Example 1 and Comparative Examples 1-4 in the above table that the nano hydrogen production material prepared by the present invention has a greatly improved hydrogen production efficiency.

[0078] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a photocatalytic hydrogen production nanomaterial, characterized in that: Use the following steps: S1. Deionized water and isopropanol are mixed, and 37%wt concentrated hydrochloric acid is added dropwise to adjust the pH to 1-3 to obtain a mixed solution, 1 mol / L titanium tetrachloride solution is slowly added dropwise to the mixed solution, an ice bath is maintained during the addition process, and then the porous gel is placed in the mixed solution and soaked for 0.5-2 hours, and then 25% ammonia water is continuously added dropwise to the mixed solution, the pH is adjusted to 8-9, and the solution is heated to 55-65°C and kept warm for 1-3 hours, and then the solution is allowed to stand at room temperature for 10-15 hours to obtain a porous gel loaded with nano-titanium dioxide; S2, dissolving sodium molybdate in a mixed solution of hexadecyltrimethylammonium, glucose and deionized water, adding 5 mol / L sodium hydroxide solution to adjust the pH to 9-11, and placing the porous gel loaded with nano-titanium dioxide prepared in step S1 into the mixed solution and soaking for 2-4 hours to obtain a mixture; S3, putting the mixture in step S2 into a reactor, adding thioacetamide and silicotungstic acid thereto, heating to 150-250° C., reacting for 12-24 hours, after the reaction is completed, filtering out the product and washing it with deionized water, and calcining it at 400-600° C. for 2-5 hours under a nitrogen atmosphere to obtain a photocatalytic hydrogen production nanomaterial; In step S1, the mass ratio of titanium tetrachloride, deionized water and isopropanol is 1:(25-35):(5-7); In step S2, the mass ratio of sodium molybdate, hexadecyltrimethylammonium, glucose and deionized water is 1:(0.5-1):(1-3):(90-140); The mass ratio of the titanium tetrachloride solution used in step S1 to the sodium molybdate used in step S2 is 1:(0.3-0.6); The mass ratio of thioacetamide and silicotungstic acid in step S3 to sodium molybdate in step S2 is 1:(0.5-2):1; The porous gel in step S1 is prepared by the following method: S101: adding EDTA, ethylene oxide and agar into deionized water at 95° C., stirring and mixing until completely dissolved, to obtain a gel solution; S102: The gel solution prepared in step S101 is placed in a freezer at -25 to -35°C for 3 to 4 hours to obtain a porous gel.

2. The method for preparing a photocatalytic hydrogen production nanomaterial according to claim 1, characterized in that: In step S101, the mass ratio of EDTA, ethylene oxide, agar and deionized water is 1:(0.2-0.4):(2-3):(20-24).

3. A photocatalytic hydrogen production nanomaterial, characterized in that: The photocatalytic hydrogen production nanomaterial is prepared according to the method for preparing the photocatalytic hydrogen production nanomaterial according to any one of claims 1-2.