A method for regenerating silicon-based low-removal wafer

Through physical film removal methods of grinding, pre-polishing, medium polishing and fine polishing, the problem of major damage in traditional silicon wafer regeneration methods is solved, and the surface treatment of low loss and low pollution of silicon wafers is achieved, suitable for low removal quantity of regeneration operations within the fab.

CN118650502BActive Publication Date: 2024-12-03ZHEJIANG HOUJI TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411148113.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-12-03
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

Traditional silicon wafer regeneration film removal methods such as thinner removal and chemical film removal will cause major damage and are not suitable for low-damage wafer recycling operations, especially in wafer baffles, control panels and During the regeneration process of the test piece.

Method used

Using physical film removal methods of grinding, pre-polishing, medium-polishing and fine polishing, the material on the surface of the silicon wafer is gradually removed through the combination of atomizing grinding, polishing liquid and polishing pads, and the material on the surface of the silicon wafer is gradually removed to achieve low loss and low pollution surface treatment. .

Benefits of technology

Achieve low damage silicon wafer surface treatment, reducing loss and chip rate during processing, suitable for regeneration operations within wafer fabs with low removal volume, meeting the required roughness requirements and reducing contamination .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118650502B_ABST
    Figure CN118650502B_ABST
Patent Text Reader

Abstract

The invention provides a regeneration method for a silicon-based low-removal wafer, comprising the following steps: step 1: atomizing and grinding the silicon wafer by a grinding device, with a removal amount of 1-2 um; step 2: pre-polishing the silicon wafer by a polishing device, with a removal amount of 0.2-0.5 um; step 3: intermediate polishing the silicon wafer by a polishing device, with a removal amount of 3-4 um; step 4: fine polishing the silicon wafer by a polishing device, with a removal amount of 0.1-0.3 um.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon wafer processing methods, and in particular to a regeneration method for silicon-based low-removal wafers. Background Art

[0002] Silicon wafer: Wafer is the silicon element that has been purified (99.999%), and then the pure silicon is made into long silicon crystal rods, which become the material for quartz semiconductors for manufacturing integrated circuits. After processes such as photolithography, grinding, polishing, and slicing, the polycrystalline silicon is melted and pulled out into single-crystal silicon crystal rods, and then cut into thin wafers. The traditional method of silicon wafer regeneration and film removal is to remove it with a thinner or chemical film removal, but both methods will cause a large damage layer, which needs to be removed through subsequent CMP polishing. A thickness of 20-30um needs to be removed, resulting in a large loss of silicon base and a small number of regeneration times. Moreover, such a large removal method is not suitable for low-damage silicon wafer recovery operations such as baffles, control wafers, and test wafers in the wafer factory. Summary of the invention

[0003] To achieve the above object, the present invention provides the following technical solutions:

[0004] A method for regenerating a silicon-based low-removal wafer comprises the following steps: step one: atomizing and grinding the silicon wafer by a grinding device, with a removal amount of 1-2um; step two: pre-polishing the silicon wafer by a polishing device, with a removal amount of 0.2-0.5um; step three: intermediate polishing the silicon wafer by a polishing device, with a removal amount of 3-4um; step four: fine polishing the silicon wafer by a polishing device, with a removal amount of 0.1-0.3um.

[0005] Compared with the prior art, the present invention has the following beneficial effects:

[0006] The present invention can remove low-damage silicon wafer surfaces through grinding, pre-polishing, medium polishing and fine polishing. Compared with thinning machine removal or high-removal chemical film removal, the present solution adopts a physical film removal method, which has less loss during the processing and can also meet the required roughness requirements. It has lower pollution than the chemical film removal method, and the breakage rate during the processing can be reduced, thereby reducing the loss during the processing. Through this process, a minimum removal amount of only 4.3um can be achieved, which is suitable for recycled wafers such as baffles, control wafers and test wafers in wafer factories with low removal amounts.

[0007] Preferably, in step 1, the downward pressure of the grinding head is 40-50 kg, the rotation speed is 20-30 rpm, and the processing time is 240 seconds.

[0008] Preferably, in step one, a grinding liquid is used on the grinding equipment, the components of the grinding liquid are water and silicon carbide particles with a particle size of 10-12 um, the silicon carbide accounts for 20%-30% of the water component, and the flow rate of the grinding liquid is 2-4 cc / s.

[0009] Preferably, in step 2, the downward pressure of the polishing head is 8-10 kg, the rotation speed of the polishing head is 300-350 rpm, and the processing time is 2400 seconds.

[0010] Preferably, in step 2, a polishing liquid is used on the polishing equipment, and the components of the polishing liquid are: SiO2 particles, tetramethylammonium hydroxide and a chelating agent, the particle size of the SiO2 particles is 80-120um, the flow rate of the polishing liquid is: 8-10cc / s, and the ratio of SiO2 particles, tetramethylammonium hydroxide and chelating agent is 100:10:1.

[0011] Preferably, in step 2, a polishing pad is used on the polishing disc surface, and the polishing pad is a non-woven fabric impregnated with polyurethane, and the polishing disc surface does not rotate at this time.

[0012] Preferably, in step three, the rotation speed of the polishing head is 20-30 rpm, the downward pressure of the polishing head is 80-100 kg, the rotation speed of the polishing disk is 40-60 rpm, and the processing time is 240 seconds.

[0013] Preferably, in step three, a polishing liquid is used on the polishing equipment, and the components of the polishing liquid are: silica sol, tetramethylammonium hydroxide and chelating agent, the flow rate of the polishing liquid is 8-10cc / s, the particle size of the silica sol is 80-120um, and the composition ratio of silica sol, tetramethylammonium hydroxide and chelating agent is 100:10:1.

[0014] Preferably, in step three, a polishing pad is used on the polishing disc surface, and the material of the polishing pad is non-woven fabric impregnated with polyurethane.

[0015] Preferably, in step 4, the rotation speed of the polishing head is 15-30 rpm, the downward pressure of the polishing head is 30-40 kg, the rotation speed of the polishing disk surface is 40-60 rpm, and the processing time is 240 seconds.

[0016] Preferably, in step four, a polishing liquid is used on the polishing equipment, and the components of the polishing liquid are: silica sol, tetramethylammonium hydroxide and chelating agent, the flow rate of the polishing liquid is 12-15cc / s, the particle size of the silica sol is 30-60um, and the composition ratio of silica sol, tetramethylammonium hydroxide and chelating agent is 150:10:1.

[0017] Preferably, in step 4, a porous polyurethane polishing pad is used on the polishing equipment.

[0018] Preferably, the rotation direction of the polishing disk surface is opposite to the rotation direction of the polishing head. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The present invention is a logic block diagram of a method for regenerating a silicon-based low-removal wafer. DETAILED DESCRIPTION

[0020] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them.

[0021] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents some embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0022] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features and technical solutions in the embodiments may be combined with each other.

[0023] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0024] In the description of the present invention, it should be noted that the orientation or positional relationship indicated by the terms "upper", "lower", etc. is based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the invention product is usually placed when in use, or the orientation or positional relationship commonly understood by those skilled in the art. Such terms are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.

[0025] The present invention is further described in detail below:

[0026] Embodiment 1: A method for regenerating a silicon-based low-removal wafer, comprising the following steps:

[0027] Step 1: The silicon wafer is subjected to atomization grinding by a grinding device, and the removal amount is 1um; after grinding, the surface of the wafer is matte, and the roughness is 60nm;

[0028] Step 2: Pre-polish the silicon wafer using a polishing device, removing 0.2um; polish the wafer matte surface to a bright surface with a roughness of 5nm;

[0029] Step 3: Use a polishing device to perform intermediate polishing on the silicon wafer, with a removal amount of 3um and a roughness of 0.8nm;

[0030] Step 4: Fine-polish the silicon wafer using polishing equipment, removing 0.1um, and further improve the polishing effect to a roughness of 0.2nm.

[0031] The present invention can remove low-damage silicon wafer surfaces through grinding, pre-polishing, medium polishing and fine polishing. Compared with thinning machine removal or high-removal chemical film removal, the present solution adopts a physical film removal method, which has less loss during the processing and can also meet the required roughness requirements. It has lower pollution than the chemical film removal method, and the breakage rate during the processing can be reduced, thereby reducing the loss during the processing. Through this process, only 4.3um of removal can be achieved, which is suitable for recycled wafers such as baffles, control wafers and test wafers in wafer factories with low removal volumes.

[0032] In this embodiment, in step 1, the downward force of the grinding head is 40 kg, the rotation speed is 20 rpm, and the processing time is 240 seconds.

[0033] In this embodiment, in step one, a grinding liquid is used on the grinding equipment. The components of the grinding liquid are water and silicon carbide particles with a particle size of 10, silicon carbide accounts for 20% of the water component, and the flow rate of the grinding liquid is 2cc / s.

[0034] In this embodiment, in step 2, the downward pressure of the polishing head is 8 kg, the rotation speed of the polishing head is 300 rpm, and the processing time is 2400 seconds.

[0035] In this embodiment, in step 2, a polishing liquid is used on the polishing equipment, and the components of the polishing liquid are: SiO2 particles, tetramethylammonium hydroxide and a chelating agent. The particle size of the SiO2 particles is 80um, the flow rate of the polishing liquid is 8cc / s, and the ratio of SiO2 particles, tetramethylammonium hydroxide and the chelating agent is 100:10:1.

[0036] In this embodiment, in step 2, a polishing pad is used on the polishing disc surface, and the polishing pad is a non-woven fabric impregnated with polyurethane.

[0037] In this embodiment, in step three, the rotation speed of the polishing head is 20 rpm, the downward pressure of the polishing head is 80 kg, the rotation speed of the polishing disk is 40 rpm, and the processing time is 240 seconds.

[0038] In this embodiment, in step three, a polishing liquid is used on the polishing equipment, and the components of the polishing liquid are: silica sol, tetramethylammonium hydroxide and a chelating agent. The flow rate of the polishing liquid is 8cc / s, the particle size of the silica sol is 80um, and the composition ratio of the silica sol, tetramethylammonium hydroxide and the chelating agent is 100:10:1.

[0039] In this embodiment, in step three, a polishing pad is used on the polishing disk surface, and the material of the polishing pad is non-woven fabric impregnated with polyurethane.

[0040] In this embodiment, in step four, the rotation speed of the polishing head is 15rpm, the downward pressure of the polishing head is 30kg, the rotation speed of the polishing disk is 40rpm, and the processing time is 240 seconds. In this way, the polishing disk can drive the polishing pad and the silicon wafer to rotate together to improve the polishing effect.

[0041] In this embodiment, in step four, a polishing liquid is used on the polishing equipment, and the components of the polishing liquid are: silica sol, tetramethylammonium hydroxide and a chelating agent. The flow rate of the polishing liquid is 12cc / s, the particle size of the silica sol is 30um, and the composition ratio of the silica sol, tetramethylammonium hydroxide and the chelating agent is 150:10:1.

[0042] In this embodiment, in step 4, a porous polyurethane polishing pad is used on the polishing equipment.

[0043] In this embodiment, the diameter of the silicon wafer is 8-10 inches.

[0044] In this embodiment, the grinding device and the polishing device are both existing structures and will not be described in detail here. The grinding head adopts an aluminum alloy grinding head.

[0045] Embodiment 2: A method for regenerating a silicon-based low-removal wafer, comprising the following steps:

[0046] Step 1: The silicon wafer is subjected to atomization grinding by a grinding device, and the removal amount is 1.5um; after grinding, the surface of the wafer is matte, and the roughness is 52nm;

[0047] Step 2: Pre-polish the silicon wafer using a polishing device, removing 0.35um; polish the wafer matte surface to a bright surface with a roughness of 6nm;

[0048] Step 3: Use a polishing device to perform intermediate polishing on the silicon wafer, with a removal amount of 3.5um and a roughness of 0.6nm;

[0049] Step 4: Fine-polish the silicon wafer using polishing equipment, removing 0.15um, and further improve the polishing effect to a roughness of 0.15nm.

[0050] The present invention can remove low-damage silicon wafer surfaces through grinding, pre-polishing, medium polishing and fine polishing. Compared with thinning machine removal or high-removal chemical film removal, the present solution adopts a physical film removal method, which has less loss during the processing and can also meet the required roughness requirements. It has lower pollution than the chemical film removal method, and the breakage rate during the processing can be reduced, thereby reducing the loss during the processing. Through this process, only 5.5um of removal can be achieved, which is suitable for recycled wafers such as baffles, control wafers and test wafers in wafer factories with low removal volumes.

[0051] In this embodiment, in step 1, the downward pressure of the grinding head is 45 kg, the rotation speed is 25 rpm, and the processing time is 240 seconds.

[0052] In this embodiment, in step 1, a grinding liquid is used on the grinding equipment. The components of the grinding liquid are water and silicon carbide particles with a particle size of 11 um, silicon carbide accounts for 25% of the water component, and the flow rate of the grinding liquid is 3 cc / s.

[0053] In this embodiment, in step 2, the downward pressure of the polishing head is 9 kg, the rotation speed of the polishing head is 325 rpm, and the processing time is 2400 seconds.

[0054] In this embodiment, in step 2, a polishing liquid is used on the polishing equipment, and the components of the polishing liquid are: SiO2 particles, tetramethylammonium hydroxide and a chelating agent. The particle size of the SiO2 particles is 100um, the flow rate of the polishing liquid is 9cc / s, and the ratio of SiO2 particles, tetramethylammonium hydroxide and the chelating agent is 100:10:1.

[0055] In this embodiment, in step 2, a polishing pad is used on the polishing disc surface, and the polishing pad is a non-woven fabric impregnated with polyurethane.

[0056] In this embodiment, in step three, the rotation speed of the polishing head is 25 rpm, the downward pressure of the polishing head is 90 kg, the rotation speed of the polishing disk is 50 rpm, and the processing time is 240 seconds.

[0057] In this embodiment, in step three, a polishing liquid is used on the polishing equipment, and the components of the polishing liquid are: silica sol, tetramethylammonium hydroxide and a chelating agent. The flow rate of the polishing liquid is 9cc / s, the particle size of the silica sol is 100um, and the composition ratio of the silica sol, tetramethylammonium hydroxide and the chelating agent is 100:10:1.

[0058] In this embodiment, in step three, a polishing pad is used on the polishing disk surface, and the material of the polishing pad is non-woven fabric impregnated with polyurethane.

[0059] In this embodiment, in step four, the rotation speed of the polishing head is 22.5rpm, the downward pressure of the polishing head is 35kg, the rotation speed of the polishing disk is 50rpm, and the processing time is 240 seconds. In this way, the polishing disk can drive the polishing pad and the silicon wafer to rotate together to improve the polishing effect.

[0060] In this embodiment, in step four, a polishing liquid is used on the polishing equipment, and the components of the polishing liquid are: silica sol, tetramethylammonium hydroxide and a chelating agent. The flow rate of the polishing liquid is 13.5cc / s, the particle size of the silica sol is 45um, and the composition ratio of the silica sol, tetramethylammonium hydroxide and the chelating agent is 150:10:1.

[0061] In this embodiment, in step 4, a porous polyurethane polishing pad is used on the polishing equipment.

[0062] In this embodiment, the diameter of the silicon wafer is 8-10 inches.

[0063] In this embodiment, the grinding device and the polishing device are both existing structures and will not be described in detail here. The grinding head adopts an aluminum alloy grinding head.

[0064] Embodiment 3: A method for regenerating a silicon-based low-removal wafer, comprising the following steps:

[0065] Step 1: The silicon wafer is subjected to atomization grinding by a grinding device, and the removal amount is 2um; after grinding, the surface of the wafer is matte, and the roughness is 45nm;

[0066] Step 2: Pre-polish the silicon wafer using a polishing device, removing 0.5um; polish the wafer matte surface to a bright surface with a roughness of 1nm;

[0067] Step 3: Use a polishing device to perform intermediate polishing on the silicon wafer, with a removal amount of 4um and a roughness of 0.4nm;

[0068] Step 4: Fine-polish the silicon wafer using polishing equipment, removing 0.3um, and further improve the polishing effect to a roughness of 0.1nm.

[0069] The present invention can remove low-damage silicon wafer surfaces through grinding, pre-polishing, medium polishing and fine polishing. Compared with thinning machine removal or high-removal chemical film removal, the present solution adopts a physical film removal method, which has less loss during the processing and can also meet the required roughness requirements. It has lower pollution than the chemical film removal method, and the breakage rate during the processing can be reduced, thereby reducing the loss during the processing. Through this process, only 6.8um of removal can be achieved, which is suitable for recycled wafers such as baffles, control wafers and test wafers in wafer factories with low removal volumes.

[0070] In this embodiment, in step 1, the downward force of the grinding head is 50 kg, the rotation speed is 30 rpm, and the processing time is 240 seconds.

[0071] In this embodiment, in step one, a grinding liquid is used on the grinding equipment. The components of the grinding liquid are water and silicon carbide particles with a particle size of 12 um, silicon carbide accounts for 30% of the water component, and the flow rate of the grinding liquid is 4 cc / s.

[0072] In this embodiment, in step 2, the downward pressure of the polishing head is 10 kg, the rotation speed of the polishing head is 350 rpm, and the processing time is 2400 seconds.

[0073] In this embodiment, in step 2, a polishing liquid is used on the polishing equipment, and the components of the polishing liquid are: SiO2 particles, tetramethylammonium hydroxide and a chelating agent. The particle size of the SiO2 particles is 120um, the flow rate of the polishing liquid is 10cc / s, and the ratio of SiO2 particles, tetramethylammonium hydroxide and the chelating agent is 100:10:1.

[0074] In this embodiment, in step 2, a polishing pad is used on the polishing disc surface, and the polishing pad is a non-woven fabric impregnated with polyurethane.

[0075] In this embodiment, in step three, the rotation speed of the polishing head is 30 rpm, the downward pressure of the polishing head is 100 kg, the rotation speed of the polishing disk is 60 rpm, and the processing time is 240 seconds.

[0076] In this embodiment, in step three, a polishing liquid is used on the polishing equipment, and the components of the polishing liquid are: silica sol, tetramethylammonium hydroxide and a chelating agent. The flow rate of the polishing liquid is 10cc / s, the particle size of the silica sol is 120um, and the composition ratio of the silica sol, tetramethylammonium hydroxide and the chelating agent is 100:10:1.

[0077] In this embodiment, in step three, a polishing pad is used on the polishing disk surface, and the material of the polishing pad is non-woven fabric impregnated with polyurethane.

[0078] In this embodiment, in step four, the rotation speed of the polishing head is 30rpm, the downward pressure of the polishing head is 40kg, the rotation speed of the polishing disk is 60rpm, and the processing time is 240 seconds. In this way, the polishing disk can drive the polishing pad and the silicon wafer to rotate together to improve the polishing effect.

[0079] In this embodiment, in step four, a polishing liquid is used on the polishing equipment, and the components of the polishing liquid are: silica sol, tetramethylammonium hydroxide and a chelating agent. The flow rate of the polishing liquid is 15cc / s, the particle size of the silica sol is 60um, and the composition ratio of the silica sol, tetramethylammonium hydroxide and the chelating agent is 150:10:1.

[0080] In this embodiment, in step 4, a porous polyurethane polishing pad is used on the polishing equipment.

[0081] In this embodiment, the diameter of the silicon wafer is 8-10 inches.

[0082] In this embodiment, the grinding device and the polishing device are both existing structures and will not be described in detail here. The grinding head adopts an aluminum alloy grinding head.

[0083] Although the embodiments of the present invention have been shown and described, it is understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the attached claims and their equivalents. The above embodiments are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention. Although the present invention has been described in detail with reference to the above embodiments, the present invention is not limited to the above specific implementation methods. Therefore, any modification or equivalent substitution of the present invention; and all technical solutions and improvements that do not depart from the spirit and scope of the invention are included in the scope of the claims of the present invention.

Claims

1. A method for regenerating a silicon-based low-removal wafer, characterized in that: The following steps are involved: Step 1: The silicon wafer is atomized and ground by a grinding device, and the removal amount is 1-2um; the downward pressure of the grinding head is 40-50kg, the rotation speed is 20-30rpm, and the processing time is 240 seconds; the grinding device uses a grinding liquid, which is composed of water and silicon carbide particles with a particle size of 10-12um, with silicon carbide accounting for 20%-30% of the water component, and the flow rate of the grinding liquid is 2-4cc / s; Step 2: Pre-polishing the silicon wafer by polishing equipment, the removal amount is 0.2-0.5um, the downward pressure of the polishing head is 8-10kg, the speed of the polishing head is 300-350rpm, the processing time is 2400 seconds, and the polishing liquid is used on the polishing equipment. The components of the polishing liquid are: SiO2 particles, tetramethylammonium hydroxide and chelating agent. The particle size of SiO2 particles is 80-120um, the flow rate of the polishing liquid is 8-10cc / s, and the ratio of SiO2 particles, tetramethylammonium hydroxide and chelating agent is 100:10:1; Step 3: The silicon wafer is subjected to intermediate polishing by a polishing device, the removal amount is 3-4um, the rotation speed of the polishing head is 20-30rpm, the downward pressure of the polishing head is 80-100kg, the rotation speed of the polishing disk is 40-60rpm, the processing time is 240 seconds, and a polishing liquid is used on the polishing device. The components of the polishing liquid are: silica sol, tetramethylammonium hydroxide and chelating agent, the flow rate of the polishing liquid is 8-10cc / s, the particle size of the silica sol is 80-120um, and the composition ratio of the silica sol, tetramethylammonium hydroxide and chelating agent is 100:10:1; Step 4: Fine polish the silicon wafer through polishing equipment, the removal amount is 0.1-0.3um, the rotation speed of the polishing head is 15-30rpm, the downward pressure of the polishing head is 30-40kg, the rotation speed of the polishing disk is 40-60rpm, the processing time is 240 seconds, and the composition of the polishing liquid is: silica sol, tetramethylammonium hydroxide and chelating agent. The flow rate of the polishing liquid is 12-15cc / s, the particle size of the silica sol is 30-60um, and the composition ratio of silica sol, tetramethylammonium hydroxide and chelating agent is 150:10:1.

Citation Information

Patent Citations

  • Polishing method for zinc oxide single crystal substrate level substrate

    CN101125416A

  • Semiconductor silicon wafer manufacture process

    CN101791779A

  • Silicon dioxide-based CMP (Chemical Mechanical Polishing) solution and preparation method thereof

    CN102796460A

  • Chemical mechanical polishing solution

    CN104559800A

  • Silicon-wafer polishing composition and silicon-wafer polishing method

    WO2011142362A1