A heat-resistant polyethylene film with high water vapor barrier properties and a preparation method thereof
Through the stacking structure and micro-nano stacking technology of modified high-density polyethylene and modified low-density polyethylene, the problems of insufficient heat resistance and water vapor barrier properties of polyethylene films are solved, and efficient thermal stability and water are achieved Improved vapor barrier performance.
Patent Information
- Application Number
- CN202411125373.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The existing polyethylene films have poor heat resistance and water vapor barrier properties and cannot meet certain application needs.
Modified high-density polyethylene and modified low-density polyethylene are used to alternately combine the polyethylene film with a layer structure of 25~1025 layers through a laminate. The preparation materials for modified high-density polyethylene include high-density polyethylene and bicyclic heptane. The preparation materials for modified low-density polyethylene include low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2- [[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]vinylamine, the thermal stability and water vapor barrier properties of the film are improved through micro-nano lamination technology and unidirectional stretching process.
It significantly improves the heat resistance and water vapor barrier properties of polyethylene films, ensuring that they can effectively block water vapor at high temperatures, and is suitable for application scenarios where high performance is required.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyethylene films, and in particular to a heat-resistant polyethylene film with high water vapor barrier properties and a preparation method thereof. Background Art
[0002] Polyethylene film refers to a film produced from polyethylene material. Polyethylene film has a very wide range of uses. CN108752689A discloses a high melting point heat-resistant transparent polyethylene film, but it has the problem of poor water vapor barrier properties. CN101631826A discloses the barrier properties of a substantially linear HDPE film containing a nucleating agent, but when the polyethylene film uses hexahydrophthalic acid calcium salt as the nucleating agent, due to the planar rigid structure of the benzene ring, its thermal stability is poor; when it uses dicycloheptane dicarboxylic acid disodium salt, its water vapor barrier properties are poor.
[0003] In summary, after extensive searching by the applicant, it is found that at least in this field, the existing polyethylene films have the problem of poor heat resistance and water vapor barrier properties. Therefore, it is necessary to develop or improve a heat-resistant polyethylene film with high water vapor barrier properties and a preparation method thereof. Summary of the invention
[0004] Based on this, in order to solve the problem that the existing polyethylene film has poor heat resistance and water vapor barrier properties, the present invention provides a heat-resistant polyethylene film with high water vapor barrier properties and a preparation method thereof. The specific technical scheme is as follows:
[0005] A heat-resistant polyethylene film with high water vapor barrier properties, comprising a layer A material and a layer B material, wherein the layer A material and the layer B material are alternately combined and extruded through a laminator to form a polyethylene film with a structure of 25 to 1025 layers;
[0006] The upper surface layer and the lower surface layer of the polyethylene film are both the A layer material;
[0007] The A layer material is modified high-density polyethylene;
[0008] The B layer material is modified low-density polyethylene;
[0009] The preparation materials of the modified high-density polyethylene include high-density polyethylene, disodium dicycloheptane dicarboxylate and calcium stearate;
[0010] The preparation materials of the modified low-density polyethylene include low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine.
[0011] Furthermore, the density of the high-density polyethylene is greater than 0.950 g / cm 3The melt index of the high-density polyethylene is 0.5~3.0g / 10min.
[0012] Further, the high-density polyethylene includes at least one of high-density polyethylene resin Dow AT6900, high-density polyethylene resin Nova 2607-UV14 and high-density polyethylene resin Hanwha F920A.
[0013] The preparation method of the modified high-density polyethylene comprises the following steps:
[0014] The high-density polyethylene, disodium dicycloheptane dicarboxylate and calcium stearate are added into a twin-screw extruder respectively, and mixed and extruded to obtain the modified high-density polyethylene;
[0015] The mass ratio of the high-density polyethylene, disodium bicycloheptane dicarboxylate and calcium stearate is 92.1-96:3-7:0.5-1.5.
[0016] Furthermore, the density of the low-density polyethylene is 0.912-0.940 g / cm 3 The melt index of the low-density polyethylene is 0.5~3.0g / 10min.
[0017] Furthermore, the low-density polyethylene includes low-density polyethylene Dow Elite 5400G or low-density polyethylene FP120-A.
[0018] Furthermore, the preparation method of the modified low-density polyethylene comprises the following steps:
[0019] The low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine are added into a twin-screw extruder respectively, and mixed and extruded to obtain the modified low-density polyethylene;
[0020] The mass ratio of the low-density polyethylene, the ethylene-norbornene copolymer and the 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine is 60-80:10-30:5-15.
[0021] Furthermore, the thickness of the polyethylene film is 20-50 μm, the ΔH of the polyethylene film is greater than 150 J / g, and the density of the polyethylene film is greater than 0.92 g / cm 3 The water vapor permeability of the polyethylene film is less than 1.0 g / (m 2 ·24h).
[0022] The technical solution also provides a method for preparing a heat-resistant polyethylene film with high water vapor barrier properties, which comprises the following steps:
[0023] The modified high-density polyethylene and the modified low-density polyethylene are added to the A layer and the B layer of the multi-layer co-extrusion blown film line respectively, and then alternately combined and extruded through a laminator to be divided into a 25-1025-layer structure, and then co-extruded into an annular film bubble with an initial film thickness of 100-250 μm in a blown film die head. After the annular film bubble is cooled, it is preheated, stretched, annealed, and cooled through an MDO unit, and then corona treated and rolled up to obtain the polyethylene film with a thickness of 20-50 μm.
[0024] Furthermore, the stretching temperature is 113-120° C., and the stretching ratio is 3-10.
[0025] The heat-resistant and high water vapor barrier polyethylene film provided by the above technical solution comprises a layer A material of modified high-density polyethylene and a layer B material of modified low-density polyethylene, and the layer A material and the layer B material are alternately combined and extruded into a 25-1025-layer structure through a laminator. Specifically, the preparation material of the modified high-density polyethylene comprises high-density polyethylene, disodium dicycloheptane dicarboxylate, and calcium stearate, and the preparation material of the modified low-density polyethylene comprises low-density polyethylene, ethylene-norbornene copolymer, and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy] Since both dicycloheptane dicarboxylic acid disodium salt and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine have macromolecular ring structures, which are different from the rigid structure of the planar benzene ring, the ring structures of the two substances are spatially twistable and can absorb or release a certain amount of energy, thereby respectively improving the thermal stability of high-density polyethylene and low-density polyethylene; further, 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine can significantly improve the thermal stability of low-density polyethylene The water vapor barrier property of the polyethylene film prepared therefrom has excellent heat resistance and water vapor barrier property; specifically, the disodium salt of dicycloheptane dicarboxylate can further improve the crystallinity of high-density polyethylene by providing crystallization sites, refining the crystal size, and improving the crystal perfection, thereby increasing the torsional space for heat storage and release; 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine modified low-density polyethylene can effectively improve the heat resistance and hydrophobicity of low-density polyethylene, increase the glass transition temperature of the mixture, and increase The difficulty for small molecules to pass through the film segments is reduced, thereby improving the stability and water vapor barrier properties of the polyethylene film; further, by alternately extruding 25 to 1025 layers of structure through a laminator, the advantages of modified high-density polyethylene and modified low-density polyethylene can be effectively combined, so that the functional groups and cyclic structures of dicycloheptane dicarboxylic acid disodium salt and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine work together, thereby controlling the growth of polymer crystals in the layered confined space, and obtaining a polyethylene film with high strength, heat resistance and high water vapor barrier properties;
[0026] The present invention uses a stacker to adjust the layer thickness of the polymer film through micro-nano stacking technology, thereby controlling the growth of polymer crystals in the layered confined space. When the spatial scale of the confined layer space is almost equal to the thickness of the polymer layered crystal, the crystal will deform and grow in two dimensions along the plane direction. Compared with other technologies, micro-nano stacking technology can be used to efficiently and quickly prepare solvent-free, environmentally friendly layered and confined polymer composites on a large scale. Since the growth of the lamellar crystals is restricted, when the gas enters the multilayer film, its permeation path is blocked by a large number of lamellar walls (lamellar crystals formed by crystal confinement). Therefore, the diffusion path of the gas is greatly increased, so that the gas barrier performance of the multilayer film increases exponentially. After the film is uniaxially stretched, the crystals are further oriented, extending the path length of the gas molecules when passing through the film, thereby improving other barrier properties. The heat-resistant and high water vapor barrier polyethylene film provided by the present invention simultaneously connects the micro-nano stacking technology and the uniaxial stretching process in series, further improving the water vapor barrier performance of the film. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.
[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0029] A heat-resistant polyethylene film with high water vapor barrier properties in one embodiment of the present invention comprises a layer A material and a layer B material, wherein the layer A material and the layer B material are alternately combined and extruded through a laminator to form a polyethylene film with a structure of 25 to 1025 layers;
[0030] The upper surface layer and the lower surface layer of the polyethylene film are both the A layer material;
[0031] The A layer material is modified high-density polyethylene;
[0032] The B layer material is modified low-density polyethylene;
[0033] The preparation materials of the modified high-density polyethylene include high-density polyethylene, disodium dicycloheptane dicarboxylate and calcium stearate;
[0034] The preparation materials of the modified low-density polyethylene include low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine.
[0035] In one embodiment, the density of the high-density polyethylene is greater than 0.950 g / cm 3 The melt index of the high-density polyethylene is 0.5~3.0g / 10min.
[0036] In one embodiment, the high-density polyethylene includes at least one of high-density polyethylene resin Dow AT6900, high-density polyethylene resin Nova 2607-UV14 and high-density polyethylene resin Hanwha F920A.
[0037] In one embodiment, the method for preparing the modified high-density polyethylene comprises the following steps:
[0038] The high-density polyethylene, disodium dicycloheptane dicarboxylate and calcium stearate are added into a twin-screw extruder respectively, and mixed and extruded to obtain the modified high-density polyethylene;
[0039] The mass ratio of the high-density polyethylene, disodium bicycloheptane dicarboxylate and calcium stearate is 92.1-96:3-7:0.5-1.5.
[0040] In one embodiment, the density of the low-density polyethylene is 0.912-0.940 g / cm 3 The melt index of the low-density polyethylene is 0.5~3.0g / 10min.
[0041] In one embodiment, the low-density polyethylene includes low-density polyethylene Dow Elite 5400G or low-density polyethylene FP120-A.
[0042] In one embodiment, the method for preparing the modified low-density polyethylene comprises the following steps:
[0043] The low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine are added into a twin-screw extruder respectively, and mixed and extruded to obtain the modified low-density polyethylene;
[0044] The mass ratio of the low-density polyethylene, the ethylene-norbornene copolymer and the 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine is 60-80:10-30:5-15.
[0045] In one embodiment, the ΔH of the polyethylene film is greater than 150 J / g, and the density of the polyethylene film is greater than 0.92 g / cm 3 The water vapor permeability of the polyethylene film is less than 1.0 g / (m 2 ·24h).
[0046] In one embodiment, the technical solution provides a method for preparing a heat-resistant polyethylene film with high water vapor barrier properties, which comprises the following steps:
[0047] The modified high-density polyethylene and the modified low-density polyethylene are added to the A layer and the B layer of the multi-layer co-extrusion blown film line respectively, and then alternately combined and extruded through a laminator to be divided into a 25-1025-layer structure, and then co-extruded into an annular film bubble with an initial film thickness of 100-250 μm in a blown film die head. After the annular film bubble is cooled, it is preheated, stretched, annealed, and cooled through an MDO unit, and then corona treated and rolled up to obtain the polyethylene film with a thickness of 20-50 μm.
[0048] In one embodiment, the stretching temperature is 113-120° C., and the stretching ratio is 3-10.
[0049] The embodiments of the present invention will be described in detail below with reference to specific examples.
[0050] Embodiment 1:
[0051] Preparation of modified high-density polyethylene: density 0.969g / cm 3 High-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate are subjected to twin-screw extrusion to obtain modified high-density polyethylene; wherein the mass ratio of high-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate is 95:3.5:1.5;
[0052] Preparation of modified low-density polyethylene: Low-density polyethylene Dow Elite 5400G, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine are mixed and extruded using a twin-screw extruder to obtain modified low-density polyethylene; wherein the mass ratio of low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine is 70:20:10.
[0053] Preparation of polyethylene film: The modified high-density polyethylene and modified low-density polyethylene are added to the A layer and B layer of the multi-layer co-extrusion blown film line respectively, and then alternately combined and extruded through a laminator to form a 65-layer structure, and then co-extruded into an annular film bubble with an initial film thickness of 125 μm in a blown film die head. After the annular film bubble is cooled, it is preheated, stretched, annealed, and cooled through an MDO unit, and then corona treated and rolled to obtain a polyethylene film with a thickness of 25 μm. The upper and lower surface layers of the polyethylene film are both modified high-density polyethylene, and the stretching temperature is 116°C and the stretching ratio is 5.
[0054] Embodiment 2:
[0055] Preparation of modified high-density polyethylene: density 0.969g / cm 3 The high-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate are subjected to twin-screw extrusion to obtain modified high-density polyethylene; wherein the mass ratio of the high-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate is 95:3:1.5;
[0056] Preparation of modified low-density polyethylene: Low-density polyethylene Dow Elite 5400G, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine are mixed and extruded using a twin-screw extruder to obtain modified low-density polyethylene; wherein the mass ratio of low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine is 70:20:10.
[0057] Preparation of polyethylene film: The modified high-density polyethylene and modified low-density polyethylene are added to the A layer and B layer of the multi-layer co-extrusion blown film line respectively, and then alternately combined and extruded through a laminator to form a 65-layer structure, and then co-extruded into an annular film bubble with an initial film thickness of 125 μm in a blown film die head. After the annular film bubble is cooled, it is preheated, stretched, annealed, and cooled through an MDO unit, and then corona treated and rolled to obtain a polyethylene film with a thickness of 25 μm. The upper and lower surface layers of the polyethylene film are both modified high-density polyethylene, and the stretching temperature is 116°C and the stretching ratio is 5.
[0058] Embodiment 3:
[0059] Preparation of modified high-density polyethylene: density 0.969g / cm 3The high-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate are subjected to twin-screw extrusion to obtain modified high-density polyethylene; wherein the mass ratio of the high-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate is 95:7:1.5;
[0060] Preparation of modified low-density polyethylene: Low-density polyethylene Dow Elite 5400G, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine are mixed and extruded using a twin-screw extruder to obtain modified low-density polyethylene; wherein the mass ratio of low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine is 70:20:10.
[0061] Preparation of polyethylene film: The modified high-density polyethylene and modified low-density polyethylene are added to the A layer and B layer of the multi-layer co-extrusion blown film line respectively, and then alternately combined and extruded through a laminator to form a 129-layer structure, and then co-extruded into an annular film bubble with an initial film thickness of 125 μm in a blown film die head. After the annular film bubble is cooled, it is preheated, stretched, annealed, and cooled through an MDO unit, and then corona treated and rolled to obtain a polyethylene film with a thickness of 25 μm. The upper and lower surface layers of the polyethylene film are both modified high-density polyethylene, and the stretching temperature is 116°C and the stretching ratio is 5.
[0062] Embodiment 4:
[0063] Preparation of modified high-density polyethylene: density 0.969g / cm 3 High-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate are subjected to twin-screw extrusion to obtain modified high-density polyethylene; wherein the mass ratio of high-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate is 95:3.5:1.5;
[0064] Preparation of modified low-density polyethylene: Low-density polyethylene Dow Elite 5400G, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine are mixed and extruded using a twin-screw extruder to obtain modified low-density polyethylene; wherein the mass ratio of low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine is 70:20:5.
[0065] Preparation of polyethylene film: The modified high-density polyethylene and modified low-density polyethylene are added to the A layer and B layer of the multi-layer co-extrusion blown film line respectively, and then alternately combined and extruded through a laminator to form a 1025-layer structure, and then co-extruded into an annular film bubble with an initial film thickness of 125 μm in a blown film die head. After the annular film bubble is cooled, it is preheated, stretched, annealed, and cooled through an MDO unit, and then corona treated and rolled to obtain a polyethylene film with a thickness of 25 μm. The upper and lower surface layers of the polyethylene film are both modified high-density polyethylene, and the stretching temperature is 116°C and the stretching ratio is 5.
[0066] Embodiment 5:
[0067] Preparation of modified high-density polyethylene: density 0.967g / cm 3 High-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate are subjected to twin-screw extrusion to obtain modified high-density polyethylene; wherein the mass ratio of high-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate is 95:3.5:1.5;
[0068] Preparation of modified low-density polyethylene: Low-density polyethylene Dow Elite 5400G, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine are mixed and extruded using a twin-screw extruder to obtain modified low-density polyethylene; wherein the mass ratio of low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine is 70:20:15.
[0069] Preparation of polyethylene film: The modified high-density polyethylene and modified low-density polyethylene are added to the A layer and B layer of the multi-layer co-extrusion blown film line respectively, and then alternately combined and extruded through a laminator to form a 1025-layer structure, and then co-extruded into an annular film bubble with an initial film thickness of 200 μm in a blown film die head. After the annular film bubble is cooled, it is preheated, stretched, annealed, and cooled through an MDO unit, and then corona treated and rolled to obtain a polyethylene film with a thickness of 40 μm. The upper and lower surface layers of the polyethylene film are both modified high-density polyethylene, and the stretching temperature is 116°C and the stretching ratio is 5.
[0070] Comparative Example 1:
[0071] Preparation of modified high-density polyethylene: density 0.969g / cm 3High-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate are subjected to twin-screw extrusion to obtain modified high-density polyethylene; wherein the mass ratio of high-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate is 95:3.5:1.5;
[0072] Preparation of modified low-density polyethylene: Low-density polyethylene Dow Elite 5400G, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine are mixed and extruded using a twin-screw extruder to obtain modified low-density polyethylene; wherein the mass ratio of low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine is 70:20:10.
[0073] Preparation of polyethylene film: The modified high-density polyethylene and modified low-density polyethylene are respectively added to the two surface layers and the core layer of the multi-layer co-extrusion blown film line, and then co-extruded into an annular film bubble with an initial film thickness of 125 μm in the film blowing die head. After the annular film bubble is cooled, it is preheated, stretched, annealed, and cooled by an MDO unit, and then corona treated and rolled to obtain a polyethylene film with a thickness of 25 μm. The upper and lower surface layers of the polyethylene film are both modified high-density polyethylene, and the stretching temperature is 116°C and the stretching ratio is 5.
[0074] Comparative Example 2:
[0075] Preparation of modified low-density polyethylene: Low-density polyethylene Dow Elite 5400G, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine are mixed and extruded using a twin-screw extruder to obtain modified low-density polyethylene; wherein the mass ratio of low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine is 70:20:10.
[0076] Preparation of polyethylene film: High-density polyethylene F920A and modified low-density polyethylene are added to the A layer and B layer of the multi-layer co-extrusion blown film line respectively, and then alternately combined and extruded through a stacker to form a 33-layer structure, and then co-extruded into an annular film bubble with an initial film thickness of 125 μm in a blown film die head. After the annular film bubble is cooled, it is preheated, stretched, annealed, and cooled through an MDO unit, and then corona treated and rolled to obtain a polyethylene film with a thickness of 25 μm. The upper and lower surface layers of the polyethylene film are both high-density polyethylene F920A, the stretching temperature is 116°C, and the stretching ratio is 5.
[0077] Comparative Example 3:
[0078] Preparation of modified high-density polyethylene: density 0.969g / cm 3 High-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate are subjected to twin-screw extrusion to obtain modified high-density polyethylene; wherein the mass ratio of high-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate is 95:3.5:1.5;
[0079] Preparation of modified low-density polyethylene: Low-density polyethylene Dow Elite 5400G and ethylene-norbornene copolymer are mixed and extruded using a twin-screw extruder to obtain modified low-density polyethylene; wherein the mass ratio of low-density polyethylene to ethylene-norbornene copolymer is 70:20.
[0080] Preparation of polyethylene film: The modified high-density polyethylene and modified low-density polyethylene are added to the A layer and B layer of the multi-layer co-extrusion blown film line respectively, and then alternately combined and extruded through a laminator to form a 33-layer structure, and then co-extruded into a ring-shaped film bubble with an initial film thickness of 125 μm in a blown film die head. After the ring-shaped film bubble is cooled, it is preheated, stretched, annealed, and cooled through an MDO unit, and then corona treated and rolled to obtain a polyethylene film with a thickness of 25 μm. The upper and lower surface layers of the polyethylene film are both modified high-density polyethylene, and the stretching temperature is 116°C and the stretching ratio is 5.
[0081] Comparative Example 4:
[0082] Preparation of modified high-density polyethylene: density 0.969g / cm 3 High-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate are subjected to twin-screw extrusion to obtain modified high-density polyethylene; wherein the mass ratio of high-density polyethylene resin Dow AT6900, dicycloheptane dicarboxylic acid disodium salt and calcium stearate is 95:3.5:1.5;
[0083] Preparation of modified low-density polyethylene: Low-density polyethylene Dow Elite 5400G, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine are mixed and extruded using a twin-screw extruder to obtain modified low-density polyethylene; wherein the mass ratio of low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine is 70:20:10.
[0084] Preparation of polyethylene film: The modified high-density polyethylene and modified low-density polyethylene are added to a three-layer co-extrusion blown film line respectively, wherein the modified high-density polyethylene is in the upper and lower surface layers, and the modified low-density polyethylene is in the middle layer, and the layer thickness ratios are 25:50:25, respectively. An annular film bubble is blown out through a co-extrusion die head. After the film bubble is cooled, it is subjected to corona treatment and rolled up to obtain a polyethylene film with a thickness of 40 μm.
[0085] The polyethylene films obtained in Examples 1 to 5 and Comparative Examples 1 to 4 were tested for water vapor performance, printed film electric eye size and ΔH. The results are shown in Table 1.
[0086] △H is the reaction heat when the polyethylene film undergoes phase change. The greater the reaction heat, the higher its thermal stability.
[0087] Use a gravure roller with a circumference of 520.5 mm, a printing speed of 150 m / min, an oven temperature of 65°C, and use a tape measure to measure the size of the electric eye. The closer the size is to 520.5 mm, the better the thermal stability of the polyethylene film.
[0088] Table 1:
[0089] project △H / (J / g) Printed film sensor size / mm <![CDATA[Water vapor transmission rate g / (m 2 ·24h)]]> Example 1 160 520.3 0.86 Example 2 159 520.3 0.92 Example 3 159 520.3 0.64 Example 4 159 520.3 0.73 Example 5 158 520.3 0.35 Comparative Example 1 158 520.0 3.8 Comparative Example 2 140 516.1 5.1 Comparative Example 3 138 517.2 4.6 Comparative Example 4 140 516.5 3.4
[0090] As can be seen from Table 1, the heat-resistant high water vapor barrier polyethylene film provided by the present invention comprises a layer A material of modified high-density polyethylene and a layer B material of modified low-density polyethylene, and the layer A material and the layer B material are alternately combined and extruded through a laminator to form a 25-1025-layer structure. Specifically, the modified high-density polyethylene and the modified low-density polyethylene have excellent heat resistance and water vapor barrier properties. Specifically, the ΔH of the polyethylene films of Examples 1 to 5 provided by the present invention is not less than 158 / g, the size of the printed film electric eye is maintained stable at 520.3 mm, and the water vapor permeability is as low as 1.0 g / (m 2 Furthermore, by alternately extruding 25 to 1025 layers of structure through a laminator, the advantages of modified high-density polyethylene and modified low-density polyethylene can be effectively combined, and by changing the layer thickness of the polymer film and controlling the growth of polymer crystals in the layered confined space, a polyethylene film with high water vapor barrier properties can be obtained.
[0091] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0092] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A heat-resistant polyethylene film with high water vapor barrier properties, characterized in that: It comprises an A-layer material and a B-layer material, wherein the A-layer material and the B-layer material are alternately combined and extruded through a laminator to form a polyethylene film having a structure of 25 to 1025 layers; The upper surface layer and the lower surface layer of the polyethylene film are both the A layer material; The A layer material is modified high-density polyethylene; The B layer material is modified low-density polyethylene; The preparation materials of the modified high-density polyethylene include high-density polyethylene, disodium dicycloheptane dicarboxylate and calcium stearate; The preparation materials of the modified low-density polyethylene include low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine; Preparation method of modified low-density polyethylene The following steps are involved: The low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine are added into a twin-screw extruder respectively, and mixed and extruded to obtain the modified low-density polyethylene; The mass ratio of the low-density polyethylene, ethylene-norbornene copolymer and 1,2,2-trichloro-N-[2-[[4-(trifluoromethyl)-2-pyridyl]oxy]ethoxy]ethyleneamine is 60-80:10-30:5-15; The preparation method of the modified high-density polyethylene comprises the following steps: The high-density polyethylene, disodium dicycloheptane dicarboxylate and calcium stearate are added into a twin-screw extruder respectively, and mixed and extruded to obtain the modified high-density polyethylene; The mass ratio of the high-density polyethylene, disodium bicycloheptane dicarboxylate and calcium stearate is 92.1-96:3-7:0.5-1.5; The method for preparing the polyethylene film comprises the following steps: The modified high-density polyethylene and the modified low-density polyethylene are added to the A layer and the B layer of the multi-layer co-extrusion blown film line respectively, and then alternately combined and extruded through a laminator to form a 25-1025-layer structure, and then co-extruded in a blown film die head to form an annular film bubble with an initial film thickness of 100-250 μm, and after the annular film bubble is cooled, it is preheated, stretched, annealed, and cooled through an MDO unit, and then corona treated and rolled to obtain the polyethylene film with a thickness of 20-50 μm; The stretching temperature is 113-120° C., and the stretching ratio is 3-10.
2. The polyethylene film according to claim 1, characterized in that The density of the high-density polyethylene is greater than 0.950 g / cm 3 The melt index of the high-density polyethylene is 0.5~3.0g / 10min.
3. The polyethylene film according to claim 1, characterized in that: The high-density polyethylene includes at least one of high-density polyethylene resin Dow AT6900, high-density polyethylene resin Nova 2607-UV14, and high-density polyethylene resin Hanwha F920A.
4. The polyethylene film according to claim 1, characterized in that: The density of the low-density polyethylene is 0.912-0.940 g / cm 3 The melt index of the low-density polyethylene is 0.5~3.0g / 10min.
5. The polyethylene film according to claim 1, characterized in that: The low-density polyethylene includes low-density polyethylene Dow Elite 5400G or low-density polyethylene FP120-A.