A modified CuO material and its gas sensor application

By modifying Pd nanoparticles on the CuO surface and covering MOF, Pd-CuO@MOF composite material is formed, which solves the problem of insufficient sensitivity of gas-sensitive sensors in high humidity environments, and achieves high-efficiency acetone sensing and excellent moisture-proof performance.

CN118652439BActive Publication Date: 2024-12-03WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410855896.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-12-03
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

Existing gas-sensitive sensors are insufficiently sensitive and costly in high humidity environments, and lack effective hydrophobic and breathable coated modified P-type MOS materials, making it difficult to achieve high-performance acetone gas sensing.

Method used

Using modified CuO material, the precious metal Pd nanoparticles are modified on the surface of octahedral CuO and coated with Cu-based MOF to form a Pd-CuO@MOF composite material to improve moisture resistance and sensitivity.

Benefits of technology

The humidity resistance and sensitivity of the gas-sensitive sensor are significantly improved, the acetone sensing performance is significantly improved, the humidity coefficient of variation is less than 5%, and the sensitivity is increased to about 2.5 times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652439B_ABST
    Figure CN118652439B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of gas sensors, and in particular to a modified CuO material and its gas sensor application. The modified CuO material includes octahedral CuO, noble metal PdNPs and Cu-based MOF, wherein the noble metal is modified on the surface of the octahedral CuO, and the Cu-based MOF grows on the surface of CuO modified with the noble metal Pd NPs to achieve hydrophobic coating. The present invention prepares an octahedral CuO material, and modifies the noble metal Pd on the octahedral CuO to obtain Pd-CuO, and then coats MOF on its surface, finally preparing a Pd-CuO@MOF composite material, and constructing a corresponding gas sensor to prove the acetone sensing performance of the gas-sensitive material, and has excellent moisture resistance, achieving a dual improvement in the moisture resistance and sensitivity of the CuO material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gas sensors, and in particular to a modified CuO material and an application of the same to a gas sensor. Background Art

[0002] With the rapid development of the Internet of Things, the application fields of gas sensors have expanded rapidly, covering multiple fields such as wearable devices, indoor gas detection and breath diagnosis. In particular, breath detection has attracted much attention in clinical diagnosis and scientific research in recent years. Among them, acetone, as one of the metabolites of the human body, has shown its potential to quickly distinguish healthy people from diabetic patients through its detection in breath diagnosis. It can reflect the metabolism of ketone bodies, so it is of great significance in the early diagnosis of diabetes, prevention and treatment of ketoacidosis, etc. For example, Wang C et al. (A Study on Breath Acetone in Diabetic Patients Using a Cavity Ringdown Breath Analyzer: Exploring Correlations of Breath Acetone With Blood Glucose and Glycohemoglobin A1C [J]. IEEE Sensors Journal, 2010, 10 (1): 54-63) used a small acetone breathalyzer to detect the breath acetone and blood glucose levels of confirmed diabetic patients, and obtained a high linear relationship between the two through correlation analysis. Therefore, monitoring of patients' breath acetone may become a new standard for insulin management. In recent years, thanks to the continuous maturity of semiconductor sensor preparation technology, low-cost, portable non-invasive breath detection technology has made significant breakthroughs and progress. Metal oxide semiconductors have become widely used semiconductor gas sensors. Since human breathing is a high-humidity environment (relative humidity RH>70%), during the operation of MOS gas sensors, water molecules will compete with the target gas for adsorbed oxygen on the surface of the material through adsorption-desorption equilibrium, resulting in a deterioration in sensitivity. Most MOS are strongly affected by humidity and P-type MOS has low sensitivity. Therefore, the ultimate goal of gas sensors for breath detection is to ensure that they have a certain sensitivity while not being easily affected by humidity changes.

[0003] At present, the research on moisture-resistant gas sensors mainly includes configuring dehumidification devices, such as waterproof and dustproof covers; humidity compensation, such as connecting a hygroscopic resistor in series with the original measurement circuit to compensate for the error caused by humidity changes; algorithm compensation, such as data calibration through artificial intelligence algorithms. From the perspective of material design, it can be divided into modification methods such as doping hydroxyl absorbents, regulating the chemical adsorption characteristics of surface oxygen, and hydrophobic and breathable coating. Among them, the hydrophobic and breathable coating can directly isolate the contact between water molecules and sensitive materials, and can better maintain the baseline and response stability of the sensor in a humid environment. For example, by coating the ZIF-DMBIM film on the surface of Au-ZnO nanorods, the moisture resistance of the material is improved, and the humidity coefficient of variation (CV) in the detection of 100ppm acetone is only 6.33%. Similarly, Zhou Tingting et al. (Gas adsorption at metal sites forenhancing gas sensing performance of ZnO@ZIF-71nanorod arrays, Langmuir 35 (2019) 3248-3255) achieved moisture resistance sensing by coating the surface of ZnO nanorods with ZIF-71 film, with CV = 4.49% for 10 ppm ethanol detection and CV = 5.02% for 5.02 ppm acetone detection. Nanoparticles of precious metals (Au, Ag, Pt, Pd), precious metal oxides (PdO) and some metal oxides (Co3O4 and NiO) with catalytic properties can effectively improve the reaction efficiency of the gas molecules to be measured on the surface of semiconductor metal oxides, the surface recognition function, and effectively reduce the activation energy required for the reaction, thereby improving the sensitivity of the gas sensor, reducing the energy consumption of the sensor and improving the response recovery speed. For example, by modifying PdO onto the ring-shaped NiO nanostructure, the response (Rg / Ra) to 20ppmCo increased from 8.2 to 27.5 compared with the sensitive material without noble metal modification. At the same time, existing studies have reported that the response value of the hierarchical NiO sensitive material modified with Au nanoparticles to acetone gas increased by 6.7 times.

[0004] However, existing gas sensors still have the following disadvantages: (1) The structures of methods based on dehumidification devices, humidity compensation, algorithm compensation, etc. are relatively complex, all of which require increasing the cost of the sensor, and do not solve the technical problem of MOS material's moisture resistance from the source of material performance. (2) The sensitive materials based on previous hydrophobic and breathable coating modification methods are relatively single, mostly N-type sensing materials, such as ZnO. So far, there are few reports on P-type gas-sensitive materials modified by hydrophobic and breathable coatings. (3) Compared with N-type sensing materials, P-type MOS gas sensors have unique oxygen adsorption characteristics, which means that P-type semiconductor oxides have great potential as sensitive materials for constructing high-performance gas sensors. However, since the gas response of P-type MOS is unsatisfactory compared with N-type MOS, there are few reports on P-type MOS gas sensors, which fully demonstrates that P-type semiconductor oxides have great challenges in improving their sensitivity. Summary of the invention

[0005] In view of this, the present invention proposes a modified CuO material and an application of a gas sensor thereof to solve the problems of insufficient moisture resistance and sensitivity of acetone gas sensors in the prior art.

[0006] The technical solution of the present invention is achieved in this way:

[0007] In a first aspect, the present invention provides a modified CuO material, comprising octahedral CuO, noble metal Pd NPs and Cu-based MOF, wherein the noble metal is modified on the surface of the octahedral CuO, and the Cu-based MOF grows on the surface of the CuO modified with the noble metal PdNPs to achieve hydrophobic coating.

[0008] CuO is an important P-type semiconductor metal oxide. Due to its low toxicity, low cost, easy controllable synthesis and stable chemical and electrical properties, as an oxide of a transition metal, it presents different oxidation states due to the electrons in the d shell of its metal atoms, usually exhibits good acetone catalytic activity, and can promote the oxidation state of volatile organic compounds. Therefore, this means that the P-type semiconductor CuO has the potential to construct a high-performance acetone gas sensor. In the present invention, the octahedral CuO provides basic gas-sensitive performance. As a transition metal oxide, CuO has good chemical stability and can maintain a stable structure and performance under various working environments; at the same time, the octahedral CuO structure has a high surface area and abundant surface active sites. The crystal structure is conducive to the adsorption and chemical reaction of gas molecules, thereby improving the basic gas-sensitive performance. The higher surface energy of the (110) crystal plane of the octahedral CuO is conducive to the gas adsorption process, and gas adsorption is a key step in the gas-sensitive reaction. Noble metal modification can change the surface chemistry and electronic effects of gas-sensitive materials. On the one hand, it can regulate the gas-sensitive reaction activity of gas-sensitive materials and improve sensitivity; on the other hand, it can regulate the surface chemical adsorption characteristics of gas-sensitive materials and inhibit or eliminate the influence of water molecules on the sensing performance of gas-sensitive materials. The subsequent coating of hydrophobic MOF can not only weaken the influence of water molecules on gas-sensitive materials through its hydrophobic groups, but also achieve pre-concentration of gas molecules and improve the sensitivity of gas-sensitive materials.

[0009] Specifically, the sensing performance of gas sensors for volatile organic compounds is closely related to the presence of surface-bound chemisorbed oxygen. When oxygen molecules are chemisorbed onto CuO, it leads to the formation of a hole accumulation layer on the CuO surface. Therefore, due to the large presence of holes, CuO-based sensors tend to exhibit a highly conductive state in ambient air. Subsequently, when reducing acetone molecules are introduced, a reaction occurs between oxygen species and the surface of the sensing material. In this process, the accumulated holes are consumed, resulting in a significant decrease in the conductivity of the CuO-based sensor. The sensing process is greatly modulated by the introduction of PdNPs and the surface Cu-MOF filter membrane. In the Pd-CuO structure, the PdNPs modified on the CuO surface act as adsorption sites and catalysts, enhancing the dissociation of oxygen molecules on the CuO surface. The palladium nanoparticles enhance the coverage of negative oxygen ions on the CuO surface through the spillover effect. CuO@MOF sensors still exhibit superior performance compared to CuO under the same conditions. This improvement is mainly attributed to the ability of the external CuO@MOF membrane to enhance the adsorption of acetone, a phenomenon known as the pre-enrichment effect. This enhancement in gas sensing performance is attributed to the large specific surface area of ​​MOF materials.

[0010] Under high humidity conditions, the moisture resistance of the Pd-CuO material is significantly improved because Pd-NPs can act as hydroxyl absorbers. In addition, the formation of a Cu-based MOF hydrophobic and breathable layer significantly improves the moisture resistance of the composite sensor.

[0011] In summary, first of all, Cu-MOF can not only filter out most of the water, but also has the ability to pre-concentrate acetone molecules, thereby significantly improving the moisture resistance and sensitivity of the sensor. Subsequently, the acetone molecules contact the Pd-CuO interface. The overflow and electronic sensitization effect of PdNPs can significantly increase the content of adsorbed oxygen on the surface of the CuO material. Acetone molecules react with these surface oxygen, causing the surface resistance of the gas-sensitive material to change, thereby achieving a response to acetone. Therefore, the modified CuO material used in gas sensors has efficient acetone sensing ability and excellent moisture resistance. It is the synergistic effect of PdNPs and Cu-BTC with CuO.

[0012] In a second aspect, the present invention provides a method for preparing a modified CuO material, comprising the following steps:

[0013] S1, mixing the copper acetate solution and the sodium hydroxide solution, adding a reducing agent, stirring and dissolving, and heating in a water bath to react to obtain a solid product Cu2O;

[0014] S2, drying the solid product Cu2O and calcining it at a constant temperature to obtain CuO, wherein the CuO is octahedral;

[0015] S3, dissolving CuO and sodium chloropalladate in water, adding sodium borohydride, and reacting to obtain a solid product Pd-CuO;

[0016] S4. The solid product Pd-CuO is mixed with an organic ligand, dimethylformamide and water to undergo a solvothermal reaction to obtain a modified CuO material.

[0017] Specifically, in step S1, when the NaOH solution is added dropwise to the Cu(CH3COO)2·H2O solution, a Cu(OH)2 precipitate is first generated, and then the Cu(OH)2 precipitate rapidly reacts with the excess OH - Ions combine to form [Cu(OH)4] 2- The mixed solution appears dark blue. The reaction equation is: Cu 2+ (aq)+2OH - (aq)=Cu(OH)2(s); Cu(OH)2(s)+2OH - (aq) = [Cu(OH)4] 2- (aq). When a reducing agent is added, [Cu(OH)4] 2-The complex ion is reduced to generate Cu2O. Glucose can act as a reducing agent to convert [Cu(OH)4] 2- The complex ion is reduced to generate Cu2O, and the reaction equation is 2[Cu(OH)4] 2- (aq)+C6H 12 O6(aq)=Cu2O(s)+C6H 12 O 7- (aq)+3H2O(l)+3OH - (aq). [Cu(OH)4] 2- After the complex ions come into contact with glucose, Cu2O micronuclei are generated. After heating, the crystals grow faster along the

[100] crystal direction, leaving the (111) crystal plane. The Cu2O polyhedron presents an octahedral shape. The temperature and the directing agent have a crucial influence on the nucleation and growth process during the reaction to generate octahedrons. If the amount of NaOH, glucose or the heating order is changed, Cu2O with different morphologies will be obtained, such as cubes, cubic octahedrons, etc.

[0018] In step S2, calcination is performed in a muffle furnace to convert Cu2O into CuO. In step S3, sodium chloropalladate Na2PdCl4 is mixed with deionized water and CuO as a palladium source. At this time, the Pd in ​​the solution is +2 valent. The purpose of adding sodium borohydride aqueous solution and stirring is to convert the +2 valent Pd 2+ During the reduction to Pd, constant stirring is required to allow Pd NPs to be evenly modified on the CuO surface. In step S4, CuO is a common MOS material. 2+ It can become the metal center of MOF under certain conditions. At a certain temperature, it can react with solvent and organic ligand trimesic acid in a high-pressure reactor to form a copper-based metal organic framework. The growth process of MOF on the CuO matrix includes two parts: (1) the partial dissolution of CuO octahedron provides Cu 2+ ions; (2) trimesic acid and Cu 2+ The composite MOF crystals are wrapped around the outside of CuO and the inside of CuO to form a core-shell structure. Therefore, the dissolution rate of CuO and the crystallization rate of MOF are the key factors in the formation of the core-shell structure. The factors affecting the thickness of the MOF coating layer depend on many factors such as the content ratio of the solvent (dimethylformamide and deionized water), the content of the organic ligand (trimesic acid) and the content of CuO, the hydrothermal time, the hydrothermal temperature, etc.

[0019] On the basis of the above technical solution, preferably, in step S1, the mass ratio of the copper acetate, sodium hydroxide and reducing agent is 1.8-2.2:1:0.3-0.5.

[0020] On the basis of the above technical solution, preferably, the reducing agent is glucose, the water bath heating temperature is 65-75° C., and the water bath heating time is 0.3-0.7 h.

[0021] Specifically, step S1 specifically comprises: mixing a copper acetate solution and a sodium hydroxide solution to obtain a transparent dark blue mixed solution, then adding glucose, stirring and dissolving at room temperature (25-27° C.) to obtain a mixed solution; then slowly heating the mixed solution in a water bath, collecting the precipitate by centrifugation after the reaction, washing with deionized water for multiple times, and collecting by centrifugation to obtain a solid product Cu2O. Specifically, the concentration of the copper acetate solution is 0.0125-0.01 g / ml; the concentration of the sodium hydroxide solution is 0.00625-0.005 g / ml.

[0022] The amount of NaOH determines the Cu 2+ and OH - The concentration ratio of ions affects the kinetics of nucleation and crystal growth. The right amount of NaOH is conducive to the formation of octahedral structure, while excess or deficiency will lead to other morphologies such as cubes, polyhedrons, etc. Glucose is used as a reducing agent, and its content determines the Cu 2+ The rate of reduction. An appropriate amount of glucose can control the slow reduction rate, which is conducive to the orderly growth of the octahedral structure. Excessive or insufficient glucose will make the reduction process too fast or too slow, affecting the crystal morphology.

[0023] On the basis of the above technical solution, preferably, in step S2, the constant temperature calcination temperature is 450-550°C, the heating rate is 1-5°C / min, the annealing time is 1-3h, and the atmosphere of the constant temperature calcination is air.

[0024] Under the calcination process conditions of the present invention, CuO octahedron can be obtained. A higher calcination temperature can completely oxidize Cu2O into CuO. Long-term calcination (1-3h) is conducive to the improvement of CuO crystallinity. If the calcination temperature or calcination time is insufficient, the Cu2O phase may remain. A slow heating rate (1-5°C / min) is conducive to the orderly growth of the CuO octahedral structure. A too fast heating rate may destroy the orientation of the CuO crystal and cause an irregular structure. For example, under the calcination conditions of (400°C, 2h and 10°C / min), Cu2O can only be partially oxidized into CuO and finally obtain a Cu2O-CuO octahedron.

[0025] On the basis of the above technical solution, preferably, in step S3, the mass ratio of CuO, sodium chloropalladate and sodium borohydride is 35-45:1:1, the reaction temperature is 25-27° C., and the reaction time is 0.8-1.2 h.

[0026] Specifically, CuO reacts with sodium chloropalladate to deposit uniform Pd nanoparticles on the surface of CuO. Pd, as a metal, forms a strong interface interaction with CuO, a semiconductor oxide. This metal-semiconductor heterostructure can change the electronic structure and energy band characteristics of CuO, thereby improving the adsorption and reaction activity of CuO to target gas molecules and enhancing gas-sensitive performance. The modification of Pd nanoparticles can also improve the chemical adsorption characteristics of CuO to water molecules, reduce the interference of water molecules on gas-sensitive responses, and improve the anti-interference ability of the sensor.

[0027] On the basis of the above technical scheme, preferably, in step S4, the mass ratio of the solid product Pd-CuO, the organic ligand and dimethylformamide is 1:1-3:0.2-0.7, the temperature of the solvent thermal reaction is 60-80°C, and the reaction time is 5-7h.

[0028] On the basis of the above technical solution, preferably, the organic ligand is 1,3,5-benzenetricarboxylic acid.

[0029] A Cu-based MOF structure is grown on the Pd-CuO surface by a solvothermal method. MOF has a large specific surface area and abundant hydrophobic functional groups, which can effectively suppress the interference of water molecules. The hydrophobic functional groups improve the selective adsorption of Pd-CuO to the target gas molecules. The open pore structure of MOF can enrich and pre-concentrate the target gas molecules, thereby amplifying the sensing signal.

[0030] In a third aspect, the present invention provides an application of a modified CuO material, wherein the modified CuO material is made into a slurry and coated on a gas sensor body.

[0031] On the basis of the above technical scheme, preferably, the modified CuO material is ground with anhydrous ethanol to form a slurry, the slurry is coated on a planar electrode substrate with a gold electrode so that it completely covers the gold electrode, dried to form a film, and aged at 220-260°C to obtain a Pd-CuO@MOF acetone sensor.

[0032] Compared with the prior art, the modified CuO material and its gas sensor application of the present invention have the following advantages:

[0033] Beneficial effects:

[0034] (1) The present invention prepares an octahedral CuO material, and modifies the octahedral CuO with a noble metal Pd to obtain Pd-CuO, and then coats the surface of the octahedral CuO with MOF to finally prepare a Pd-CuO@MOF composite material, and constructs a corresponding gas sensor to prove the acetone sensing performance of the gas-sensitive material, and has excellent moisture resistance, thereby achieving a dual improvement in the moisture resistance and sensitivity of the CuO material;

[0035] (2) The modified CuO material prepared by the present invention is applied to gas sensors, which can significantly improve the sensitivity and excellent moisture resistance of gas sensors. It is sensitive to acetone under humidity interference. The sensitivity of Pd-CuO@MOF gas sensor is improved to about 2.5 times that of pure CuO gas sensor, and the humidity variation coefficient is less than 5%. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0037] Figure 1 This is an electron microscope image of the modified CuO material sample of Example 1 of the present invention;

[0038] Figure 2 The electron microscope images of the modified CuO material samples of Comparative Examples 1-3 of the present invention;

[0039] Figure 3 X-ray diffraction patterns of the modified CuO material samples of Example 1 and Comparative Examples 1-3 of the present invention;

[0040] Figure 4 The response values ​​of the gas sensors prepared in Example 1 and Comparative Examples 1-3 of the present invention to 50 ppm acetone at different working temperatures are shown in FIG.

[0041] Figure 5 The concentration-resistance relationship of the gas sensor prepared in Example 1 of the present invention to acetone at the optimal working temperature;

[0042] Figure 6 The concentration-resistance relationship of acetone at the optimal working temperature for the gas sensor prepared in Comparative Example 1 of the present invention;

[0043] Figure 7 The concentration-resistance relationship of acetone for the gas sensor prepared in Comparative Example 2 of the present invention at the optimal working temperature;

[0044] Figure 8 The concentration-resistance relationship of acetone for the gas sensor prepared in Comparative Example 3 of the present invention at the optimal working temperature;

[0045] Fig. 9 The humidity coefficient of variation and response value of the gas sensors prepared in Example 1 and Comparative Examples 1-3 of the present invention to 50 ppm acetone under different humidity conditions. DETAILED DESCRIPTION

[0046] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] Example 1

[0048] This embodiment provides a modified CuO material and its gas sensor application, which specifically includes the following steps:

[0049] (1) 1.00 g of copper acetate monohydrate is dissolved in 80 ml of deionized water to form solution 1, 0.5 g of sodium hydroxide is dissolved in 20 ml of deionized water to form solution 2, and the mixture is stirred and dissolved at room temperature (25-27° C.); solution 1 and solution 2 are mixed to obtain a transparent dark blue mixed solution, and then 0.2 g of glucose is added to obtain a mixed solution, and the mixture is stirred and dissolved at room temperature; the obtained mixed solution is slowly heated in a water bath at a heating temperature of 70° C. for a reaction of 0.5 h, and after the reaction, the precipitate is collected by centrifugation, washed with deionized water for multiple times, and finally collected by centrifugation to obtain a solid product Cu2O.

[0050] (2) The solid product Cu2O obtained in step (1) is placed in a blast drying oven for drying, and then placed in a muffle furnace for constant temperature calcination at 500° C., and annealed at a rate of 2.5° C. / min for 2 h to obtain a CuO octahedral material.

[0051] (3) Add 0.2 ml of sodium chloropalladate (concentration of 5 mg / ml) and 3 ml of deionized water to 40 mg of CuO octahedral material to obtain a black mixed solution, which is stirred at room temperature for 0.5 h to dissolve; slowly add 0.2 ml of sodium borohydride (5 mg / ml) dropwise to the black mixed solution, and stir at room temperature for 0.5 h to dissolve; after the reaction, collect the precipitate by centrifugation, wash it with deionized water several times, and finally collect it by centrifugation to obtain the solid product Pd-CuO.

[0052] (4) 40 mg of the solid product Pd-CuO was placed in a forced air drying oven to dry the obtained material and 80 mg of 1,3,5-benzenetricarboxylic acid in a polytetrafluoroethylene liner, 20 ml of dimethylformamide and 20 ml of deionized water were added and magnetically stirred to form a mixed solution. The solvent thermal reaction was carried out for 6 hours at a reaction temperature of 70°C to grow a Cu-based MOF on the surface of Pd-CuO to obtain a Pd-CuO@MOF gas-sensitive material.

[0053] (5) The platinum wire of the planar substrate is welded to the four-pin socket of the planar base by tin and solder paste, and 3-8 mg of the final sample (Pd-CuO@MOF gas-sensitive material) is weighed and mixed with anhydrous ethanol in an agate mortar to form a slurry. The slurry is applied to the planar electrode substrate with a gold electrode with a fine brush to completely cover the gold electrode, and then inserted into a 4-pin 30-way test board gas sensor planar aging station; it is placed on the aging station of the gas-sensitive component test system to dry and then aged in an air environment at 240°C for two days to obtain the corresponding gas-sensitive element.

[0054] Example 2

[0055] This embodiment provides a modified CuO material and its gas sensor application, which specifically includes the following steps:

[0056] (1) 0.9 g of copper acetate monohydrate is dissolved in 60 ml of deionized water to form solution 1, and 0.5 g of sodium hydroxide is dissolved in 20 ml of deionized water to form solution 2, and the mixture is stirred and dissolved at room temperature (25-27° C.); solution 1 and solution 2 are mixed to obtain a transparent dark blue mixed solution, and then 0.15 g of glucose is added to obtain a mixed solution, and the mixture is stirred and dissolved at room temperature; the obtained mixed solution is slowly heated in a water bath at a heating temperature of 65° C. and reacted for 0.3 h. After the reaction, the precipitate is collected by centrifugation, washed with deionized water for multiple times, and finally collected by centrifugation to obtain a solid product Cu2O.

[0057] (2) The solid product Cu2O obtained in step (1) is placed in a blast drying oven for drying, and then placed in a muffle furnace for constant temperature calcination at 450° C., and annealed at a rate of 1° C. / min for 1 h to obtain a CuO octahedral material.

[0058] (3) Add 0.2 ml of sodium chloropalladate (concentration of 5 mg / ml) and 2.5 ml of deionized water to 35 mg of CuO octahedral material to obtain a black mixed solution, which is stirred at room temperature for 0.4 h to dissolve; slowly add 0.2 ml of sodium borohydride (5 mg / ml) dropwise to the black mixed solution, and stir at room temperature for 0.4 h to dissolve; after the reaction, collect the precipitate by centrifugation, wash it with deionized water several times, and finally collect it by centrifugation to obtain a solid product Pd-CuO.

[0059] (4) 40 mg of the solid product Pd-CuO was placed in a forced air drying oven to dry the obtained material and 40 mg of 1,3,5-benzenetricarboxylic acid. 10 ml of dimethylformamide and 10 ml of deionized water were added and magnetically stirred to form a mixed solution. The solution was subjected to solvent thermal reaction for 5 h at a reaction temperature of 60 ° C to grow Cu-based MOF on the surface of Pd-CuO to obtain Pd-CuO@MOF gas-sensitive material.

[0060] (5) The platinum wire of the planar substrate is welded to the four-pin socket of the planar base by tin and solder paste, and 3-8 mg are weighed to obtain the final sample (Pd-CuO@MOF gas-sensitive material), which is ground and mixed evenly with anhydrous ethanol in an agate mortar to form a slurry. The slurry is applied to the planar electrode substrate with a gold electrode with a fine brush to completely cover the gold electrode, and then inserted into a 4-pin 30-way test board gas sensor planar aging station; it is placed on the aging station of the gas-sensitive component test system to dry and then aged in an air environment at 220°C for two days to obtain the corresponding gas-sensitive element.

[0061] Example 3

[0062] This embodiment provides a modified CuO material and its gas sensor application, which specifically includes the following steps:

[0063] (1) 1.1 g of copper acetate monohydrate is dissolved in 90 ml of deionized water to form solution 1, and 0.5 g of sodium hydroxide is dissolved in 10 ml of deionized water to form solution 2, and the mixture is stirred and dissolved at room temperature (25-27° C.); solution 1 and solution 2 are mixed to obtain a transparent dark blue mixed solution, and then 0.25 g of glucose is added to obtain a mixed solution, and the mixture is stirred and dissolved at room temperature; the obtained mixed solution is slowly heated in a water bath at a heating temperature of 75° C. and reacted for 0.7 h. After the reaction, the precipitate is collected by centrifugation, washed with deionized water for multiple times, and finally collected by centrifugation to obtain a solid product Cu2O.

[0064] (2) The solid product Cu2O obtained in step (1) is placed in a forced air drying oven for drying, and then placed in a muffle furnace for constant temperature calcination at 550° C., and annealed at a rate of 5° C. / min for 3 h to obtain a CuO octahedral material.

[0065] (3) Add 0.2 ml of sodium chloropalladate (concentration of 5 mg / ml) and 4 ml of deionized water to 45 mg of CuO octahedral material to obtain a black mixed solution, which is stirred at room temperature for 0.6 h to dissolve; slowly add 0.2 ml of sodium borohydride (5 mg / ml) dropwise to the black mixed solution and stir at room temperature for 0.6 h to dissolve; after the reaction, collect the precipitate by centrifugation, wash it with deionized water several times, and finally collect it by centrifugation to obtain a solid product Pd-CuO.

[0066] (4) 40 mg of the solid product Pd-CuO was placed in a forced air drying oven to dry the obtained material and 120 mg of 1,3,5-benzenetricarboxylic acid in a polytetrafluoroethylene liner, 30 ml of dimethylformamide and 30 ml of deionized water were added and magnetically stirred to form a mixed solution. The solvent thermal reaction was carried out for 7 hours at a reaction temperature of 80°C to grow a Cu-based MOF on the surface of Pd-CuO to obtain a Pd-CuO@MOF gas-sensitive material.

[0067] (5) The platinum wire of the planar substrate is welded to the four-pin socket of the planar base by tin and solder paste, and 3-8 mg are weighed to obtain the final sample (Pd-CuO@MOF gas-sensitive material), which is ground and mixed evenly with anhydrous ethanol in an agate mortar to form a slurry. The slurry is applied to the planar electrode substrate with a gold electrode with a fine brush to completely cover the gold electrode, and then inserted into a 4-pin 30-way test board gas sensor planar aging station; it is placed on the aging station of the gas-sensitive component test system to dry and then aged in an air environment at 260°C for two days to obtain the corresponding gas-sensitive element.

[0068] Example 4

[0069] This embodiment provides a modified CuO material and its gas sensor application. The specific preparation method is the same as that of Embodiment 1, except that:

[0070] (1) 1.00 g of copper acetate monohydrate, 0.5 g of sodium hydroxide and 0.2 g of glucose were dissolved in 100 ml of deionized water to obtain a mixed solution, which was slowly heated in a water bath at 70° C. for 0.5 h. After the reaction, the precipitate was collected by centrifugation, washed with deionized water for multiple times, and finally collected by centrifugation to obtain a solid product Cu2O.

[0071] Example 5

[0072] This embodiment provides a modified CuO material and its gas sensor application. The specific preparation method is the same as that of Embodiment 1, except that:

[0073] (1) 1.00 g of copper acetate monohydrate is dissolved in 80 ml of deionized water to form solution 1, and 1.00 g of sodium hydroxide is dissolved in 40 ml of deionized water to form solution 2, and the mixture is stirred and dissolved at room temperature (25-27° C.); solution 1 and solution 2 are mixed to obtain a transparent dark blue mixed solution, and then 0.3 g of glucose is added to obtain a mixed solution, and the mixture is stirred and dissolved at room temperature; the obtained mixed solution is slowly heated in a water bath at a heating temperature of 80° C. and reacted for 0.5 h. After the reaction, the precipitate is collected by centrifugation, washed with deionized water for multiple times, and finally collected by centrifugation to obtain a solid product Cu2O.

[0074] Example 6

[0075] This embodiment provides a modified CuO material and its gas sensor application. The specific preparation method is the same as that of Embodiment 1, except that:

[0076] (2) The solid product Cu2O obtained in step (1) is placed in a blast drying oven for drying, and then placed in a muffle furnace for constant temperature calcination at 400° C., and annealed at a rate of 10° C. / min for 2 h to obtain a CuO octahedral material.

[0077] Example 7

[0078] This embodiment provides a modified CuO material and its gas sensor application. The specific preparation method is the same as that of Embodiment 1, except that:

[0079] (4) 40 mg of the solid product Pd-CuO was placed in a forced air drying oven to dry the obtained material and 30 mg of 1,3,5-benzenetricarboxylic acid in a polytetrafluoroethylene liner, 5 ml of dimethylformamide and 20 ml of deionized water were added and magnetically stirred to form a mixed solution. The solution was subjected to solvothermal reaction for 6 h at a reaction temperature of 70 °C to grow a Cu-based MOF on the surface of Pd-CuO to obtain a Pd-CuO@MOF gas-sensitive material.

[0080] Comparative Example 1

[0081] This comparative example provides a modified CuO material and its gas sensor application, and the specific preparation method is as follows:

[0082] (1) 1.00 g of copper acetate monohydrate is dissolved in 80 ml of deionized water to form solution 1, 0.5 g of sodium hydroxide is dissolved in 20 ml of deionized water to form solution 2, and the mixture is stirred and dissolved at room temperature (25-27° C.); solution 1 and solution 2 are mixed to obtain a transparent dark blue mixed solution, and then 0.2 g of glucose is added to obtain a mixed solution, and the mixture is stirred and dissolved at room temperature; the obtained mixed solution is slowly heated in a water bath at a heating temperature of 70° C. for a reaction of 0.5 h, and after the reaction, the precipitate is collected by centrifugation, washed with deionized water for multiple times, and finally collected by centrifugation to obtain a solid product Cu2O.

[0083] (2) The solid product Cu2O obtained in step (1) is placed in a blast drying oven for drying, and then placed in a muffle furnace for constant temperature calcination at 500° C., and annealed at a rate of 2.5° C. / min for 2 h to obtain a CuO octahedral material.

[0084] (3) Solder the platinum wire of the planar substrate to the four-pin socket of the planar base by tin and solder paste, weigh 3-8 mg of the final sample prepared in step (2), grind and mix with anhydrous ethanol in an agate mortar to form a slurry, use a fine brush to dip the slurry and apply it on the planar electrode substrate with gold electrodes to completely cover the gold electrodes, and then insert it into a 4-pin 30-way test board gas sensor plane aging station; place it on the aging station matching the gas sensitive component test system to dry, and then age it in an air environment at 240°C for two days to obtain the corresponding gas sensitive element.

[0085] Comparative Example 2

[0086] This comparative example provides a modified CuO material and its gas sensor application, and the specific preparation method is as follows:

[0087] (1) 0.2 ml of sodium chloropalladate (concentration of 5 mg / ml) and 3 ml of deionized water were added to 40 mg of the CuO octahedral material prepared in Comparative Example 1 to obtain a black mixed solution, which was stirred at room temperature for 0.5 h to dissolve; 0.2 ml of sodium borohydride (5 mg / ml) was slowly added dropwise to the black mixed solution, and stirred at room temperature for 0.5 h to dissolve; after the reaction, the precipitate was collected by centrifugation, washed with deionized water for multiple times, and finally collected by centrifugation to obtain a solid product Pd-CuO.

[0088] (2) Solder the platinum wire of the planar substrate to the four-pin socket of the planar base by tin and solder paste, weigh 3-8 mg of the final sample prepared in step (1), grind and mix with anhydrous ethanol in an agate mortar to form a slurry, use a fine brush to dip the slurry and apply it on the planar electrode substrate with gold electrodes to completely cover the gold electrodes, and then insert it into a 4-pin 30-way test board gas sensor plane aging station; place it on the aging station matching the gas sensitive component test system to dry, and then age it in an air environment at 240°C for two days to obtain the corresponding gas sensitive element.

[0089] Comparative Example 3

[0090] This comparative example provides a modified CuO material and its gas sensor application, and the specific preparation method is as follows:

[0091] (1) 40 mg of the CuO octahedral material prepared in Comparative Example 1 was placed in a blast drying oven and dried. The obtained material and 80 mg of 1,3,5-benzenetricarboxylic acid were placed in a polytetrafluoroethylene liner, 20 ml of dimethylformamide and 20 ml of deionized water were added and magnetically stirred to form a mixed solution. The solution was subjected to solvent thermal reaction for 6 h at a reaction temperature of 70° C., so that the Cu-based MOF was grown on the surface of CuO to obtain a CuO@MOF gas-sensitive material.

[0092] (2) Solder the platinum wire of the planar substrate to the four-pin socket of the planar base by tin and solder paste, weigh 3-8 mg of the final sample prepared in step (1), grind and mix with anhydrous ethanol in an agate mortar to form a slurry, use a fine brush to dip the slurry and apply it on the planar electrode substrate with gold electrodes to completely cover the gold electrodes, and then insert it into a 4-pin 30-way test board gas sensor plane aging station; place it on the aging station matching the gas sensitive component test system to dry, and then age it in an air environment at 240°C for two days to obtain the corresponding gas sensitive element.

[0093] Performance Testing

[0094] The acetone sensing performance of the gas sensors prepared in the embodiments and comparative examples was tested. The response value of the gas sensor to acetone was tested in the humidity range of 40-90% RH. The response value was defined as the ratio of Rg (resistance when exposed to the test gas) to Ra (resistance exposed to the air), and the coefficient of variation was calculated, where the coefficient of variation was the standard deviation / average value of multiple response values ​​measured within the humidity range. The smaller the coefficient of variation, the better the moisture resistance. The results are shown in Table 1.

[0095] Table 1

[0096]

[0097] Figure 1 The electron microscope image of the modified CuO material sample of Example 1 is shown. Figure 2 The electron microscope images of the modified CuO material samples of comparative examples 1-3 are shown. It can be seen from the figure that the sample of comparative example 1 is octahedral and the particle size is about 1 μm; a number of nano-scale granular substances can be observed on the surface of the sample of comparative example 2, and the morphology is octahedral; the surface of the sample of comparative example 3 is wrapped by a number of small particles, and the surface has obvious changes compared with comparative example 2, but the morphology is still octahedral; the sample of embodiment 1 and its EDS mapping image clearly show the presence of Pd element, indicating that Pd nanoparticles are uniformly distributed on the octahedral Pd-CuO@MOF.

[0098] Figure 3 The X-ray diffraction patterns of the modified CuO material samples of Example 1 and Comparative Examples 1-3 are shown. It can be seen from the figure that clear diffraction peaks are observed in all four groups of samples, and they match the CuO standard card (PDF#89-5895), indicating that the samples have very high purity. On the other hand, new diffraction peaks appear in the samples of Comparative Example 3 and Example 1, which indicates the successful synthesis of the Cu-based MOF structure.

[0099] Figure 4 The response values ​​of the gas sensors prepared in Example 1 and Comparative Examples 1-3 to 50 ppm acetone at different operating temperatures are shown. It can be seen from the figure that the optimal operating temperature of the gas sensor based on CuO octahedral material is 190°C.

[0100] Figure 5-8The concentration-resistance relationship of the gas sensors prepared in Example 1 and Comparative Examples 1-3 at the optimal working temperature for acetone, as shown in the figure, indicates that each sensor can show an observable response to acetone of different concentrations (5-100ppm), which is due to the fact that the high-energy crystal face of the CuO octahedral gas-sensitive material is exposed to the maximum extent, and its higher surface energy is conducive to the gas adsorption process, and gas adsorption is a key step in the gas-sensitive reaction. Compared with Comparative Example 1 (the response value to 50ppm acetone is 1.61), the sensors of Comparative Example 2, Comparative Example 3, and Example 1 have better sensitivity (Comparative Example 2 is 2.94, Comparative Example 3 is 2.49, and Example 1 is 4.05), among which the response value of Example 1 is increased by about 2.52 times compared with Comparative Example 1. Most importantly, compared with Comparative Example 1, the sensors of Comparative Example 2, Comparative Example 3, and Example 1 have better moisture resistance.

[0101] Fig. 9 The humidity coefficient of variation and response value of the gas sensors prepared for Example 1 and Comparative Examples 1-3 to 50ppm acetone under different humidity conditions. It can be seen from the figure that in the humidity range of 40-90%RH, the gas sensors of Comparative Example 2, Comparative Example 3, and Example 1 show a nearly constant response to 50ppm acetone, and their humidity coefficients of variation are all less than the humidity coefficient of variation of Comparative Example 1, among which, Comparative Example 2 is 10.06%, Comparative Example 3 is 8.14%, and its humidity coefficient of variation is less than 10%, and Example 1 is 4.46%, and its humidity coefficient of variation is less than 5%. Compared with the gas sensor of Comparative Example 1, the humidity coefficient of variation of the gas sensor constructed based on Pd-CuO@MOF is significantly reduced, and the dual improvement of sensitivity and moisture resistance is due to the successful construction of the Pd-CuO@MOF composite structure.

[0102] As can be seen from Table 1, by comparing Examples 1-3, it can be seen that the modified CuO material prepared by the technical solution of the present invention can be applied to gas sensors to achieve both improved moisture resistance and sensitivity; by comparing Example 1 with Examples 4 and 5, it can be seen that changing the reaction operation sequence or the ratio of the raw materials will affect the crystal structure of Cu2O, and octahedral Cu2O cannot be obtained, thereby affecting the performance of the prepared gas sensor; by comparing Example 1 with Example 6, Cu2O-CuO octahedron is prepared in Example 6, and it can be seen that adjusting the calcination process parameters will affect the reduction degree of CuO, thereby affecting the performance of the prepared gas sensor; by comparing Example 1 with Example 7, it can be seen that the amount of organic ligand added will affect the formation of Cu-based MOF, thereby affecting the performance of the prepared gas sensor.

[0103] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A modified CuO material, Features: The modified CuO material includes octahedral CuO, noble metal Pd NPs and Cu-based MOF, wherein the noble metal Pd NPs are modified on the surface of the octahedral CuO, and the Cu-based MOF grows on the surface of the CuO modified with the noble metal Pd NPs to achieve hydrophobic coating; The preparation method of the modified CuO material comprises the following steps: S1. Mix the copper acetate solution and the sodium hydroxide solution, add a reducing agent, stir and dissolve, and heat in a water bath to react to obtain a solid product Cu 2 O; S2, the solid product Cu 2 O is dried and calcined at a constant temperature to obtain CuO, wherein the CuO is octahedral; S3, dissolving CuO and sodium chloropalladate in water, adding sodium borohydride, and reacting to obtain a solid product Pd-CuO; S4. Mixing the solid product Pd-CuO with an organic ligand, dimethylformamide and water for a solvothermal reaction to obtain a modified CuO material, wherein the mass ratio of the solid product Pd-CuO, the organic ligand and dimethylformamide is 1:1-3:0.2-0.7, and the organic ligand is 1,3,5-benzenetricarboxylic acid.

2. A modified CuO material as claimed in claim 1, Features: In step S1, the mass ratio of the copper acetate, sodium hydroxide and reducing agent is 1.8-2.2:1:0.3-0.

5.

3. A modified CuO material as claimed in claim 2, Features: The reducing agent is glucose, the water bath heating temperature is 65-75° C., and the water bath heating time is 0.3-0.7 h.

4. A modified CuO material as claimed in claim 1, Features: In step S2, the constant temperature calcination temperature is 450-550°C, the constant temperature calcination atmosphere is air, and the annealing is performed at a rate of 1-5°C / min for 1-3h.

5. A modified CuO material as claimed in claim 1, Features: In step S3, the mass ratio of CuO, sodium chloropalladate and sodium borohydride is 35-45:1:1, the reaction temperature is 25-27° C., and the reaction time is 0.8-1.2 h.

6. A modified CuO material as claimed in claim 1, Features: In step S4, the temperature of the solvent thermal reaction is 60-80° C., and the reaction time is 5-7 h.

7. Use of a modified CuO material as claimed in claim 1, Features: The modified CuO material is made into slurry and coated on the gas sensor body.

8. Use of a modified CuO material as claimed in claim 7, Features: The modified CuO material and anhydrous ethanol were ground into a slurry, the slurry was coated on a planar electrode substrate with a gold electrode to completely cover the gold electrode, dried to form a film, and aged at 220-260° C. to obtain a Pd-CuO@MOF acetone sensor.