Etching ink, preparation method and application of etching ink to patterned floor in digital printing
The preparation of etching inks for components such as polyurethane modified epoxy acrylate polymers has solved the problems of slow curing speed and weak adhesion inks, and achieved rapid curing and strong adhesion, which improved digital printing to flower floors texture clarity and layering.
Patent Information
- Application Number
- CN202411105056.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The existing etching inks are slow curing speed, weak adhesion and complex operation in digital printing flooring process, which affects the clarity of the texture and sense of layering.
The etching ink is prepared by non-UV stirring using polyurethane modified epoxy acrylate polymer, photosensitive material, modified epoxy resin and photoinitiator. In digital printing, the embossing of different heights is formed by UV irradiation. Effect.
It realizes etching ink with good storage stability, fast curing, strong adhesion and smooth printing, improving the depth and three-dimensional effect of the texture.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inkjet ink, and in particular to an etching ink, a preparation method and application of the etching ink to a patterned floor in digital printing. Background Art
[0002] Digital printing flooring production process is a modern technology that uses high-precision digital printers to print high-resolution patterns and textures directly on artificial wood floor substrates. The digital printing flooring production process uses digital printing to achieve accurate replication and pattern matching, and then uses UV curing technology to quickly cure the ink to form a durable and realistic floor surface. Compared with traditional processes, digital printing reduces production steps, reduces costs, and improves production efficiency.
[0003] Etching ink plays a key role in the production process of digital printed flooring. It creates realistic texture effects on the floor surface through special chemical or physical effects. During the digital printing process, etching ink is accurately printed onto the floor substrate, and then processed through specific processes such as ultraviolet light irradiation or chemical reaction, so that the ink forms concave or convex textures on the floor surface, simulating the texture of natural materials such as wood and stone. This technology not only enhances the beauty and realism of the floor, but also improves the durability and touch of the product.
[0004] CN115873447B discloses an inkjet etching ink and a preparation method thereof, wherein the inkjet etching ink comprises the following components: 47-67 parts of a water-soluble monofunctional monomer, 15-25 parts of a water-soluble multifunctional monomer, 3-7 parts of an alkali-soluble UV resin, 7-13 parts of a polyvinyl alcohol resin, 5-9 parts of a photoinitiator, and 1-3 parts of a water-soluble leveling agent. The inkjet etching ink provided by the invention can form a UV printing inkjet layer after printing on a PVC or SPC substrate. After light curing, the surface of the UV printing inkjet layer is slightly polished to expose it to the outside, and then the UV printing inkjet layer is dissolved by high-pressure washing with hot water, thereby producing a texture that is synchronized with the pattern of the substrate, thereby obtaining an artificial wood floor with a deeper texture, a more layered and three-dimensional effect. Although the etching ink can increase the clarity of the texture on the artificial wood board, it has a slow curing speed, weak adhesion, and a complex operation process for forming textures in the artificial wood floor. Summary of the invention
[0005] In view of the above-mentioned defects of the prior art, the present invention provides an etching ink, which has the characteristics of good storage stability, fast curing speed, strong adhesion and good printing fluency, and simple operation process.
[0006] The present invention provides a method for preparing etching ink, comprising the following steps:
[0007] Under non-ultraviolet light and stirring conditions, a photocurable polymer is added to a photosensitive material to obtain a mixture; a photoinitiator, a modified epoxy resin, a leveling agent and a pigment are sequentially added to the mixture, and the mixture is stirred until completely dissolved to obtain etching ink.
[0008] Preferably, the weight ratio of each raw material component is:
[0009] 35-55 parts of photocurable polymer, 50-70 parts of photosensitive material, 1-5 parts of photoinitiator, 5-10 parts of modified epoxy resin, 0.5-2 parts of leveling agent, and 0.1-0.5 parts of pigment.
[0010] Preferably, the photocurable polymer is selected from one of polyurethane-modified epoxy acrylate polymer, polyurethane acrylate resin and epoxy acrylate UV resin.
[0011] Preferably, the preparation method of the polyurethane modified epoxy acrylate polymer comprises the following steps, measured in parts by weight:
[0012] S1, adding 35-40 parts of epoxy acrylate UV resin, 20-25 parts of ε-caprolactone and 1-1.5 parts of stannous octoate into a reactor, mixing, heating, and reacting at a constant temperature of 110-120° C. at a stirring speed of 150-300 r / min, measuring the ε-caprolactone content in the reaction liquid system every 1 hour, stopping the reaction when the ε-caprolactone content drops to 0, cooling, discharging and setting aside, and obtaining an epoxy acrylate prepolymer;
[0013] S2, 35-45 parts of isophorone diisocyanate, 0.1-0.3 parts of dibutyltin dilaurate and 0.01-0.05 parts of p-hydroxyanisole are added to a reactor and mixed, the temperature is raised to 50-60°C for insulation, 20-25 parts of hydroxyethyl acrylate are dripped into the reactor, after the dropwise addition is completed, the reaction is carried out at a constant temperature of 50-60°C at a stirring speed of 150-300r / min, the -NCO group content in the reaction system is measured every 1h, the reaction is stopped when the -NCO group content drops to half of the initial content, the material is discharged for standby use, and an isocyanate-containing prepolymer is obtained;
[0014] S3. Add 50-60 parts of epoxy acrylate prepolymer, 60-65 parts of isocyanate prepolymer and 0.1-0.2 parts of dibutyltin dilaurate into a reactor, mix, heat up, and react at a constant temperature of 65-75° C. at a stirring speed of 150-300 r / min. Determine the -NCO group content in the reaction system every 1 hour. When the -NCO group content of the reaction system reaches 0, stop the reaction to obtain a polyurethane-modified epoxy acrylate polymer.
[0015] Preferably, the photosensitive material is a mixture of a photosensitive monomer and trimethylolpropane tris(3-mercaptopropionate) in a weight ratio of 15-20:0.2-0.5.
[0016] Preferably, the photosensitive monomer is selected from one of vinyl ether acrylate, 1,6-hexanediol diacrylate and tripropylene glycol diacrylate.
[0017] Preferably, the leveling agent is selected from at least one of polyacrylate leveling agents and polymethylsiloxane leveling agents.
[0018] Preferably, the pigment is an organic pigment.
[0019] Preferably, the preparation method of the modified epoxy resin comprises the following steps, measured by weight:
[0020] 4-6 parts of o-cresol epoxy resin and 6-8 parts of diethylene glycol monoethyl ether acetate are added to a reactor and mixed, the mixture is heated, and the mixture is stirred at a constant temperature of 80-90°C for 20-60 minutes at a stirring speed of 150-300 r / min to obtain a mixed solution A; the mixture is cooled to room temperature, 1.5-2.5 parts of 10-undecynoic acid, 0.02-0.05 parts of catalyst 4-dimethylaminopyridine and 0.05-0.1 parts of inhibitor hydroquinone are added to the mixed solution A, the mixture is heated, and the mixture is stirred at a constant temperature of 95-105°C for 2-4 hours at a stirring speed of 150-300 r / min to obtain a mixed solution B; the mixture is cooled to room temperature, 3-4 parts of tetrahydrophthalic anhydride and 0.01-0.03 parts of hydroquinone are added to the mixed solution B, and the mixture is stirred at a constant temperature of 90-100°C for 2-4 hours at a stirring speed of 150-300 r / min to obtain a modified epoxy resin.
[0021] Preferably, the photoinitiator is a mixture of a free radical photoinitiator and a cationic photoinitiator in a weight ratio of 3-5:1.
[0022] Further preferably, the free radical photoinitiator is selected from at least one of (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, 2-isopropylthioxanthone, benzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, and α-hydroxyisopropylbenzophenone; the cationic photoinitiator is selected from at least one of diphenyliodonium hexafluoroarsenate, benzanilide salt, and benzoylphenothiazine salt.
[0023] The invention also provides an etching ink prepared by the above preparation method.
[0024] The present invention also provides the use of the etching ink in digital printing of a patterned floor, wherein the etching ink forms a pattern of the patterned floor in the form of inkjet printing.
[0025] The method for preparing the digitally printed pattern floor comprises the following steps:
[0026] (1) Design pattern: Design the drawing files in layers, input the drawing and embossed pattern layers into the printer in layers, and set the corresponding colors for the embossed patterns;
[0027] (2) Printing pattern: Print UV ink on the substrate layer according to the pattern designed in step (1) to form a pattern texture, and then print etching ink on the formed pattern texture to form a mixed ink printing layer; then use UV paint for multi-layer UV coating to form a protective layer on the mixed ink layer. After drying under UV light, the etching ink in the mixed ink printing layer absorbs UV energy and peels off the surface UV paint from the bottom, thereby forming embossing of varying heights;
[0028] (3) Embossing treatment: Use film pressing or rolling to make fine embossing on the pattern, so that the surface texture is deep and shallow, and a digitally printed pattern floor is obtained.
[0029] Preferably, the substrate layer in step (2) is a single substrate layer or a composite substrate layer; further, the substrate layer includes a white film coated with white or containing a polymer on the substrate layer, a polymer sheet, an inorganic calcium silicate board, a glass magnesium board, and the substrate layer is a random combination of one or more thereof.
[0030] The etching ink provided by the present invention can obtain a cleavable UV printing inkjet layer after printing on a substrate, and then a corresponding UV paint protective layer is coated on the surface. After being irradiated by a UV lamp, the etching ink undergoes a chemical reaction inside after absorbing UV energy, resulting in volume expansion or the generation of gas to generate a large internal pressure. This internal pressure will act on the UV paint protective layer above it, and the UV paint on the surface can be peeled off from below, thereby forming an embossed pattern that is synchronized with the substrate pattern and has different heights, and a floor with a deeper pattern, a more layered and three-dimensional effect can be obtained.
[0031] Beneficial effects of the present invention:
[0032] The present invention prepares an etching ink with good storage stability, fast curing speed, good adhesion and good printing fluency by rationally proportioning each raw material component. The etching ink provided by the present invention is applied to digital printing of flowered flooring. Under ultraviolet light irradiation, the photoinitiator 2-benzyl-2-dimethylamino-1-(4-morpholinephenyl)butanone and diphenyliodonium hexafluoroarsenate absorb light energy to activate, generate free radicals or ions, and trigger a polymerization reaction. In this process, vinyl ether acrylate rapidly undergoes polymerization reaction under the action of free radicals generated by the photoinitiator to form a preliminary cross-linked network. At the same time, the thiol group in trimethylolpropane tris (3-mercaptopropionate) and the alkynyl group in the modified epoxy resin undergo a thiol-alkyne click chemical reaction to further enhance the cross-linking density. At the same time, the epoxy group and acrylate group in the polyurethane-modified epoxy acrylate polymer participate in the polymerization reaction, increasing the complexity and cross-linking degree of the network. As the polymerization reaction proceeds, the liquid components in the ink are transformed into solid polymers, which shrink in volume. The resulting large internal stress acts on the UV paint protective layer above, peeling off the UV paint on the surface from below, thus forming cracks. DETAILED DESCRIPTION
[0033] Parameters for specific chemical substances used, sources.
[0034] Polyacrylate leveling agent, grade: BYK-358N, brand: BYK, Germany;
[0035] Epoxy acrylate UV resin, grade: 621A-80, brand: Changxing, Taiwan, China;
[0036] o-Cresol epoxy resin, brand: NPCN-704, brand: Taiwan Nanya, China;
[0037] Vinyl ether acrylate, CAS number: 86273-46-3, from Hubei Baidu Chemical Co., Ltd., product number: BD8626;
[0038] Polyurethane acrylate resin, sourced from Hunan Jinhai Technology Co., Ltd., item number: JS230;
[0039] UV ink, brand: LUS-210, brand: mimaki;
[0040] UV matte primer, grade: HB-4301, brand: Jiangsu Haitian.
[0041] Embodiment 1,
[0042] A method for preparing etching ink comprises the following steps:
[0043] 40 parts by weight of polyurethane modified epoxy acrylate polymer and 60 parts by weight of photosensitive material are mixed and stirred at 600 r / min, 35° C. and non-ultraviolet light conditions for 30 minutes to obtain a mixture; 3 parts by weight of photoinitiator, 8 parts by weight of modified epoxy resin, 1 part by weight of polyacrylate leveling agent and 0.15 parts by weight of oil-soluble yellow are added to the mixture in sequence, and the mixing and stirring is continued at 600 r / min, 35° C. and non-ultraviolet light conditions for 30 minutes to obtain etching ink.
[0044] The preparation method of the polyurethane modified epoxy acrylate polymer comprises the following steps:
[0045] S1, 38 parts by weight of epoxy acrylate UV resin, 22 parts by weight of ε-caprolactone and 1.3 parts by weight of stannous octoate are added to a reactor and mixed, the temperature is raised, and the reaction is carried out at a constant temperature of 112° C. under a stirring speed of 200 r / min, and the ε-caprolactone content in the reaction liquid system is measured every 1 hour. When the ε-caprolactone content drops to 0, the reaction is stopped, the reaction is cooled, and the material is discharged for standby use, thereby obtaining an epoxy acrylate prepolymer;
[0046] S2, 40 parts by weight of isophorone diisocyanate, 0.2 parts by weight of dibutyltin dilaurate and 0.03 parts by weight of p-hydroxyanisole are added to a reactor and mixed, the temperature is raised to 55°C for insulation, 22 parts by weight of hydroxyethyl acrylate is dripped into the reactor at a drip rate of 2 drops / s, after the dropwise addition is completed, the reaction is carried out at a constant temperature of 55°C at a stirring speed of 200r / min, the -NCO group content in the reaction system is measured every 1h, the reaction is stopped when the -NCO group content drops to half of the initial content, the material is discharged for standby use, and an isocyanate-containing prepolymer is obtained;
[0047] S3. Add 55 parts by weight of epoxy acrylate prepolymer, 62 parts by weight of isocyanate prepolymer and 0.1 parts by weight of dibutyltin dilaurate into a reactor, mix, heat up, and react at a constant temperature of 70°C with a stirring speed of 200 r / min. Measure the -NCO group content in the reaction system every 1 hour. When the -NCO group content of the reaction system reaches 0, stop the reaction to obtain a polyurethane-modified epoxy acrylate polymer.
[0048] The preparation method of the modified epoxy resin comprises the following steps:
[0049] 5 parts by weight of o-cresol epoxy resin and 7 parts by weight of diethylene glycol monoethyl ether acetate are added to a reactor and mixed, the temperature is increased, and the mixture is stirred at a constant temperature of 85°C for 30 minutes at a stirring speed of 200 r / min to obtain a mixed solution A; after cooling to room temperature, 2 parts by weight of 10-undecynoic acid, 0.03 parts by weight of catalyst 4-dimethylaminopyridine and 0.07 parts by weight of inhibitor hydroquinone are added to the mixed solution A, the temperature is increased, and the mixture is stirred at a constant temperature of 100°C for 3 hours at a stirring speed of 200 r / min to obtain a mixed solution B; after cooling to room temperature, 3.5 parts by weight of tetrahydrophthalic anhydride and 0.02 parts by weight of hydroquinone are added to the mixed solution B, and the mixture is stirred at a constant temperature of 95°C for 3 hours at a stirring speed of 200 r / min to obtain a modified epoxy resin.
[0050] The photosensitive material is a mixture of vinyl ether acrylate and trimethylolpropane tris(3-mercaptopropionate) at a weight ratio of 18:0.4.
[0051] The photoinitiator is a mixture of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone and diphenyliodonium hexafluoroarsenate in a weight ratio of 4:1.
[0052] The etching ink prepared in this embodiment is used to prepare a digital printed floor, and the preparation method of the digital printed floor comprises the following steps:
[0053] (1) Design pattern: Design the drawing files in layers, input the drawing and embossed pattern layers into the printer in layers, and set the corresponding colors for the embossed patterns;
[0054] (2) Printing pattern: Print UV ink on the calcium silicate board according to the pattern designed in step (1) to form a pattern texture, and then print etching ink on the formed pattern texture to form a mixed ink printing layer; then use UV matte primer to perform multi-layer UV coating to form a protective layer on the mixed ink layer. After drying under UV light, the etching ink in the mixed ink printing layer absorbs UV energy and peels off the UV paint on the surface from the bottom, thereby forming embossing of varying heights;
[0055] (3) Embossing treatment: Use film pressing or rolling to make fine embossing on the pattern, so that the surface texture is deep and shallow, and a digitally printed pattern floor is obtained.
[0056] Embodiment 2,
[0057] The difference between the method for preparing etching ink and Example 1 is that the photosensitive material is a mixture of 1,6-hexanediol diacrylate and trimethylolpropane tris(3-mercaptopropionate) in a weight ratio of 18:0.4.
[0058] The etching ink prepared in this example is used to prepare a digitally printed flooring, and the preparation method of the digitally printed flooring is consistent with that of Example 1.
[0059] Embodiment 3,
[0060] The difference between the method for preparing etching ink and Example 1 is that the photosensitive material is a mixture of tripropylene glycol diacrylate and trimethylolpropane tris(3-mercaptopropionate) in a weight ratio of 18:0.4.
[0061] The etching ink prepared in this example is used to prepare a digitally printed flooring, and the preparation method of the digitally printed flooring is consistent with that of Example 1.
[0062] Embodiment 4,
[0063] The difference between the method for preparing an etching ink and Example 1 is that 40 parts by weight of the polyurethane-modified epoxy acrylate polymer is replaced with 40 parts by weight of polyurethane acrylate resin.
[0064] The etching ink prepared in this example is used to prepare a digitally printed flooring, and the preparation method of the digitally printed flooring is consistent with that of Example 1.
[0065] Embodiment 5,
[0066] The difference between the method for preparing an etching ink and Example 1 is that 40 parts by weight of the polyurethane-modified epoxy acrylate polymer is replaced with 40 parts by weight of epoxy acrylate UV resin.
[0067] The etching ink prepared in this example is used to prepare a digitally printed flooring, and the preparation method of the digitally printed flooring is consistent with that of Example 1.
[0068] Comparative Example 1
[0069] The difference between a method for preparing etching ink and Example 1 is that the photosensitive material is vinyl ether acrylate.
[0070] Comparative Example 2
[0071] A method for preparing etching ink comprises the following steps:
[0072] 40 parts by weight of polyurethane-modified epoxy acrylate polymer and 60 parts by weight of photosensitive material were mixed and stirred at 600 r / min, 35° C. and non-ultraviolet light conditions for 30 minutes to obtain a mixture; 3 parts by weight of photoinitiator, 1 part by weight of polyacrylate leveling agent and 0.15 parts by weight of oil-soluble yellow were added to the mixture in sequence, and the mixture was mixed and stirred at 600 r / min, 35° C. and non-ultraviolet light conditions for 30 minutes to obtain etching ink.
[0073] The preparation method of the polyurethane modified epoxy acrylate polymer is consistent with that in Example 1.
[0074] The photosensitive material is a mixture of vinyl ether acrylate and trimethylolpropane tris(3-mercaptopropionate) at a weight ratio of 18:0.4.
[0075] The photoinitiator is a mixture of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone and diphenyliodonium hexafluoroarsenate in a weight ratio of 4:1.
[0076] The etching ink prepared in this example is used to prepare a digitally printed flooring, and the preparation method of the digitally printed flooring is consistent with that of Example 1.
[0077] Comparative Example 3
[0078] A method for preparing etching ink comprises the following steps:
[0079] 40 parts by weight of polyurethane modified epoxy acrylate polymer and 60 parts by weight of photosensitive material were mixed and stirred at 600 r / min, 35° C. and non-ultraviolet light conditions for 30 minutes to obtain a mixture; 3 parts by weight of photoinitiator, 8 parts by weight of modified epoxy resin and 0.15 parts by weight of oil-soluble yellow were added to the mixture in sequence, and the mixture was mixed and stirred at 600 r / min, 35° C. and non-ultraviolet light conditions for 30 minutes to obtain etching ink.
[0080] The preparation method of the polyurethane modified epoxy acrylate polymer is consistent with that in Example 1.
[0081] The photosensitive material is a mixture of vinyl ether acrylate and trimethylolpropane tris(3-mercaptopropionate) at a weight ratio of 18:0.4.
[0082] The preparation method of the modified epoxy resin is consistent with that of Example 1.
[0083] The photoinitiator is a mixture of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone and diphenyliodonium hexafluoroarsenate in a weight ratio of 4:1.
[0084] The etching ink prepared in this example is used to prepare a digitally printed flooring, and the preparation method of the digitally printed flooring is consistent with that of Example 1.
[0085] Test Example 1:
[0086] Curing performance test
[0087] Light curing time test method: According to the standard "QB / T4580-2013 UV light curing inkjet printing ink", the inks of Examples 1-5 and Comparative Examples 1-3 were tested for light curing time. The shorter the curing time, the better the curing performance.
[0088] The test results of the time taken for light curing are shown in Table 1.
[0089] Adhesion test
[0090] Test method: According to the standard "QB / T4580-2013 UV-curable inkjet printing ink", the inks of Examples 1-5 and Comparative Examples 1-3 were tested for adhesion, requiring the adhesion level to be level 0, i.e., no peeling.
[0091] The test results are shown in Table 1.
[0092] Printing Fluency Test
[0093] Test method: The inks of Examples 1-5 and Comparative Examples 1-3 were respectively used for continuous printing on an inkjet printer for 10 minutes. 2 The number of broken lines of the pattern nozzle is the printing smoothness of the ink. The more broken lines there are, the worse the ink smoothness is; the printing effect is obtained by visual inspection.
[0094] The test results are shown in Table 1;
[0095]
[0096] It can be seen from the test results in Table 1 that the etching inks prepared by the embodiments of the present invention and the comparative examples can be quickly cured under ultraviolet light, wherein the photocuring time of the etching inks corresponding to embodiments 1-5 and comparative example 3 is less than the photocuring time of the etching inks corresponding to comparative examples 1-2, and the photocuring time of the etching ink corresponding to embodiment 1 is as low as 7s; through the adhesion test, it can be seen that the adhesion test of the etching inks prepared by embodiments 1-5 and comparative example 3 is level 0, and the adhesion is better than that of comparative examples 1-2. Based on the differences in the photocuring time and adhesion test results of each embodiment and comparative example in Table 1, the reason may be that compared with traditional polyurethane acrylate resins and epoxy acrylate UV resins, polyurethane-modified epoxy acrylate polymers contain epoxy groups and acrylate groups, and under ultraviolet light, they can be mixed with a photoinitiator composed of 2-benzyl-2-dimethylamino-1-(4-morpholinephenyl)butanone and diphenyliodonium hexafluoroarsenate to undergo crosslinking and free radical polymerization reactions, and this multiple reactivity helps to accelerate the curing speed. In addition, the introduction of ε-caprolactone units into the polyurethane-modified epoxy acrylate polymer can increase the flexibility of the polymer and help partially release the internal stress generated by rapid curing during UV curing, thereby improving the curing speed and adhesion. At the same time, the vinyl ether acrylate in the photosensitive material is used in conjunction with the polyurethane-modified epoxy acrylate polymer. The vinyl ether acrylate can not only be used as an active diluent to improve the activity and reactivity of the polyurethane-modified epoxy acrylate polymer and accelerate the curing speed, but also the vinyl ether group in the vinyl ether acrylate is highly reactive and can react quickly with free radicals under UV light to form a cross-linked structure, further accelerating the photocuring process. In addition, the thiol group in the trimethylolpropane tris (3-mercaptopropionate) structure in the photosensitive material can react with the alkyne group in the modified epoxy resin by a thiol-alkyne click reaction, which can be rapidly and efficiently photocured under UV light initiation, accelerating the photocuring process, and forming a highly cross-linked network structure during the photocuring process, which may enhance the adhesion between the cured film and the substrate.
[0097] It can be seen from the printing fluency test results of Table 1 that Examples 1-3 and Comparative Example 1 are smooth and clear in inkjet printers, and there is no nozzle clogging, and the printing fluency is better than Examples 4-5 and Comparative Examples 2-3. The reason for the analysis may be that the introduction of the ε-caprolactone unit in the polyurethane-modified epoxy acrylate polymer increases the flexibility of the molecular chain, resulting in a decrease in viscosity, which is conducive to improving the printing fluency of the ink. At the same time, since the 10-undecynoic acid-modified epoxy resin introduces a longer carbon chain in the modified epoxy resin structure, this helps to improve the viscosity of the ink and is conducive to improving the printing fluency of the ink. In addition, the introduction of polyacrylate leveling agents can improve the wettability and fluidity of the ink, and can reduce the pores and foams generated by the ink during stirring and printing. The present invention uses polyurethane-modified epoxy acrylate polymers, modified epoxy resins and polyacrylate leveling agents in coordination, which is conducive to the flow of ink in the nozzle during printing, and can reduce the risk of clogging the nozzle, thereby improving the printing fluency of the ink during printing.
[0098] Test Example 2:
[0099] Storage stability test
[0100] Test method: Use a rheometer (Anton Paar Shanghai Trading Co., Ltd., model: MCR 302) to test the initial viscosity of the inks of Examples 1-5 and Comparative Examples 1-3, respectively. After the inks of each Example and Comparative Example are stably placed at room temperature and in a light-proof environment for 3 months, 6 months, 12 months, and 24 months, the viscosity of the ink after placement is tested again, and the change rate (%) of the ink viscosity after placement to the initial viscosity is calculated. The greater the viscosity change rate, the more unstable the ink is. The viscosity change rate is less than 3%, which means the stability is qualified. The calculation formula of the viscosity change rate (%) is as follows:
[0101] Viscosity change rate (%) = |A X -A0| / A0×100%
[0102] In the formula, A X is the ink viscosity after placement (mPa•s), and A0 is the initial ink viscosity (mPa•s).
[0103] The test results are shown in Table 2;
[0104]
[0105] From the test results in Table 2, it can be seen that the viscosity change rate of Examples 1-5 and Comparative Examples 1-3 is less than 3% after stable storage for 24 months, and has good storage stability, while the viscosity change rate of Comparative Example 3 is greater than 3% when stored for 12 months, and has poor storage stability. Comparing the change range of the viscosity change rate of Comparative Examples 1-5 and Comparative Examples 1-2 with the increase of storage time, it is found that the change range of Examples 1 and Comparative Examples 1-2 is smaller than that of Examples 2-5, among which the change range of Example 1 is the smallest, indicating that Example 1 has the best storage stability. The reason for the analysis may be that in the preparation process of polyurethane-modified epoxy acrylate polymer, the urethane bond generated by the reaction of isophorone diisocyanate and hydroxyethyl acrylate has good chemical stability and aging resistance, which helps to maintain the stability of the ink during storage. At the same time, the vinyl ether group in vinyl ether acrylate has high chemical stability, and is not prone to heat or light-induced degradation reactions during long-term storage, which helps to maintain the long-term stability of the ink. In addition, the leveling agent can improve the fluidity and wettability of the ink, reduce the sedimentation or stratification of components that may occur during storage, help maintain the uniformity of the ink, and maintain the stability of the ink during long-term storage.
Claims
1. A method for preparing etching ink, characterized in that: The following steps are involved: Under non-ultraviolet light and stirring conditions, adding a photocurable polymer to a photosensitive material to obtain a mixture; adding a photoinitiator, a modified epoxy resin, a leveling agent and a pigment to the mixture in sequence, stirring until completely dissolved, to obtain an etching ink; The weight proportion of each raw material component is: 35-55 parts of photocurable polymer, 50-70 parts of photosensitive material, 1-5 parts of photoinitiator, 5-10 parts of modified epoxy resin, 0.5-2 parts of leveling agent, 0.1-0.5 parts of pigment; The photocurable polymer is a polyurethane modified epoxy acrylate polymer; The photosensitive material is a mixture of a photosensitive monomer and trimethylolpropane tris(3-mercaptopropionate) at a weight ratio of 15-20:0.2-0.5; the photosensitive monomer is selected from one of vinyl ether acrylate, 1,6-hexanediol diacrylate, and tripropylene glycol diacrylate; The preparation method of the polyurethane modified epoxy acrylate polymer comprises the following steps, measured by weight: S1, adding 35-40 parts of epoxy acrylate UV resin, 20-25 parts of ε-caprolactone and 1-1.5 parts of stannous octoate into a reactor, mixing, heating, and reacting at a constant temperature of 110-120° C. at a stirring speed of 150-300 r / min, measuring the ε-caprolactone content in the reaction liquid system every 1 hour, stopping the reaction when the ε-caprolactone content drops to 0, cooling, discharging and setting aside, and obtaining an epoxy acrylate prepolymer; S2, 35-45 parts of isophorone diisocyanate, 0.1-0.3 parts of dibutyltin dilaurate and 0.01-0.05 parts of p-hydroxyanisole are added to a reactor and mixed, the temperature is raised to 50-60°C for insulation, 20-25 parts of hydroxyethyl acrylate are dripped into the reactor, after the dropwise addition is completed, the reaction is carried out at a constant temperature of 50-60°C at a stirring speed of 150-300r / min, the -NCO group content in the reaction system is measured every 1h, the reaction is stopped when the -NCO group content drops to half of the initial content, the material is discharged for standby use, and an isocyanate-containing prepolymer is obtained; S3, adding 50-60 parts of epoxy acrylate prepolymer, 60-65 parts of isocyanate prepolymer and 0.1-0.2 parts of dibutyltin dilaurate into a reactor, mixing, heating, and reacting at a constant temperature of 65-75° C. at a stirring speed of 150-300 r / min, measuring the -NCO group content in the reaction system every 1 hour, and stopping the reaction when the -NCO group content of the reaction system reaches 0, to obtain a polyurethane-modified epoxy acrylate polymer; The preparation method of the modified epoxy resin comprises the following steps, measured by weight: 4-6 parts of o-cresol epoxy resin and 6-8 parts of diethylene glycol monoethyl ether acetate are added to a reactor and mixed, the mixture is heated, and the mixture is stirred at a constant temperature of 80-90°C for 20-60 minutes at a stirring speed of 150-300 r / min to obtain a mixed solution A; the mixture is cooled to room temperature, 1.5-2.5 parts of 10-undecynoic acid, 0.02-0.05 parts of catalyst 4-dimethylaminopyridine and 0.05-0.1 parts of inhibitor hydroquinone are added to the mixed solution A, the mixture is heated, and the mixture is stirred at a constant temperature of 95-105°C for 2-4 hours at a stirring speed of 150-300 r / min to obtain a mixed solution B; the mixture is cooled to room temperature, 3-4 parts of tetrahydrophthalic anhydride and 0.01-0.03 parts of hydroquinone are added to the mixed solution B, and the mixture is stirred at a constant temperature of 90-100°C for 2-4 hours at a stirring speed of 150-300 r / min to obtain a modified epoxy resin.
2. The method for preparing the etching ink according to claim 1, wherein: The leveling agent is selected from at least one of polyacrylate leveling agents and polymethylsiloxane leveling agents; and the pigment is an organic pigment.
3. The method for preparing the etching ink according to claim 1, wherein: The photoinitiator is prepared by mixing a free radical photoinitiator and a cationic photoinitiator in a weight ratio of 3-5:
1.
4. The method for preparing the etching ink according to claim 3, wherein: The free radical photoinitiator is selected from at least one of (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, 2-isopropylthioxanthone, benzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, and α-hydroxyisopropylbenzophenone; the cationic photoinitiator is selected from at least one of diphenyliodonium hexafluoroarsenate, benzanilide salt, and benzoylphenothiazine salt.
5. An etching ink, characterized in that: The etching ink is prepared by the method for preparing the etching ink according to any one of claims 1 to 4.
6. The use of the etching ink in digital printing for patterned flooring according to claim 5, characterized in that: The etching ink forms the pattern of the monogrammed floor in the form of inkjet printing.
Citation Information
Patent Citations
Inkjet etching ink and preparation method thereof
CN115873447B
UV curable inkjet inks
CN108137975A
Ink-jet printing ink, color film substrate and display panel
CN112980246A