A kind of 15.9 grade non-quenched and tempered cold heading steel wire rod for bolts and its manufacturing method
Through high-carbon composition system and online salt bath phase change control technology, cold heading steel strips with mixed structure of tempered pearlite and tempered bainite are formed, solving the high material cost, complex process and risk of processing cracking in the existing technology. The problem of this problem has achieved efficient green manufacturing of 15.9-level non-temperature bolts, meeting the needs of high strength and high plasticity.
Patent Information
- Application Number
- CN202411133211.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-19
AI Technical Summary
In the production of existing 15.9-level high-strength non-temperature bolts, the material cost is high, the process is complex and the efficiency is low. Cold heading steel strips are difficult to match high strength and high plasticity, and it is easy to cause brittle breakage of coil collection, transportation and unwinding. , and saves the risk of processing cracking after the annealing process.
Cold heading steel strips using high carbon composition system, the chemical compositions include C: 0.87%~0.90%, Si: 0.40%~0.58%, Mn: 0.40%~0.60%, Cr: 0.10%~0.30%, Al: 0.20 %~0.40%, V: 0.010%~0.025%, through online salt bath phase change regulation, form a mixed structure of tempered pearlite and tempered bainite, combined with austenite forming elements, inhibit ferrite precipitation and improve matrix strength and plasticity.
Achieve efficient green manufacturing of 15.9-level non-temperature bolts, simplify the manufacturing process, reduce the risk of processing cracking, achieve tensile strength of 1430~1480MPa, and cross-section shrinkage rate of 40%~45%, suitable for 15.9-level non-temperature The high strength of the mass bolt matches the high plasticity.
Smart Images

Figure CN118653094B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cold heading steel wire rods, and in particular relates to a cold heading steel wire rod for 15.9-grade non-quenched and tempered bolts and a manufacturing method thereof. Background Art
[0002] Fasteners, as the most basic and universal mechanical parts, are widely used in the fields of automobiles, transportation, energy and electricity, mechanical equipment, bridges, construction, etc. In recent years, with the rapid development of strategic emerging industries such as new energy vehicles, the accelerated development of high-strength and high-performance fasteners has become an inevitable trend. Existing high-strength fasteners usually undergo multiple spheroidizing annealing and tempering treatments before the bolt blanks are formed. Spheroidizing annealing is used to improve the cold deformation performance, and tempering treatment is used to improve the comprehensive mechanical properties to achieve the corresponding strength grade. However, the intermediate heat treatment process not only increases the production cost, but also reduces the production efficiency and increases energy consumption. Therefore, controlling the organizational properties of hot-rolled raw materials is an effective way to simplify the fastener production process. However, in order to save the annealing and tempering processes, it also brings greater challenges to the research and development of cold heading steel wire rods.
[0003] At present, there are few reports on 15.9 grade ultra-high strength non-quenched and tempered bolt fasteners and their cold heading steel wire rods. The existing production of 15.9 grade high-strength bolt steel will add high content of hardenability components and micro-alloy components on the basis of medium carbon steel components to improve the matrix strength, but it also brings about the problem of increased material cost and increased risk of abnormal organization precipitation such as martensite and bainite that deteriorates the drawing performance. In order to avoid brittle fracture of coiling, round steel slow cooling will be used for manufacturing, but the subsequent blanking, heat treatment and other processes are more, the efficiency is poor, and it is not conducive to the manufacture of small-size bolts, or low-temperature controlled rolling and controlled cooling and insulation cooling treatment are used, for example:
[0004] Patent CN114107822B discloses a 15.9 grade high-strength bolt steel and its production method and heat treatment method, which adopts a medium C-Si-Mn-Cr-Mo-V-Nb-Ti-Al composition design, combines low-temperature rolling and wire spinning with heat preservation cooling to avoid martensite formation, obtains pearlite + ferrite + bainite structure, and then performs offline treatment through deformation heat treatment and high-frequency tempering heat treatment after coiling to obtain tempered troostite + dispersed precipitated carbides to achieve product mechanical properties, but first, for the purpose of reducing costs, omitting alloy components or reducing alloy dosage will bring obvious strength loss, and it is difficult to achieve the final strength through drawing and cold heading without quenching and tempering process, etc. The low-temperature rolling and wire drawing process intensifies the wear of the rolling line and affects the rolling efficiency. Low-temperature rolling and insulation cooling also affect the strengthening effect of the micro-alloy components. The hot-rolled structure obtained contains a bainite structure with high distortion and dislocation density, and is highly brittle. The wire rod is prone to breakage during coiling in the steel plant, transportation to the downstream, downstream drawing, or unwinding before off-line heat treatment, resulting in waste of raw materials and reduced yield. In addition, it is easy to cause drawing fracture when the annealing process is omitted. Although the wire rod structure is improved by further heat treatment, it also brings problems such as increased procedures, energy consumption and costs for bolt manufacturing, and insufficient production efficiency.
[0005] Carbon is a necessary and relatively economical strengthening element in cold heading steel. Replacing alloying elements in steel is beneficial to reducing material costs. However, the existing high-carbon steel wire rod mainly improves the drawing performance by increasing the sorbite content in the organization. It is used in the fields of bridge cables and cords. However, due to the limitation of the cooling capacity of the Stelmor air-cooled wire after spinning, the dislocation density of the obtained sorbite organization is high, and the final plasticity is not enough to meet the cold heading requirements. The existing high-carbon steel wire rod is difficult to meet the technical difficulties and causes of the manufacturing of 15.9 grade non-quenched and tempered bolts. First, as the carbon content increases, in order to reduce the risk of uncontrollable abnormal organization precipitation during the controlled cooling process after spinning, the wire rod after spinning will be used. Low cooling speed air cooling or insulation cooling process, but it also increases the time that the wire rod stays in the temperature range of secondary cementite precipitation, produces serious network carbides, reduces the utilization value of carbon, destroys the continuity of the organization, deteriorates the mechanical properties, especially the plasticity and toughness of the wire rod, and causes cold heading cracking. Although the network carbon of some wire rods can be improved during the offline salt bath treatment after air cooling, it will also increase the heat treatment process of bolt manufacturing, which is not conducive to non-quenching and tempering high-efficiency production; second, with the increase of carbon content, after adding strengthening elements such as Mn, the activity of C is suppressed, the cementite precipitation becomes coarser, and the difficulty of plasticity improvement is increased. At the same time, low speed or insulation cooling is directly adopted after spinning, and the wire rod During the continuous cooling process, after being inoculated with troostite or pearlite, it is already in a low-temperature state. The large interlamellar spacing of pearlite also increases the difficulty of softening, resulting in a large stress in the final structure, causing the risk of wire breakage during drawing or cracking during cold heading under a non-quenching and tempering process; Third, although some cold heading steel wire rods are used to improve the strength of the wire rods by introducing bainite through rapid cooling after spinning or air cooling after insulation cooling to obtain a mixed structure, the resulting bainite has a high distortion and dislocation density, which can easily cause brittle fracture in subsequent coiling, and offline heat treatment with a loss of yield will increase the process, energy consumption and cost, while high-temperature coiling and subsequent processing after spinning will aggravate the wire rod due to its softness. There is a risk of surface scratches and deterioration of surface quality, which affects the uniform heat transfer on the surface of the wire rod and makes it difficult to quickly control the phase change; Fourth, although some cold heading steel wire rods increase the ferrite content in the organization to improve the plasticity of the wire rod, it will excessively deteriorate the strength of the wire rod. In the process of strengthening the bolts by large surface reduction drawing, the plasticity loss is large, which will increase the risk of cold heading cracking; Fifth, although some cold heading steel wire rods add V elements to improve the strength of the wire rod, in the low-speed or heat-insulating continuous cooling process after spinning, the vanadium-containing carbides do not have time to disperse and precipitate in large quantities, so that the V element cannot be effectively utilized. The amount of V added is too large, which increases the material cost. Summary of the invention
[0006] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a cold heading steel wire rod for 15.9-grade non-quenched and tempered bolts and a manufacturing method thereof. The wire rod structure regulation and high strength and high plasticity matching can be achieved through a high-carbon component system, thereby reducing material costs. The wire rod is suitable for efficient and green manufacturing of 15.9-grade non-quenched and tempered bolts, and the manufacturing process of the wire rod and the bolts can be simplified, the yield rate can be improved, and the risk of processing cracking can be reduced.
[0007] The technical solution adopted by the present invention to solve its technical problem is:
[0008] The invention discloses a 15.9-grade cold heading steel wire rod for non-quenched and tempered bolts. The chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.87%-0.90%, Si: 0.40%-0.58%, Mn: 0.40%-0.60%, Cr: 0.10%-0.30%, Al: 0.20%-0.40%, V: 0.010%-0.025%, P≤0.015%, S≤0.015%, and the rest is Fe and unavoidable impurities. The microstructure of the cold heading steel wire rod includes a mixed structure consisting of tempered pearlite with a volume percentage of ≥60% and tempered bainite with a volume percentage of ≥35%.
[0009] The design basis of the chemical composition and mass percentage of the above-mentioned cold heading steel wire rod includes:
[0010] (1) Carbon: As the most economical and effective element for solid solution strengthening and precipitation strengthening, C is the main added element in the present invention to ensure the matrix strength and high hardenability of steel. As an austenite-forming element, it can expand the austenite phase region and inhibit the formation of ferrite, but at the same time increases the decarburization sensitivity and the risk of cementite being distributed in a network along the grain boundary. If the C content is too high, the cementite will precipitate and become coarser, which will increase the difficulty of tempering softening and be unfavorable for the control of the matrix structure. Therefore, in order to ensure the cold deformation performance of the cold heading steel wire rod and meet the final performance level requirements of the 15.9 grade bolt, the mass percentage of C is controlled to be 0.87%~0.90%.
[0011] (2) Silicon: Si is the main deoxidizing element in steel. It can dissolve in austenite to increase the strength of steel. It can inhibit grain coarsening and cementite precipitation in the early stage of online salt bath phase transformation control, which is beneficial to pearlite nucleation, making cementite thinner and beneficial to tempering softening. However, excessive silicon will increase non-metallic inclusions and impurity element segregation, which is not conducive to cold heading and cold extrusion, and is not conducive to inhibiting ferrite precipitation during pearlite phase transformation control. Therefore, the mass percentage of Si is controlled to be 0.40%~0.58%.
[0012] (3) Manganese: Mn is often added to steel as a deoxidizer during the smelting process. As an austenite-forming element, it can expand the austenite phase and inhibit the formation of ferrite. As a solid solution strengthening element, it can improve the strength and hardenability of steel. However, too high Mn content will aggravate the segregation during the solidification process of the steel billet, reduce the activity of carbon and the diffusion rate of carbon, increase the difficulty of tempering softening, and cause deformation resistance. Too high Mn content will also increase material costs. Therefore, the mass percentage of Mn is controlled to be 0.40%~0.60%.
[0013] (4) Chromium: As a solid solution strengthening element, Cr can greatly improve the hardenability of the material and regulate the matrix phase composition. It is beneficial to control the formation of pearlite and bainite structures in the online salt bath phase transformation. After the online salt bath phase transformation, fine dispersed carbide particles are precipitated to improve the strength of the material. However, if the Cr content is too high, it will increase the temper brittleness tendency and low-temperature structure risk of the steel, and increase the difficulty of improving plasticity. The precipitation and coarsening of Cr will also significantly deteriorate the strength and plasticity of the wire rod. Therefore, the mass percentage of Cr is controlled to be 0.10%~0.30%.
[0014] (5) Aluminum: Al acts as a deoxidizer during the smelting process and forms fine precipitates during hot rolling, which helps to inhibit the coarsening of cementite, thereby facilitating tempering softening and improving the impact toughness of steel. Mo, which can inhibit the coarsening of cementite, has a lower cost. However, excessive Al content will promote graphitization of steel and increase the risk of decarburization. Therefore, the mass percentage of Al is controlled to be 0.20%~0.40%.
[0015] (6) Alum: As a microalloying element, V can be precipitated in large quantities in the tempering isothermal zone, greatly improving the strength and delayed fracture resistance of the wire rod. However, the cost of V is relatively high. Excessive addition is not conducive to controlling the cost of cold heading steel wire rod and has the risk of coarsening. Based on the role of V and cost considerations, the present invention controls the V content to 0.010% to 0.025%.
[0016] (7) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.
[0017] The above-mentioned cold heading steel wire rod adopts a high C-Si-Mn-Cr-Al-V composition design, and carbon is used to replace the addition of alloy components such as Ni, Nb, B, and Mo. The amount of Si, Mn, Cr, and V is less than that of the existing 15.9 grade cold heading steel raw materials, which can effectively reduce the material cost. The microstructure includes most of the tempered pearlite and a small part of the tempered bainite. The pearlite structure has a larger interlamellar spacing than the troostite, better plasticity than the troostite, and better strength than the pearlite. After the pearlite is tempered and the carbides therein are transformed into spheroidized structure to form tempered pearlite, the tempered pearlite can retain the characteristics of moderate strength and plasticity of the pearlite, further reduce stress concentration and dislocation density, so that the plastic toughness can be further improved. Compared with the troostite, the bainite has higher distortion, higher strength, and plasticity. After the bainite is tempered to form tempered bainite, the dislocation density is significantly reduced, so that the tempered bainite can retain the bainite. The cold heading steel wire rod has the characteristics of high strength and significantly improves brittleness, obtaining a strong and tough organizational state. Therefore, compared with the existing wire rod organization composed of pearlite and ferrite soft phases, the cold heading steel wire rod can use tempered pearlite and tempered bainite, cooperate with austenite forming elements C and Mn to expand the austenite phase region, inhibit ferrite precipitation, and provide matrix strength with solid solution and precipitation strengthening of C, Mn, Cr, and V, to make up for the strength loss caused by reducing alloy dosage and eliminating alloy components. Compared with the existing wire rod mixed organization of high troostite content + ferrite, or pearlite + bainite, the cold heading steel wire rod is regulated by tempering state organization, so that the organizational stress and dislocation density are effectively improved, without martensitic abnormal organization, and can take into account the plastic and toughness properties of the wire rod on the basis of high strength of the wire rod, and can effectively avoid brittle fracture during coiling, transportation and uncoiling, and improve the yield rate, which is beneficial to the efficient manufacture of 15.9 grade bolts without annealing and tempering processes.
[0018] The higher the interlamellar spacing of tempered pearlite, the lower the strength of the cold heading steel wire rod and the higher the plasticity. On the contrary, the lower the interlamellar spacing of tempered pearlite, the higher the strength of the cold heading steel wire rod and the lower the plasticity. In a preferred embodiment, the interlamellar spacing of tempered pearlite is 155-210 nm.
[0019] In a preferred embodiment, the network carbide of the cold heading steel wire rod is level 0, which can suppress the influence of network carbon deterioration phase and improve the use value of carbon element.
[0020] In a preferred embodiment, the diameter of the cold heading steel wire rod is 12.0~28.0mm, the tensile strength is 1430~1480MPa, and the cross-sectional reduction rate is 40%~45%. Compared with round steel manufacturing, cold heading steel wire rods with smaller diameters can be directly obtained, reducing the difficulty of manufacturing small-specification bolts. The cold heading steel wire rod has both high tensile strength and cross-sectional reduction rate. The high-strength and plastic matching makes it unnecessary to perform offline heat treatment before drawing the cold heading steel wire rod. 15.9 grade bolts can be manufactured by drawing, cold heading and simple aging treatment without annealing and tempering processes.
[0021] A method for manufacturing a 15.9 grade non-quenched and tempered cold heading steel wire rod for bolts, the manufacturing method comprising:
[0022] The wire rod is produced by rolling the chemical composition of the 15.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to any of the above items. After the wire rod is spun into a wire rod at a spinning temperature of ≥910°C, an online salt bath phase transformation control is performed, so that the wire rod first passes through a first section of molten salt, and the wire rod is cooled to the pearlite phase region at a cooling rate of ≥35°C / s for isothermal phase transformation, which promotes the transformation of part of the austenite in the wire rod into the pearlite structure. The wire rod is then cooled and isothermally cooled by a second section of molten salt to promote the transformation of the untransformed austenite in the wire rod into the bainite structure, and at the same time, the wire rod is tempered and softened, and the vanadium-containing carbide is dispersed and precipitated. Finally, it is slowly cooled through a roller to produce a cold heading steel wire rod with a mixed structure consisting of tempered pearlite with a volume percentage of ≥60% and tempered bainite with a volume percentage of ≥35%.
[0023] The above manufacturing method uses a higher spinning temperature. On the one hand, it can avoid the high carbon content causing the wire rod to precipitate secondary cementite during the spinning stage and aggravate the risk of network carburization. On the other hand, it can form a finer pearlite structure in the subsequent online salt bath phase transformation regulation, thereby facilitating the preparation for tempering and softening. After the wire rod is spun, it is directly subjected to online salt bath phase transformation regulation. After the wire rod passes through the first stage of molten salt, it can be quickly cooled from the austenitizing temperature of high-temperature spinning. On the one hand, compared with the low cooling rate air cooling after spinning, excessive carbon elements will cause the wire rod to form a network carbide deterioration phase during the cooling process. Directly using the first stage of molten salt can make the wire rod super-fast skip the precipitation of secondary cementite. On the other hand, compared with high-intensity air cooling after spinning, the high heat exchange capacity of molten salt can be utilized, which not only has a higher cooling rate and can avoid network carbon, but also because the molten salt can be wrapped on the surface of the wire rod when it passes through the molten salt, there is no temperature difference of the wire rod caused by the wind volume difference between the windward side and the leeward side of the strong wind cooling, which can avoid the precipitation of a large amount of uncontrollable bainite or even martensite hard and brittle phases in the wire rod, so that the wire rod can be directly lowered to the pearlite phase region for isothermal phase transformation, and the austenite phase region can be expanded by combining C and Mn, which inhibits the precipitation of ferrite and promotes the partial transformation of the high-temperature austenite structure in the wire rod structure into pearlite structure, thus preparing for the subsequent organization regulation.
[0024] The wire rod after the first stage of molten salt is then subjected to the second stage of molten salt cooling isothermal treatment. First, compared with increasing the air cooling rate after spinning, or obtaining a structure mixed with bainite during the air cooling process after low cooling rate cooling, on the one hand, since the pearlite phase transformation has been regulated, the second stage of molten salt uses a lower molten salt temperature, which can promote the transformation of the untransformed high-temperature austenite in the wire rod into a bainite structure, making the bainite formation controllable and providing appropriate matrix strength. On the other hand, compared with the continuous cooling process such as heat preservation after spinning, since the wire rod is already in a low temperature state during the continuous cooling process, the manufacturing method adopts a two-stage molten salt treatment such as a gradient cooling control method. After the wire rod is inoculated with bainite, since the wire rod can be kept consistent with the molten salt temperature for a longer period of high-temperature isothermal treatment, Si and Al are used to inhibit the coarsening of cementite and reduce the difficulty of tempering, so the pearlite in the wire rod structure can be transformed into the tempered pearlite structure, and the bainite reduces the dislocation density and transforms into the tempered structure for tempering softening; second, compared with the wire rod after spinning During the continuous cooling process after the wire, the vanadium-containing carbides do not have time to disperse and precipitate in large quantities. The wire rod is cooled to the temperature of the second molten salt. Under the action of the tempering isothermal zone where V precipitates for a long time, the driving force is greater, and a large number of fine phase precipitations can be formed, thereby improving the dispersion strengthening utilization value of V and effectively improving the strength and hydrogen embrittlement resistance of the material. Third, compared with the salt bath control method of first cooling and then heating, the gradient cooling control method of the manufacturing method, on the one hand, can make the wire rod at a relatively low temperature when passing through the second molten salt, avoiding the precipitation coarsening of Cr and V and the excessive softening of the structure and loss of strength. On the other hand, the gradient cooling makes it easier to control the temperature rise of the molten salt in the first stage, and the second stage molten salt does not need to be overheated, and the heating demand for the molten salt is smaller, which is beneficial to reducing production energy consumption. Finally, after slow cooling on the roller, the high temperature state of the wire rod passing through the molten salt can be used to reduce the cooling rate to promote further softening of the wire rod, and finally the wire rod structure control and strength-plasticity matching can be achieved, and direct drawing and cold heading can be performed without offline heat treatment.
[0025] A higher heating temperature is selected to promote the rapid high-temperature diffusion and homogenization of the chemical composition of the steel billet to avoid the risk of burning and decarburization caused by too long time in the furnace. In a preferred embodiment, before rolling, the heating furnace is controlled to have a soaking temperature of 1080-1150°C and a furnace time of 2.5-4h.
[0026] Due to the high wire laying temperature, the limitation of low temperature wire laying on low temperature rolling can be broken, and rolling can be started with a higher initial rolling temperature to improve the rolling speed and efficiency. A higher heavy-duty finishing rolling temperature is selected to reduce the deformation resistance of the steel billet and the wear on the rolling mill. With a larger finishing rolling reduction, the hot-rolled wire grains are refined and the matrix is strengthened and toughened. In a preferred embodiment, during the rolling, the initial rolling temperature is controlled to be 1060-1120°C, the heavy-duty finishing rolling temperature is ≥940°C, and the finishing rolling reduction is 5%-15%.
[0027] After finish rolling, a higher heavy-load sizing temperature is selected to reduce the deformation resistance of the wire, and a larger sizing reduction is used to avoid grain growth and control the dimensional accuracy of the wire. In a preferred embodiment, during the rolling, the heavy-load sizing temperature is ≥930°C, and the sizing reduction is 2%~5%.
[0028] In a preferred embodiment, the molten salt temperature of the first stage molten salt is 555-580°C, and the processing time is 30-50s. The higher the molten salt temperature of the first stage molten salt and the longer the processing time, the more pearlite structure is formed, the subsequent tempered bainite structure is reduced, the plasticity of the wire rod increases, and the strength decreases. However, if the molten salt temperature is too high, the spacing between pearlite lamellae is large, which is not conducive to subsequent cooling and tempering, and there is even a risk of ferrite precipitation. If the processing time is too long, the pearlite phase transformation is too much, and the matrix strength decreases. On the contrary, the lower the molten salt temperature of the first stage molten salt and the shorter the processing time, the less pearlite structure is formed, which will lead to an increase in the proportion of tempered bainite structure, an increase in the strength of the wire rod and a decrease in plasticity. However, if the molten salt temperature is too low, the spacing between the pearlite lamellae formed becomes finer, and the processing time is too short, the proportion of tempered pearlite structure decreases, which is not conducive to the plasticity of the matrix. Therefore, the molten salt temperature and processing time of the first stage molten salt can be controlled to control the formation of pearlite structure in the matrix structure of the wire rod to prepare for the subsequent cooling and isothermal.
[0029] Since the wire rod is quickly cooled from a relatively high spinning temperature to the pearlite phase region, and the gradient cooling regulated by the online salt bath phase transformation makes it easier to control the temperature rise of the molten salt in the first stage of molten salt, it is unnecessary to use an excessively large molten salt circulation amount to increase energy consumption. Properly increasing the molten salt circulation amount can reduce the temperature rise of the molten salt and control the temperature accuracy of the pearlite phase transformation. In a preferred embodiment, the molten salt circulation amount of the first stage of molten salt is 400-600t / h, and the temperature rise of the molten salt is ≤10°C.
[0030] In a preferred embodiment, the molten salt temperature of the second stage molten salt is 450-500°C, and the processing time is 100-300s. The higher the molten salt temperature of the second stage molten salt, the more unfavorable it is for the transformation of the untransformed structure in the wire rod to the bainite structure, the precipitation driving force of the vanadium-containing carbide is reduced, which is not conducive to the formation of fine precipitation phases, and the strength of the wire rod is reduced. If the molten salt temperature is too high, the proportion of tempered bainite decreases, which is not conducive to improving the strength of the wire rod. On the contrary, the lower the molten salt temperature, the more favorable it is for the rapid formation of bainite structure. However, if the molten salt temperature is too low, it is difficult to form pearlite and bainite. The bainite softening provides thermal power, which is not conducive to the softening of the organization and even has the risk of abnormal martensite organization, which is not conducive to the plasticity regulation of the wire rod; the longer the treatment time, the better the tempering softening effect of the matrix organization, but if the treatment time is too long, there is a risk of precipitation and coarsening of Cr and V, which is not conducive to both strength and plasticity. On the contrary, the shorter the treatment time, the bainite formed is in a quenched state, the matrix is more brittle, and fails to soften, which is not conducive to the plasticity of the wire rod. Therefore, the molten salt temperature and treatment time of the second stage molten salt can be further controlled to control the proportion of tempered bainite and the tempering softening effect.
[0031] In a preferred embodiment, the molten salt circulation rate of the second stage molten salt is 300-400 t / h, and the molten salt temperature rise is ≤7°C. Selecting an appropriate molten salt circulation rate can control the molten salt temperature rise of the second stage molten salt, and control the bainite transformation and isothermal tempering treatment accuracy.
[0032] Controlling the wire rod to cool at a low speed in the early stage of roller slow cooling can continue the high-temperature tempering effect of the wire rod out of the second stage molten salt. After the softening effect weakens, the cooling speed of the wire rod can be increased to reduce the online time of the wire rod, quickly reach the coiling position, and improve manufacturing efficiency. In a preferred embodiment, the roller slow cooling first controls the wire rod to cool at a cooling speed of 0.1~0.45℃ / s for 50~200s, and then controls the wire rod to cool to the coiling at a cooling speed of 0.75~1.5℃ / s.
[0033] In a preferred embodiment, during the coiling, the coiling temperature of the wire rod is 300°C or below, which can maintain the appropriate hardness of the wire rod during coiling, avoid excessively high coiling temperature and soft wire rods that may cause easy surface scratches, thereby improving the surface quality of the wire rod.
[0034] Compared with the prior art, the beneficial effects of the present invention are at least:
[0035] (1) In view of the fact that 15.9 grade high-strength fasteners need to undergo multiple spheroidizing annealing and tempering treatments before the bolt blank is formed to reach the corresponding strength grade, resulting in high production cost, low production efficiency and increased energy consumption, the cold heading steel wire rod of the present invention adopts a high C-Si-Mn-Al-Cr-V composition design, and the microstructure type is a mixed structure composed of tempered pearlite and tempered bainite, and is combined with austenite forming elements to inhibit ferrite precipitation, and provides matrix strength by solid solution and precipitation strengthening of C, Mn, Cr and V, thereby reducing the amount of alloy and saving energy. It eliminates the strength loss caused by the alloy composition, effectively reduces the material cost, has no abnormal martensitic structure, and regulates the tempered state structure to compensate for the adverse effects of high carbon and bainite brittleness on the plasticity of the wire rod. It can effectively avoid brittle fracture during coiling, transportation and uncoiling, improve the yield rate, and achieve high strength and high plasticity matching of the wire rod, achieving a tensile strength of 1430~1480MPa and a cross-sectional shrinkage rate of 40%~45%. It is suitable for the efficient and green manufacturing of 15.9 grade non-quenched and tempered bolts, can simplify the manufacturing of bolts, reduce the risk of processing cracking, and has good market application prospects.
[0036] (2) In view of the current situation that the existing cold heading steel wire rod manufacturing is difficult to meet the application of 15.9 grade non-quenched and tempered bolts, has many processes and high costs, the manufacturing method of the present invention adopts a high C-Si-Mn-Al-Cr-V composition design and combines the online salt bath phase transformation control technology process design. The wire rod is directly subjected to online salt bath phase transformation control after spinning. It first passes through the second stage of molten salt, which can quickly cool down and inhibit the influence of the carbon deterioration phase, thereby improving the use value of the carbon element, and allowing the wire rod to directly drop to the pearlite phase region for isothermal phase transformation, thereby inhibiting the precipitation of ferrite and promoting the partial transformation of the high-temperature austenite structure in the wire rod structure. It is transformed into pearlite structure, and then undergoes the second stage of molten salt cooling isothermal treatment to make the bainite formation controllable. Si and Al are combined to inhibit the coarsening of cementite, reduce the difficulty of tempering, and promote the transformation of untransformed austenite in the wire rod into bainite structure. At the same time, the wire rod is tempered and softened, and the vanadium-containing carbides are dispersed and precipitated, thereby improving the dispersion strengthening utilization value of V, effectively improving the strength and hydrogen embrittlement resistance of the material, and finally through roller slow cooling, the wire rod structure regulation and strength-plasticity matching are finally achieved. It can be directly drawn and cold headed without offline heat treatment, which can simplify the cold heading steel wire rod manufacturing process and has good industrial adaptability.
[0037] (3) The manufacturing method of the present invention uses a relatively high heating temperature, which can break the limitation of low-temperature spinning on low-temperature rolling and achieve rapid rolling. The second stage molten salt is used to have a lower molten salt temperature than the first stage molten salt for gradient cooling, which can reduce the difficulty of controlling the temperature rise of the first stage molten salt and the heating demand for the second stage molten salt, and is beneficial to reducing production energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0039] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;
[0040] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;
[0041] Figure 3 It is the metallographic structure diagram of Example 3 of the present invention. DETAILED DESCRIPTION
[0042] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention. They should not be construed as limiting the scope of the present invention, which is limited only by the appended claims. Embodiment 1:
[0043] A preferred embodiment of the manufacturing method of the 15.9 grade non-quenched and tempered bolt cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.87%, Si: 0.48%, Mn: 0.57%, Cr: 0.23%, Al: 0.28%, V: 0.025%, P: 0.01%, S: 0.014%, and the rest is Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of rolling → spinning → online salt bath phase change regulation → roller slow cooling → coiling, specifically:
[0044] The rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the steel billet composition and reduce the decarburization tendency of the steel billet. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 22mm through a rolling line. A higher rolling temperature is selected to reduce the wear of the steel billet on the rolling line and improve the rolling efficiency. A larger reduction is used to appropriately refine the grains. Specifically: the heating furnace is heated and heated in the preheating section, the heating section, and the soaking section in sequence, and the control The heating furnace has a uniform heating temperature of 1120°C, a furnace time of 3.5h, an initial rolling temperature of 1100°C, a heavy-load finishing rolling temperature of 950°C, a finishing rolling reduction of 8%, a heavy-load sizing temperature of 940°C, and a sizing reduction of 3%. The wire-spinning process is used to convert the wire rods exiting the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers to avoid the risk of cementite precipitation caused by excessively low temperatures in the wire-spinning stage of high carbon steel, and to prepare the organization for pearlite nucleation. Specifically, the wire-spinning temperature is controlled to be 920°C.
[0045] The online salt bath phase change control adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath tank, and is quickly cooled to the molten salt temperature of the first molten salt, so that the wire rod is cooled at a cooling rate of 38°C / s to eliminate the carbon deterioration phase caused by excessive carbon elements, and is cooled to the pearlite phase region for isothermal phase change, which promotes the transformation of part of the austenite in the wire rod into the pearlite structure. The wire rod that has passed through the first molten salt is then conveyed by a roller to pass through the second salt bath tank, and is quickly cooled to the second The molten salt temperature of the first section molten salt is 555°C, the processing time is 50s, the molten salt circulation volume is 600t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the second section molten salt is 500°C, the processing time is 250s, the molten salt circulation volume is 300t / h, and the molten salt temperature rise is ≤7°C.
[0046] The roller slow cooling process adopts closing the insulation cover, and conveying the wire rod coming out of the second salt bath tank into the insulation cover by rollers for slow cooling treatment to promote further softening of the wire rod structure. Specifically, the wire rod is first controlled to be slowly cooled at a cooling rate of 0.45°C / s for 50s, and then the wire rod is controlled to be cooled to coil at a cooling rate of 1.5°C / s; the coiling process is used to coil the wire rod into coils through a coiling drum, and the coiling temperature of the wire rod is 285°C. After packaging and storage, a high-carbon hot-rolled wire rod product is obtained, and its metallographic structure diagram is as follows Figure 1 shown.
[0047] Comparative Example 1:
[0048] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to the process flow of rolling → spinning → Stelmor insulation and slow cooling, specifically: controlling the heating furnace soaking temperature to 1070°C, the furnace time to 4h, the initial rolling temperature to 1050°C, the heavy-load finishing temperature to 925°C, the heavy-load sizing temperature to 915°C, the spinning temperature to 895°C, the Stelmor insulation and slow cooling adopts the method of shutting down all fans and insulation covers, conveying the wire rod with rollers, and the wire rod completes phase change in the cover at a cooling rate of 1.2°C / s, and the finished wire rod is obtained after it comes off the line.
[0049] Comparative Example 2:
[0050] A method for manufacturing a wire rod, which differs from that of Example 1 in that the method is manufactured according to a process flow of rolling → spinning → air cooling → insulation and slow cooling, specifically: controlling the heating furnace soaking temperature to 1020°C, the furnace time to 4.5h, the initial rolling temperature to 1000°C, the heavy-load finishing temperature to 880°C, the heavy-load sizing temperature to 865°C, the spinning temperature to 840°C, the air cooling adopts opening the insulation cover to cool the wire rod to 675°C at a cooling rate of 2.3°C / s, the insulation and slow cooling adopts closing all fans and the insulation cover to complete the phase change of the wire rod in the cover at a cooling rate of 0.85°C / s, and the finished wire rod is obtained after it comes off the line.
[0051] Comparative Example 3:
[0052] A method for manufacturing a wire rod, which differs from that of Example 1 in that the method is manufactured according to a process flow of rolling → spinning → Stelmor rapid cooling → roller slow cooling, specifically: controlling the heating furnace soaking temperature to 1025°C, the furnace time to 4.5h, the initial rolling temperature to 1010°C, the heavy-load finishing temperature to 885°C, the heavy-load sizing temperature to 870°C, the spinning temperature to 850°C, the Stelmor rapid cooling adopts opening 1~7# fans at 35%, so that the wire rod is cooled to 668°C at a cooling rate of 3.9°C / s, the roller slow cooling adopts closing all fans and insulation covers, so that the wire rod completes phase change in the cover at a cooling rate of 1.1°C / s, and the finished wire rod is obtained after going offline. Embodiment 2:
[0053] A preferred embodiment of the manufacturing method of the 15.9 grade non-quenched and tempered bolt cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.9%, Si: 0.4%, Mn: 0.4%, Cr: 0.3%, Al: 0.37%, V: 0.01%, P: 0.014%, S: 0.012%, and the rest is Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of rolling → spinning → online salt bath phase change regulation → roller slow cooling → coiling, specifically:
[0054] The rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the steel billet composition and reduce the decarburization tendency of the steel billet. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 18mm through a rolling line. A higher rolling temperature is selected to reduce the wear of the steel billet on the rolling line and improve the rolling efficiency. A larger reduction is used to appropriately refine the grains. Specifically: the heating furnace is heated and heated in the preheating section, the heating section, and the soaking section in sequence, and the control The heating furnace has a uniform heating temperature of 1100°C, a furnace time of 3h, an initial rolling temperature of 1080°C, a heavy-load finishing rolling temperature of 945°C, a finishing rolling reduction of 12%, a heavy-load sizing temperature of 935°C, and a sizing reduction of 4%; the wire-spinning process is used to make the wire rods exiting the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers to avoid the risk of cementite precipitation caused by excessively low temperature of high carbon steel in the wire-spinning stage, and to make organizational preparations for pearlite nucleation. Specifically, the wire-spinning temperature is controlled to be 915°C.
[0055] The online salt bath phase change control adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath tank, and is quickly cooled to the molten salt temperature of the first molten salt, so that the wire rod is cooled at a cooling rate of 37°C / s to eliminate the carbon deterioration phase caused by excessive carbon elements, and is cooled to the pearlite phase region for isothermal phase change, which promotes the transformation of part of the austenite in the wire rod into the pearlite structure. The wire rod that has passed through the first molten salt is then conveyed by a roller to pass through the second salt bath tank, and is quickly cooled to the second The molten salt temperature of the first section molten salt is 560°C, the processing time is 45s, the molten salt circulation volume is 550t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the second section molten salt is 480°C, the processing time is 100s, the molten salt circulation volume is 320t / h, and the molten salt temperature rise is ≤7°C.
[0056] The roller slow cooling process adopts closing the insulation cover, and conveying the wire rod coming out of the second salt bath tank into the insulation cover by rollers for slow cooling treatment to promote further softening of the wire rod structure. Specifically, the wire rod is first controlled to be slowly cooled at a cooling rate of 0.1°C / s for 200s, and then the wire rod is controlled to be cooled to coil at a cooling rate of 1°C / s; the coiling process is used to coil the wire rod into coils through a coiling drum, and the coiling temperature of the wire rod is 282°C. After packaging and storage, a high-carbon hot-rolled wire rod product is obtained, and its metallographic structure diagram is as follows Figure 2 shown.
[0057] Comparative Example 4:
[0058] A method for manufacturing a wire rod, which differs from that of Example 2 in that the heating furnace soaking temperature is controlled to be 1040°C, the furnace time is 4h, the initial rolling temperature is 1020°C, the heavy-load finishing temperature is 910°C, the heavy-load sizing temperature is 900°C, the spinning temperature is 880°C, the wire rod passes through a first section of molten salt and is cooled at a cooling rate of 30°C / s, and a finished wire rod is obtained after it comes off the line.
[0059] Comparative Example 5:
[0060] A method for manufacturing wire rod, which differs from Example 2 in that the wire rod passes through a first section of molten salt and is cooled at a cooling rate of 30°C / s, the molten salt temperature of the first section of molten salt is 596°C, the processing time is 55s, and the finished wire rod is obtained after going offline.
[0061] Comparative Example 6:
[0062] A method for manufacturing wire rod, which differs from Example 2 in that the wire rod passes through a first section of molten salt and is cooled at a cooling rate of 40°C / s, the molten salt temperature of the first section of molten salt is 530°C, the processing time is 20s, and the finished wire rod is obtained after going offline. Embodiment 3:
[0063] A preferred embodiment of the manufacturing method of the 15.9 grade non-quenched and tempered bolt cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.88%, Si: 0.58%, Mn: 0.45%, Cr: 0.19%, Al: 0.2%, V: 0.023%, P: 0.014%, S: 0.015%, and the rest is Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of rolling → spinning → online salt bath phase change regulation → roller slow cooling → coiling, specifically:
[0064] The rolling process is used to heat a steel billet with a specification of 220 mm × 220 mm through a heating furnace to promote the homogenization of the steel billet composition and reduce the decarburization tendency of the steel billet. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 12 mm through a rolling line. A higher rolling temperature is selected to reduce the wear of the steel billet on the rolling line and improve the rolling efficiency. A larger reduction is used to appropriately refine the grains. Specifically: the heating furnace is heated and heated in the preheating section, the heating section, and the soaking section in sequence, and the control The heating furnace has an average heating temperature of 1080°C, a furnace time of 2.5h, an initial rolling temperature of 1060°C, a heavy-load finishing rolling temperature of 940°C, a finishing rolling reduction of 15%, a heavy-load sizing temperature of 930°C, and a sizing reduction of 5%. The wire-spinning process is used to convert the wire rods exiting the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers to avoid the risk of cementite precipitation caused by excessively low temperatures in the wire-spinning stage of high carbon steel, and to prepare the organization for pearlite nucleation. Specifically, the wire-spinning temperature is controlled to be 910°C.
[0065] The online salt bath phase change control adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath tank, and is quickly cooled to the molten salt temperature of the first molten salt, so that the wire rod is cooled at a cooling rate of 35°C / s to eliminate the carbon deterioration phase caused by excessive carbon elements, and is cooled to the pearlite phase region for isothermal phase transformation, which promotes the transformation of part of the austenite in the wire rod into the pearlite structure. The wire rod that has passed through the first molten salt is then conveyed by a roller to pass through the second salt bath tank, and is quickly cooled to the second The molten salt temperature of the first section of molten salt is 572°C, the processing time is 40s, the molten salt circulation volume is 400t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the second section of molten salt is 466°C, the processing time is 200s, the molten salt circulation volume is 360t / h, and the molten salt temperature rise is ≤7°C.
[0066] The roller slow cooling process adopts closing the insulation cover, and conveying the wire rod coming out of the second salt bath tank into the insulation cover by rollers for slow cooling treatment to promote further softening of the wire rod structure. Specifically: firstly, the wire rod is controlled to be slowly cooled at a cooling rate of 0.35°C / s for 100s, and then the wire rod is controlled to be cooled to coil at a cooling rate of 1.2°C / s; the coiling process is used to coil the wire rod into coils through the coiling drum, and the coiling temperature of the wire rod is 280°C. After packaging and storage, the high carbon hot rolled wire rod product is obtained, and its metallographic structure diagram is as follows Figure 3 shown.
[0067] Comparative Example 7:
[0068] A method for manufacturing wire rod, which differs from Example 3 in that the online salt bath phase change control adopts a salt bath tank with molten salt inside, and the wire rod after spinning is conveyed by a roller through the salt bath tank, so that the wire rod is cooled at a cooling rate of 40°C / s, the molten salt temperature is 525°C, the processing time is 240s, the molten salt circulation volume is 400t / h, and the finished wire rod is obtained after going offline.
[0069] Comparative Example 8:
[0070] A method for manufacturing wire rod, which differs from Example 3 in that the molten salt temperature of the second stage molten salt is 430°C, the processing time is 90s, the molten salt circulation rate is 440t / h, and the finished wire rod is obtained after going offline.
[0071] Comparative Example 9:
[0072] A method for manufacturing a wire rod, the manufacturing method of which is different from that of Example 3 in that the processing time of the second stage molten salt is 350s, and a finished wire rod is obtained after the wire rod is off the line. Embodiment 4:
[0073] A preferred embodiment of the manufacturing method of the 15.9 grade non-quenched and tempered bolt cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.87%, Si: 0.55%, Mn: 0.6%, Cr: 0.1%, Al: 0.4%, V: 0.017%, P: 0.01%, S: 0.014%, and the rest are Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of rolling → spinning → online salt bath phase change regulation → roller slow cooling → coiling, specifically:
[0074] The rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the steel billet composition and reduce the decarburization tendency of the steel billet. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 28mm through a rolling line. A higher rolling temperature is selected to reduce the wear of the steel billet on the rolling line and improve the rolling efficiency. A larger reduction is used to appropriately refine the grains. Specifically: the heating furnace is heated and heated in the preheating section, the heating section, and the soaking section in sequence, and the control The heating furnace has an average heating temperature of 1150°C, a furnace time of 4h, an initial rolling temperature of 1120°C, a heavy-load finishing rolling temperature of 955°C, a finishing rolling reduction of 5%, a heavy-load sizing temperature of 945°C, and a sizing reduction of 2%; the wire-spinning process is used to convert the wire rods exiting the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers to avoid the risk of cementite precipitation caused by excessively low temperature of high carbon steel in the wire-spinning stage, and to make organizational preparations for pearlite nucleation. Specifically, the wire-spinning temperature is controlled to be 925°C.
[0075] The online salt bath phase change control adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath tank, and is quickly cooled to the molten salt temperature of the first molten salt, so that the wire rod is cooled at a cooling rate of 36°C / s to eliminate the carbon deterioration phase caused by excessive carbon elements, and is cooled to the pearlite phase region for isothermal phase change, which promotes the transformation of part of the austenite in the wire rod into the pearlite structure. The wire rod that has passed through the first molten salt is then conveyed by a roller to pass through the second salt bath tank, and is quickly cooled to the second The molten salt temperature of the first section of molten salt is 580°C, the processing time is 30s, the molten salt circulation volume is 450t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the second section of molten salt is 450°C, the processing time is 300s, the molten salt circulation volume is 400t / h, and the molten salt temperature rise is ≤7°C.
[0076] The roller slow cooling process adopts closing the insulation cover, and conveying the wire rod coming out of the second salt bath tank into the insulation cover by rollers for slow cooling treatment to promote further softening of the wire rod structure. Specifically: first control the wire rod to be slowly cooled at a cooling rate of 0.25°C / s for 150s, and then control the wire rod to be cooled to coil at a cooling rate of 0.75°C / s; the coiling process is used to coil the wire rod into coils through a coiling drum, the coiling temperature of the wire rod is 300°C, and the high carbon hot rolled wire rod finished product is obtained after packaging and storage.
[0077] Comparative Example 10:
[0078] A method for manufacturing a wire rod, which differs from that of Example 4 in that the method is manufactured according to a process flow of rolling → spinning → online salt bath phase change control → air cooling. Specifically, the air cooling process comprises opening a heat preservation cover, conveying the wire rod coming out of a second salt bath tank by a roller, controlling the wire rod to be cooled to 300°C at a cooling rate of 2°C / s, and obtaining a finished wire rod after it comes off the line.
[0079] The wire rods obtained in the above-mentioned Examples 1 to 4 and Comparative Examples 1 to 10 were subjected to organization and performance testing: the tensile test was conducted according to GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:
[0080] Table 1. Comparison of wire rod structure and properties by different manufacturing methods
[0081]
[0082] From the comparison results of Example 1 and Comparative Example 1, it can be seen that compared with obtaining troostite + ferrite structure by lowering the spinning temperature and then cooling with insulation, serious network carbides are produced, the utilization value of carbon is reduced, and the plasticity and toughness of the wire rod are deteriorated. The present invention adopts a high C-Si-Mn-Al-Cr-V component design and combines the online salt bath phase change control technology process design, which can quickly cool down and inhibit the influence of network carbon deterioration phase. The microstructure is mixed with a small amount of tempered bainite, which can make up for the strength loss caused by reducing the alloy dosage and eliminating the alloy component; from the comparison results of Example 1 and Comparative Example 2, it can be seen that compared with further lowering the spinning temperature and then combining air cooling + insulation cooling, serious network carbides are still produced. Increasing the ferrite content in the structure to control the structure will excessively deteriorate the strength of the wire rod. The larger lamellar spacing of pearlite also increases the difficulty of softening, making the final structure stress larger. The present invention cooperates with austenite forming elements The ferrite is inhibited by the element, and the cementite is coarsened by Si and Al, which reduces the difficulty of tempering. The tempered pearlite can retain the characteristics of moderate strength and plasticity of pearlite and further reduce stress concentration and dislocation density. It can be seen from the comparison results of Example 1 and Comparative Example 3 that compared with the mixed structure obtained by introducing bainite by increasing the cooling rate after silk-spinning after low-temperature rolling, the obtained bainite has higher distortion and dislocation density, which is easy to cause subsequent brittle fracture of coiling. The bainite formation of the present invention is more controllable, and at the same time, the wire rod is tempered and softened, and the vanadium-containing carbide is dispersed and precipitated, thereby improving the dispersion strengthening utilization value of V and effectively improving the strength and hydrogen embrittlement resistance of the material. It can be seen from Examples 1 to 4 that the present invention can achieve matching of high strength and high plasticity of the wire rod, reaching a tensile strength of 1430 to 1480 MPa and a cross-sectional shrinkage of 40% to 45%, which is suitable for efficient and green manufacturing of 15.9-grade non-quenched and tempered bolts.
[0083] From the comparison results of Example 2 and Comparative Example 4, it can be seen that the use of a higher spinning temperature can avoid the precipitation of secondary cementite in the wire rod during the spinning stage caused by high carbon components, which is beneficial to the formation of finer pearlite structure; from the comparison results of Example 2 and Comparative Example 5, it can be seen that the higher the molten salt temperature of the first stage molten salt and the longer the treatment time, the more pearlite structure is formed, the subsequent tempered bainite structure is reduced, the plasticity of the wire rod increases, and the strength decreases, but the molten salt temperature is too high, there is a risk of ferrite precipitation, and the matrix strength decreases; from the comparison results of Example 2 and Comparative Example 6, it can be seen that the lower the molten salt temperature of the first stage molten salt and the shorter the treatment time, the less pearlite structure is formed, the strength of the wire rod increases, and the plasticity decreases, but the molten salt temperature is too low, the treatment time is too short, and the proportion of tempered pearlite structure is too small, which is not good for the matrix plasticity.
[0084] From the comparison results of Example 3 and Comparative Example 7, it can be seen that after a stage of molten salt treatment, the transformation of the untransformed structure in the wire rod to the bainite structure is not conducive, the precipitation driving force of the vanadium-containing carbide is reduced, it is not conducive to the formation of fine precipitation phases, and the strength of the wire rod decreases; from the comparison results of Example 3 and Comparative Example 8, it can be seen that the lower the molten salt temperature of the second stage of the molten salt, the more beneficial it is to the rapid formation of the bainite structure, but the shorter the treatment time, the quenched bainite and the matrix cannot be fully softened; from the comparison results of Example 3 and Comparative Example 9, it can be seen that the longer the treatment time, the better the tempering and softening effect of the matrix structure, but if the treatment time is too long, there is a risk of precipitation and coarsening of Cr and V, which is not conducive to both strength and plasticity. From the comparison results of Example 4 and Comparative Example 10, it can be seen that after slow cooling on a roller, the high temperature state of the wire rod after passing through the molten salt can be utilized to reduce the cooling rate and promote further softening of the wire rod.
[0085] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A 15.9 grade non-quenched and tempered cold heading steel wire rod for bolts, characterized in that: The chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.87% to 0.90%, Si: 0.40% to 0.58%, Mn: 0.40% to 0.60%, Cr: 0.10% to 0.30%, Al: 0.20% to 0.40%, V: 0.010% to 0.025%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities, and its microstructure includes a mixed structure consisting of tempered pearlite with a volume percentage of ≥60% and tempered bainite with a volume percentage of ≥35%; The manufacturing method comprises: rolling the wire rod according to the chemical composition of the 15.9 grade non-quenched and tempered cold heading steel wire rod for bolts, spinning the wire rod into a wire rod at a spinning temperature of ≥910°C, and then performing online salt bath phase transformation control, so that the wire rod first passes through a first stage of molten salt, and the wire rod is cooled at a cooling rate of ≥35°C / s to a pearlite phase region for isothermal phase transformation, so as to promote the transformation of part of the austenite in the wire rod into a pearlite structure, and then the wire rod is cooled by a second stage of molten salt to promote the transformation of the untransformed austenite in the wire rod into a bainite structure, and at the same time, the wire rod is tempered and softened, and the vanadium-containing carbide is filled. The steel wire rod is dispersed and precipitated, and finally slowly cooled by a roller to be made into a cold heading steel wire rod whose microstructure includes a mixed structure composed of tempered pearlite and tempered bainite; the molten salt temperature of the first section of molten salt is 555-580°C, and the processing time is 30-50s; the molten salt temperature of the second section of molten salt is 450-500°C, and the processing time is 100-300s; the roller slow cooling first controls the wire rod to slowly cool at a cooling rate of 0.1-0.45°C / s for 50-200s, and then controls the wire rod to cool at a cooling rate of 0.75-1.5°C / s to coiling.
2. The 15.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 1, characterized in that: The interlamellar spacing of the tempered pearlite is 155-210 nm, and the network carbide of the cold heading steel wire rod is level 0.
3. The 15.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 1, characterized in that: The cold heading steel wire rod has a diameter of 12.0-28.0 mm, a tensile strength of 1430-1480 MPa, and a cross-sectional shrinkage of 40%-45%.
4. A method for manufacturing a 15.9 grade non-quenched and tempered cold heading steel wire rod for bolts, characterized in that: The manufacturing method thereof comprises: The wire rod is produced by rolling the chemical composition of the 15.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 1. After the wire rod is spun into a wire rod at a spinning temperature of ≥910°C, an online salt bath phase transformation control is performed, so that the wire rod first passes through a first stage of molten salt, and the wire rod is cooled to the pearlite phase region at a cooling rate of ≥35°C / s for isothermal phase transformation, promoting the transformation of part of the austenite in the wire rod into the pearlite structure, and then the wire rod is cooled and isothermally cooled by a second stage of molten salt to promote the transformation of the untransformed austenite in the wire rod into the bainite structure, and at the same time, the wire rod is tempered and softened, and the vanadium-containing carbide is dispersed and precipitated, and finally it is slowly cooled by a roller to produce a cold heading steel wire rod with a microstructure including a mixed structure consisting of tempered pearlite with a volume percentage of ≥60% and tempered bainite with a volume percentage of ≥35%; The molten salt temperature of the first section of molten salt is 555-580°C, and the processing time is 30-50s. The molten salt temperature of the second section of molten salt is 450-500°C, and the processing time is 100-300s. The roller slow cooling first controls the wire rod to slowly cool at a cooling rate of 0.1-0.45°C / s for 50-200s, and then controls the wire rod to cool at a cooling rate of 0.75-1.5°C / s until it is coiled.
5. The method for manufacturing the 15.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 4, characterized in that: Before the rolling, the heating furnace is controlled to have a soaking temperature of 1080-1150° C. and a furnace time of 2.5-4 hours.
6. The method for manufacturing the 15.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 4, characterized in that: During the rolling, the initial rolling temperature is controlled to be 1060-1120°C, the heavy-load finishing rolling temperature is ≥940°C, the finishing rolling reduction is 5%-15%, the heavy-load sizing temperature is ≥930°C, and the sizing reduction is 2%-5%.
7. The method for manufacturing the 15.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 4, characterized in that: The molten salt circulation volume of the first section molten salt is 400-600 t / h, and the molten salt temperature rise is ≤10°C; the molten salt circulation volume of the second section molten salt is 300-400 t / h, and the molten salt temperature rise is ≤7°C.