A method for avoiding delayed cracking of low alloy high strength steel plate after cutting

An optimized production process for low-alloy high-strength steel plates addresses the issue of delayed cracking by controlling chemical composition and production steps, ensuring crack-free steel plates with enhanced structural integrity.

CN118653109BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411118541.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-12-03
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Existing methods for preventing delayed cracks in thick low-alloy high-strength steel plates, particularly those with a thickness of 40 to 80mm and a strength of 1000MPa or above, are either costly or limited in thickness, and they fail to effectively prevent cracks after flame cutting, which can lead to sudden brittle fractures.

Method used

A method involving optimized continuous casting, heating, rolling, heat treatment, and cutting processes, including controlled chemical composition and production steps such as molten steel smelting, RH vacuum degassing, micro-Ti treatment, B alloying, continuous casting with slow cooling, reheating, controlled rolling and cooling, quenching, and tempering, followed by careful cutting and slow cooling of the cut edges to prevent hydrogen embrittlement.

Benefits of technology

The method effectively prevents delayed cracking in low-alloy high-strength steel plates, ensuring they remain crack-free for over 60 days by reducing internal stress and hydrogen content through controlled processes, thereby enhancing structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a method for preventing delayed cracks from being generated after cutting a low alloy high strength steel plate. The chemical composition of the steel plate is as follows: C 0.14%-0.19%, Si 0.15%-0.35%, Mn 1.05%-1.45%, P≤0.02%, S≤0.005%, Nb 0.010%-0.040%, Ti 0.010%-0.025%, Mo 0.5%-0.8%, Als 0.02%-0.05%, Ca 0.005%-0.010%, B 0.0008%-0.0018%, Cr 0.3%-0.5%, Ni 0.3%-0.5%, and the balance is Fe and impurities. The production process of steel plate includes: molten steel smelting, refining outside the furnace + RH vacuum degassing, micro-Ti treatment, B alloying, continuous casting, heating and slow cooling of the ingot, reheating of the ingot, controlled cooling, hot straightening, slow cooling of steel plate stacking, quenching, tempering and cutting. The present invention effectively solves the problem of delayed cracking after steel cutting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel plate surface quality control, and in particular to a method for preventing delayed cracks from occurring after cutting of a 1000MPa-grade low-alloy high-strength steel plate for engineering machinery with a thickness specification of 40 to 80mm. Background Art

[0002] In recent years, with the rapid development of industries such as hydropower, engineering machinery, and wind power construction, the demand for thick steel plates has increased. Low-alloy high-strength steel for engineering machinery is widely used due to its low alloy element content (low cost), high strength and high toughness (good overall performance); the steel plate can be cut by laser cutting, plasma cutting, flame cutting and other methods in the later processing process. The thickness of the steel plate corresponding to laser cutting and plasma cutting is usually below 40mm, so there are certain limitations in use; and flame cutting is widely used due to its low cost, easy operation, high cutting efficiency, and a wide range of cuttable steel plate thickness. Flame cutting is often used for thick and high-strength steel plates for engineering machinery, but delayed cracks are easily formed on the flame-cut surface after flame cutting. There are no obvious signs before the delayed cracks occur, and they will cause sudden brittle fractures after expansion, which will cause losses to users and may also lead to catastrophic consequences. Delayed cracking of the fire-cut surface is caused by the phase change of the cut surface of the steel plate due to the influence of the cutting heat cycle (such as the presence of segregation bands and large-sized inclusions with sharp corners in the structure), which easily captures hydrogen atoms, thereby causing hydrogen embrittlement and forming delayed cracks. The existence of the above problems has seriously restricted the development of engineering machinery and other fields, and how to solve them has become an urgent matter for steel manufacturing companies to consider.

[0003] The Chinese invention patent with application number CN201510453518.5 discloses a "control method for avoiding delayed cracks in cutting of thick medium and high carbon steel in winter". The high carbon steel plate designed with high C and Mn components is normalized and flame cut before slow cooling. After flame cutting, it is placed in a slow cooling pit for stress relief treatment, thereby reducing the formation of martensite structure, reducing tissue stress concentration, and avoiding stress delayed cracks after flame cutting. However, the high carbon steel plate after flame cutting is placed in a slow cooling pit or a single furnace at a temperature of 300℃ to 350℃, kept warm for 1.5h to 2.5h, and then cooled to below 100℃ with the furnace, which is bound to increase the user's production cost.

[0004] The Chinese patent application with application number CN202210040898.X discloses "a method for preventing delayed cracks in cutting of thick low-alloy martensitic steel". It adopts a reasonable content ratio of Ti, Nb, Mo, Al and B elements to control the hardenability and inclusion size of thick steel plates; in addition, secondary quenching and low-temperature tempering heat treatment processes are adopted to avoid the formation and expansion of delayed cracks; the steel plate is flame cut, and the steel plate is preheated before flame cutting. After windproof cutting, it is covered with refractory insulation cotton or moved into an insulation pit for slow cooling, which effectively avoids stress-induced delayed cracks after cutting. However, the maximum thickness of the steel plate is limited to 70 mm, and the Ti / N ratio is relatively strict. In addition, it adopts a secondary quenching process, which increases the heat treatment production cost. Summary of the invention

[0005] The present invention provides a method for avoiding delayed cracks after cutting of low-alloy high-strength steel plates. For high-strength steel plates for engineering machinery with a thickness of 1000MPa or above and a specification of 40 to 80mm, the method of optimizing continuous casting, heating, rolling, heat treatment and cutting processes is adopted to effectively solve the problem of delayed cracks after steel cutting. The cut steel plates are placed for more than 60 days without delayed cracks.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preventing delayed cracks from occurring after cutting a low alloy high strength steel plate comprises controlling the chemical composition of the steel plate and controlling the production process of the steel plate; the chemical composition of the steel plate comprises, by weight percentage: C 0.14% to 0.19%, Si 0.15% to 0.35%, Mn 1.05% to 1.45%, P≤0.02%, S≤0.005%, Nb 0.010% to 0.040%, Ti 0.010% to 0.025%, Mo 0.5% to 0.8%, Als 0.02% to 0.05%, Ca 0.005% to 0.010%, B 0.0008% to 0.0018%, Cr0.3% to 0.5%, Ni 0.3%~0.5%, the balance is Fe and unavoidable impurities, and the total amount of impurity elements is less than 0.05%; the production process of steel plate includes: molten steel smelting, refining outside the furnace + RH vacuum degassing, micro-Ti treatment, B alloying, continuous casting, heating and slow cooling of ingots into the pit, reheating of ingots, controlled cooling, hot straightening, slow cooling of steel plate stacking, quenching, tempering and cutting.

[0008] Furthermore, the production process of the steel plate is specifically as follows:

[0009] 1) Molten steel smelting to casting billet heating and slow cooling:

[0010] During the pretreatment of molten iron, the S content is controlled to be less than 0.015%, during the converter smelting, the P content is controlled to be ≤0.02%, and the C content at the end of the converter smelting is controlled to be 0.14%-0.19%; argon is blown for 25-35 minutes when the converter is tapped; during the LF refining process, Si-Ca wire is fed for refining outside the furnace; RH vacuum degassing is maintained for more than 25 minutes, and Al is added according to the Als content requirements after the degassing treatment is completed, and Ti-Fe is added for micro-Ti treatment, and B-Fe alloy is added for B alloying; during continuous casting The superheat is controlled at 15-25℃, and the continuous casting billet drawing rate is 0.8-1.3m / min; the electromagnetic stirring current intensity in the secondary cooling zone during the continuous casting stage is 100-150A, and the secondary cooling water volume is 1.3-2.0L / kg; the billet is pressed down by 30-45mm under heavy pressure at the horizontal fan-shaped section, i.e., the end of solidification; the billet is put into the pit for slow cooling after it comes off the line, and the pit temperature is not less than 600℃, the slow cooling temperature is 600-650℃, and the slow cooling time is 48-72h. The billet is cooled down to below 150℃ in the pit before leaving the pit;

[0011] 2) Reheating of ingot: the temperature of preheating section is 900-1050℃, the temperature of soaking section and heating section are both 1225-1250℃, the total heating time of soaking section and heating section is 4-5.5h, and the total time in furnace is 6-8h;

[0012] 3) Controlled rolling, controlled cooling and hot straightening: Rolling is carried out in two stages: the starting rolling temperature of rough rolling is ≥1120℃, and the final rolling temperature of rough rolling is 980~1025℃; the rough rolling is not more than 6 passes, and the reduction rate of at least the first 2 passes is more than 15%; during the intermediate billet waiting for temperature, at least 2 passes of descaling water are sprayed, and the descaling time of each pass is 1~2min, and the descaling water pressure is 15~20MPa; the starting rolling temperature of finishing rolling is 860~920℃, and the final rolling temperature of finishing rolling is 820~850℃; the finishing rolling is not more than 6 passes, and the reduction rate of at least the first 2 passes is more than 20%; slow rolling is adopted in the finishing rolling stage, and the rolling speed is 1~2m / s; the straightening temperature of hot straightening is 750~800℃, the straightening force is 3000~4500kN, the bending roll amount is 1.2~1.8mm, and the tilting value is 3.5~5.5mm;

[0013] 4) Steel plates are stacked and slowly cooled: After hot straightening, they are immediately stacked and slowly cooled. The stacking temperature is not less than 400°C and the slow cooling time is not less than 48 hours.

[0014] 5) Quenching; quenching heating includes low temperature section, high temperature section and cooling section; the temperature of low temperature section is 620~680℃, the time of low temperature section in furnace is 2.0~3.5min / mm; the temperature of high temperature section is 880~920℃, the time of high temperature section in furnace is 1.5~1.8min / mm; the temperature of cooling section is 760~810℃, the time of cooling section in furnace is 0.5~0.9min / mm; the average cooling rate of quenching is 20~45℃ / s; the final temperature of quenching is 180~250℃;

[0015] 6) Tempering: The tempering heating temperature is 150-180°C, and the tempering holding time is 2.0-3.5min / mm;

[0016] 7) Cutting: The preheating temperature of the steel plate is 100℃~200℃, and the cutting is carried out at room temperature. The welding line energy is controlled below 20kJ / cm during cutting. After cutting, the cutting edge and heat-affected zone are covered with asbestos cloth insulation blanket and slowly cooled to room temperature.

[0017] Furthermore, the finished steel plate is a steel plate of 1000MPa or above.

[0018] Furthermore, the thickness of the finished steel plate is 40 to 80 mm; the thickness of the cast billet is 250 to 300 mm; and the thickness of the intermediate billet is 2.5 to 3.5 times the thickness of the finished steel plate.

[0019] Furthermore, in step 7), the steel plate is preheated by using a flame burner, an electronic heating pad or a heating furnace.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1) Before continuous casting and when tapping the converter, argon blowing is used to calm the steel to promote the removal of inclusions in the molten steel and improve the uniformity of the molten steel composition; during the refining process outside the furnace, the Si-Ca wire is fed for refining outside the furnace, which can effectively reduce the oxygen and sulfur content in the molten steel, so that the sulfide and oxide inclusions are transformed into calcium-containing spherical inclusions, and the number of inclusions is reduced, thereby achieving the purpose of purifying the molten steel, improving the quality of steel, and reducing the local internal stress of the steel plate during rolling. By controlling the continuous casting overheat and the billet drawing rate, the quality defects in the core and corners of the billet can be effectively reduced; by optimizing the current intensity of the electromagnetic stirring in the secondary cooling zone and the secondary cooling water volume, the average carbon segregation index can be reduced, thereby inhibiting segregation; by limiting the secondary cooling intensity, the trend of the central crack of the billet can be inhibited. Putting it under heavy pressure can help reduce the segregation of the billet, refine the austenite grains, and reduce internal structural defects; slow cooling of the billet into the pit helps to reduce the central segregation of the billet and effectively reduce the H content inside the billet.

[0022] 2) When heating the ingot, the temperature of the preheating section is controlled to ensure that the carbides of Ti and Nb are quickly and fully dissolved in the matrix and fully diffused; a high heating temperature is used, and the furnace time and total furnace time of the soaking section and the heating section are guaranteed at the same time, which effectively promotes the full diffusion of elements such as C, Mn, Mo, and H, and ensures the uniformity of the structure of the rolled steel plate.

[0023] 3) A two-stage controlled rolling process is adopted. By controlling the final rolling temperature in the rough rolling stage, the intermediate billet is ensured to be in the austenite recrystallization temperature range during the warming process to ensure the uniformity of the structure. At the same time, the reduction rate and thickness of the intermediate billet in the two-stage rolling are limited to ensure the uniformity of the structure in the thickness direction of the rolled steel plate; spraying descaling water during the warming process of the intermediate billet can inhibit the growth of austenite grains, and at the same time generate a temperature gradient on the inner and outer surfaces of the billet, promote the penetration of rolling deformation to the center of the thickness, refine the grains at 1 / 2 thickness, which is beneficial to improve the core structure of thick-gauge steel plates and reduce the structural stress caused by uneven structure; slow rolling is used to increase the deformation penetration of the core of the steel plate and further improve the uniformity of the structure; at the same time, the straightening process parameters are optimized to promote the full release of internal stress.

[0024] 4) After hot straightening, the steel plate is stacked and slowly cooled, and the slow cooling time and temperature are limited to accelerate the diffusion of C, Mn, and H elements in the core of the steel plate, inhibit their segregation, and reduce the stress difference in the core of the steel plate and the occurrence of hydrogen-induced cracks in the steel plate.

[0025] 5) The quenching and heating of steel plates includes low temperature section, high temperature section and cooling section. The purpose of controlling the temperature of the low temperature section and the time in the furnace is to continue to promote the diffusion of H elements in the steel plate to the outside and reduce the H content of the steel plate. On the other hand, it promotes the precipitation of Nb and Ti composite carbides through long-term heat preservation. These carbides will provide a large number of hydrogen traps inside the steel plate. The temperature of the high temperature section and the time in the furnace are limited. The purpose is to quickly heat the steel plate to the austenitizing temperature, provide organizational guarantee for the subsequent quenching of the steel plate to obtain martensite, and prevent the coarsening of grains and Nb and Ti composite carbides caused by excessive temperature, so that the number of hydrogen traps inside the steel plate is greatly reduced and the risk of cracks is increased. The temperature of the cooling section and the time in the furnace are limited. The purpose is to reduce the austenite to above the Ar3 temperature in the cooling section, that is, to ensure the full austenitization state of the steel plate, so that the quenched steel plate is fully hardened. At the same time, the lower the temperature at which the steel plate starts quenching, the lower the stress level of the steel plate during the quenching process, which can avoid the cracking of the steel plate due to the quenching process. At the same time, in order to avoid quenching cracks caused by excessive stress in the steel plate due to excessive cooling rate during quenching, the average quenching cooling rate is designed to be 20-45℃ / s, and the quenching end temperature is limited. The purpose is to reduce the stress of the steel plate during quenching, avoid quenching cracks, and ensure that the austenite in the steel plate fully completes the martensite transformation.

[0026] 6) Preheat the steel plate and limit the welding line energy to prevent excessive input energy from causing coarsening of the heat-affected zone structure, which may lead to cracks due to excessive internal stress after the steel plate is cooled; after cutting, cover the cut edge and heat-affected zone with an asbestos cloth insulation blanket and slowly cool to room temperature. Avoid a humid environment during the slow cooling process and strictly prohibit contact with water and other liquids. The purpose is to prevent the steel plate from cooling rapidly after cutting and causing tissue stress and cracks.

[0027] 7) After adopting the process of the present invention, the cut steel plate was placed for more than 60 days without any delayed crack defects. DETAILED DESCRIPTION

[0028] The invention discloses a method for preventing delayed cracks from being generated after cutting a low alloy high strength steel plate. The chemical composition of the steel plate comprises, by weight percentage, C 0.14% to 0.19%, Si 0.15% to 0.35%, Mn 1.05% to 1.45%, P≤0.02%, S≤0.005%, Nb 0.010% to 0.040%, Ti 0.010% to 0.025%, Mo 0.5% to 0.8%, Als 0.02% to 0.05%, Ca 0.005% to 0.010%, B 0.0008% to 0.0018%, Cr 0.3% to 0.5%, Ni 0.3% to 0.5%, the remainder being Fe and unavoidable impurities, and the total amount of impurity elements being less than 0.05%.

[0029] The functions of the main elements in the steel plate are as follows:

[0030] C: Carbon is an important element to ensure the hardenability of steel plates and an important factor in determining carbon equivalent. It has a great influence on the strength, toughness, plasticity and weldability of steel. Too high carbon content affects the welding performance of steel plates. Too low carbon content affects the overall strength of steel plates. Under the premise of ensuring the required strength of steel plates, the present invention controls the carbon content to be in the range of 0.14% to 0.19%.

[0031] Si: an essential element for deoxidation, having a certain solid solution strengthening effect. Too high a content will affect the toughness of steel, the uniformity of performance of extra thick plates and weldability. In the present invention, the silicon content is controlled in the range of 0.15% to 0.35%.

[0032] Mn: An important solid solution strengthening element in steel, which can reduce the phase transition temperature, refine the microstructure, improve toughness while strengthening the steel plate, and improve hardenability. Too high manganese content will cause segregation, which is not good for welding and toughness. The present invention controls the manganese content in the range of 1.05% to 1.45%.

[0033] Ni: can improve the low temperature toughness of steel and improve plasticity. For extra thick plates, it can improve the low temperature impact performance at 1 / 4 and 1 / 2 of the thickness direction, and is an indispensable alloy element; Ni can also delay pearlite transformation, promote the formation of medium temperature transformation structure, and reduce the cooling rate limit of thick gauge steel plates. However, the price of nickel is relatively high. Considering the production cost comprehensively, the present invention controls the Ni content to 0.3% to 0.5%.

[0034] Cr: can increase the hardenability of steel, refine the structure, and reduce the ductile-brittle transition temperature; chromium and manganese are used together to improve the hardenability of steel and improve the mechanical properties of steel; chromium has a smaller segregation tendency than manganese, and replacing part of manganese with chromium can reduce the segregation in the core of the steel plate, improve the internal quality of the steel plate, and improve the uniformity of the mechanical properties; the present invention controls the chromium content to 0.3% to 0.5%.

[0035] Mo: can significantly increase the hardenability and hardenability of steel, refine the microstructure of steel after quenching, and improve toughness. However, molybdenum is a precious alloy. In order to reduce production costs, under the premise of ensuring performance, less or no molybdenum can be added according to the thickness of the steel plate. Therefore, the molybdenum content of the present invention is controlled within the range of 0.50% to 0.80%.

[0036] Nb: It is one of the commonly used elements in modern microalloyed steels. It has good fine grain strengthening and precipitation strengthening effects and can delay austenite recrystallization. However, excessive Nb will increase production costs and the difficulty of continuous casting process control. The present invention selects a Nb content range of 0.01% to 0.04%, and at the same time cooperates with a reasonable TMCP process to obtain a uniform composite phase dominated by acicular ferrite structure, so that the finished steel plate has good toughness.

[0037] Ti: It is a strong N-fixing element and exists in the form of TiN in the continuous casting billet. Fine TiN particles can effectively inhibit the growth of austenite grains during the reheating of the continuous casting billet, and help to increase the solid solubility of Nb in austenite and improve the impact toughness of the welding heat affected zone. However, when the Ti addition exceeds a certain value, the TiN particles will coarsen, thereby increasing the stress concentration level between the particle interface and the matrix. Therefore, the present invention controls the Ti content range to be 0.01% to 0.025%.

[0038] B: It is an effective element to significantly improve the hardenability of steel. It is easy to segregate at the grain boundary and prevent carbon precipitation. A trace amount of boron can play a significant role. When the boron content is too high, boron carbonitride is easily formed, which reduces toughness and causes hot brittleness. The present invention controls its content range to 0.0008% to 0.0018%.

[0039] Ca: Trace amounts of calcium can be used as a purifier for deoxidation and desulfurization in steel, improve the morphology of non-metallic inclusions, and are widely used in calcium-treated clean steel. By adding trace amounts of calcium to steel, dispersed, thermally stable second-phase calcium-containing oxide particles can be formed in the steel. Relevant research results show that the dispersed calcium-containing oxide particles pin the austenite grain boundary migration of the CGHAZ during the welding thermal cycle, restrict the growth of austenite grains, and obtain a finer weld CGHAZ grain size, thereby improving the strength and toughness of the micro-calcium steel welded CGHAZ. However, too high a level of Ca will segregate at the grain boundaries, adversely affecting the hardenability and impact toughness of the steel. The present invention controls its content in the range of 0.005% to 0.0010%.

[0040] Als: Usually used as a deoxidizer in steel, it can also refine the structure if AlN is formed. When the Al content exceeds 0.05%, excessive aluminum oxide inclusions will reduce the cleanliness of the steel. If the Al content is too low, deoxidation is insufficient, and easily oxidizable elements such as Ti will form oxides. The present invention sets the lower limit of the Al content to 0.02%.

[0041] P and S are inevitable impurity elements in steel. Too high P and S will affect the toughness and welding performance of the steel plate, so the lower the better. However, due to the consideration of smelting process, it cannot be unlimitedly low. Therefore, the upper limit of P and S content is set to 0.02% and 0.005% respectively in the present invention.

[0042] The method of the present invention is applicable to low-alloy high-strength steel plates for engineering machinery with a thickness specification of 40 to 80 mm and a strength level of 1000 MPa or above. The entire process flow of the steel plates from molten steel smelting to cutting includes molten steel smelting → refining outside the furnace + RH vacuum degassing → micro-Ti treatment → B alloying → continuous casting → heating and slow cooling of the ingot into the pit → reheating of the ingot → controlled rolling and controlled cooling → hot straightening → stacking and slow cooling of the steel plates → quenching → tempering → cutting of the steel plates.

[0043] The present invention mainly controls the following process:

[0044] 1) Molten steel smelting to casting billet heating and slow cooling:

[0045] The raw materials are pretreated with KR molten iron to control the S content below 0.015%, and then enter the converter after slag removal; the double slag method is used for converter smelting to remove P, and the P content is controlled to be ≤0.02%. The C content is controlled at 0.14%~0.19% at the end of converter smelting, and argon is blown for 25~35 minutes when the converter is tapped; argon blowing before continuous casting can promote the removal of inclusions in the molten steel and improve the uniformity of the molten steel composition.

[0046] During the LF refining process, the molten steel is treated by feeding Si-Ca wire to effectively reduce the oxygen and sulfur content in the molten steel, so that the sulfide and oxide inclusions are transformed into calcium-containing spherical inclusions, while reducing the number of inclusions, thereby achieving the purpose of purifying the molten steel, improving the quality of steel, and reducing the local internal stress of the steel plate during rolling. The RH vacuum degassing is maintained for more than 25 minutes; after the degassing treatment is completed, Al is added according to the Als content requirements; then Ti-Fe is added for micro-titanium treatment, and B-Fe alloy is added; when the alloy is added, it must be ensured that it is added to the molten steel to avoid floating on the slag layer.

[0047] During continuous casting of slabs, the continuous casting superheat is controlled at 15-25℃, and the continuous casting billet drawing rate is 0.8-1.3m / min. By controlling the continuous casting superheat and the continuous casting billet drawing speed, the quality defects in the core and corners of the billet can be effectively reduced. The electromagnetic stirring current intensity of the secondary cooling zone in the continuous casting stage is controlled to be 100-150A, and the secondary cooling water volume is 1.3-2.0L / kg to reduce the average carbon segregation index and inhibit segregation. At the same time, by controlling the secondary cooling intensity, the trend of the central crack of the billet is inhibited. When the horizontal fan-shaped section, i.e., the end of solidification, is put under heavy pressure, the continuous casting billet is pressed down by 30-45mm; putting under heavy pressure can help reduce billet segregation, refine austenite grains, and reduce internal structural defects.

[0048] After the billet comes off the production line, it enters the pit for slow cooling. The temperature entering the pit is not less than 600℃, the slow cooling temperature is 600-650℃, and the slow cooling time is 48-72h. The billet is cooled to 150℃ in the pit before leaving the pit. Slow cooling of the billet entering the pit helps to reduce the center segregation of the billet and effectively reduce the H content inside the billet.

[0049] 2) Ingot reheating: The ingot (thickness of 250-300 mm) is sent into a walking beam heating furnace for heating. The temperature range of the preheating section is 900-1050 ° C. The purpose is to promote the rapid and sufficient solid solution of Ti and Nb carbides in the matrix and to fully diffuse; the temperature of the soaking section and the heating section are both 1225-1250 ° C. The total heating time of the soaking section and the heating section is 4-5.5 hours, and the total time in the furnace is 6-8 hours. A high heating temperature is used, while ensuring the time in the soaking section and the heating section, and increasing the total time in the furnace, in order to effectively promote the full diffusion of elements such as C, Mn, Mo, and H, and ensure the uniformity of the rolled steel plate structure.

[0050] 3) Controlled rolling, controlled cooling and hot straightening:

[0051] Rolling is divided into two stages; the first stage is recrystallization rolling (rough rolling), the rough rolling start temperature is ≥1120℃, the rough rolling final rolling temperature range is 980~1025℃, the rough rolling is not more than 6 passes, and the pass reduction system is preferably that the reduction rate of the first two passes is more than 15%. The thickness of the intermediate billet is 2.5~3.5 times the thickness of the finished steel plate. During the intermediate billet waiting for temperature, 2 passes of descaling water are sprayed, the descaling time is 1~2min, and the descaling machine pressure is 15~20MPa; the purpose is to inhibit the growth of austenite grains, and at the same time generate a temperature gradient on the inner and outer surfaces of the billet, promote the penetration of rolling deformation to the center of the thickness, refine the grains at 1 / 2 thickness, improve the core structure of thick specification steel plates, and reduce the organizational stress caused by uneven organization.

[0052] The second stage is non-recrystallization rolling (finishing rolling), the starting temperature of finishing rolling is 860-920℃, the final temperature of finishing rolling is 820-850℃, the finishing rolling is no more than 6 passes, and the pass reduction system is preferably that the reduction rate of the first two passes is more than 20%. Slow rolling is adopted in the finishing rolling stage, with a rolling speed of 1-2m / s.

[0053] By controlling the final rolling temperature in the rough rolling stage, the intermediate billet is kept in the austenite recrystallization temperature range during the temperature waiting process to ensure the uniformity of the structure; by limiting the reduction rate of the two-stage rolling, the uniformity of the structure in the thickness direction of the rolled steel plate is ensured.

[0054] The straightening temperature during hot straightening is 750-800℃, the straightening force is between 3000-4500kN, the bending roller amount is set to 1.2-1.8mm, and the tilting value is set to 3.5-5.5mm; by optimizing the straightening process parameters, the internal stress is fully released.

[0055] 4) Stacking and slow cooling of steel plates: stack and slow cool immediately after hot straightening, the stacking temperature shall not be lower than 400℃, and the slow cooling time shall not be less than 48h; stacking and slow cooling can accelerate the diffusion of C, Mn and H elements in the core of the steel plate, inhibit their segregation, and slow down the stress difference of the core structure of the steel plate and the occurrence of hydrogen-induced cracks in the steel plate.

[0056] 5) Quenching;

[0057] In the present invention, the steel plate quenching heating includes a low temperature section, a high temperature section and a temperature reduction section.

[0058] The low temperature section temperature of the quenching heat treatment furnace is 620-680℃, and the low temperature section time in the furnace is 2.0-3.5min / mm. Its purpose is to continue to promote the outward diffusion of H in the steel plate and reduce the H content of the steel plate. On the other hand, it is to promote the precipitation of a large number of Nb and Ti composite carbides through long-term heat preservation. These carbides will provide a large number of hydrogen traps inside the steel plate. Considering that too high a temperature will cause the coarsening of Nb and Ti composite carbides, resulting in cracks due to stress accumulation during the subsequent forming process of the steel plate, the low temperature section heat preservation temperature should not exceed 680℃.

[0059] The temperature of the high temperature section is 880-920°C, and the furnace time of the high temperature section is 1.5-1.8 min / mm. The purpose is to quickly heat the steel plate to the austenitizing temperature to provide organizational guarantee for the subsequent quenching of the steel plate to obtain martensite; but too high a temperature will lead to grain coarsening, and further cause the coarsening of Nb and Ti composite carbides, which will greatly reduce the number of hydrogen traps inside the steel plate, thereby increasing the risk of cracks; therefore, the holding time of the high temperature section should not exceed 1.8 min / mm.

[0060] The temperature of the cooling section is 760-810°C, and the furnace time of the cooling section is 0.5-0.9 min / mm. The purpose is to reduce the austenite to above the Ar3 temperature in the cooling section, that is, to ensure that the steel plate is in a fully austenitized state and the quenched steel plate is fully hardened; at the same time, the lower the starting quenching temperature of the steel plate, the lower the stress level of the steel plate during the quenching process, which can avoid cracking of the steel plate due to the quenching process.

[0061] After the steel plate leaves the quenching heat treatment furnace, it enters the roller quenching machine for quenching. In order to obtain sufficient martensitic transformation and avoid excessive stress of the steel plate caused by excessive cooling rate and quenching cracks, the average cooling rate of quenching is 20-45℃ / s; the final quenching temperature is 180-250℃, the purpose is to reduce the stress of the steel plate during quenching, avoid quenching cracks, and ensure that the austenite of the steel plate can fully complete the martensitic transformation.

[0062] 6) Tempering: Tempering is the main technical means to reduce quenching residual stress. It can fully release the residual stress of the steel plate under the premise of ensuring the hardness of the steel plate. The present invention controls the tempering heating temperature to be 150-180°C and the tempering holding time to be 2.0-3.5min / mm.

[0063] 7) Cutting; The preheating temperature of the steel plate is 100℃~200℃, which can be carried out by flame torch, electronic heating pad, or heating furnace; welding is carried out at room temperature, and attention should be paid to controlling overheating of the welding zone, and the welding line energy should be below 20kJ / cm (control the input energy to be too large, which will cause the coarsening of the heat-affected zone structure, and cause excessive internal stress after the steel plate is cooled, resulting in cracks). After cutting, cover the cutting edge and heat-affected zone with asbestos cloth insulation blanket, and slowly cool to room temperature. Avoid humid environment during the slow cooling process, and it is strictly forbidden to contact with water and other liquids (avoid rapid cooling of the steel plate after cutting, which will cause cracks due to tissue stress).

[0064] The present invention optimizes the smelting, heating, rolling, heat treatment and cutting processes, and ultimately solves the problem of delayed cracking of low-alloy high-strength steel for engineering machinery with a thickness specification of 40 to 80 mm and a strength level of 1000 MPa or above after cutting. The cut steel plate is placed for more than 60 days without delayed cracking.

[0065] In order to more intuitively embody the present invention, the embodiments of the present invention are further described in conjunction with examples. The following examples are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any technical solution that can be obviously obtained by a person skilled in the art within the technical scope disclosed in the present invention, including simple changes or equivalent replacements, is within the protection scope of the present invention. Example

[0066] Table 1 shows the chemical composition of the steel in each embodiment, Table 2 shows the smelting, continuous casting and slow cooling process parameters of the steel in each embodiment, Table 3 shows the heating process parameters of the cast ingot in each embodiment, Table 4 shows the rolling process parameters of the steel plate in each embodiment, Table 5 shows the hot straightening and stacking slow cooling process parameters of the steel plate in each embodiment, Table 6 shows the heat treatment process parameters of the steel plate in each embodiment, and Table 7 shows the cutting process parameters and surface conditions of the steel plate in each embodiment.

[0067] Table 1 Chemical composition of steel (wt, %)

[0068] Example C Si Mn Mo Als B Ti Nb Ni Cr Ca 1 0.17 0.16 1.21 0.56 0.033 0.0013 0.018 0.025 0.42 0.39 0.007 2 0.14 0.32 1.19 0.65 0.045 0.0008 0.021 0.034 0.39 0.44 0.008 3 0.16 0.27 1.33 0.79 0.025 0.0017 0.023 0.015 0.36 0.43 0.006 4 0.18 0.33 1.09 0.74 0.037 0.0010 0.014 0.036 0.49 0.38 0.008 5 0.17 0.23 1.43 0.62 0.047 0.0013 0.019 0.032 0.38 0.47 0.010 6 0.19 0.29 1.26 0.55 0.036 0.0009 0.017 0.026 0.32 0.37 0.005

[0069] Note: Impurity elements in steel: P≤0.02%, S≤0.005%.

[0070] Table 2 Process parameters for steel smelting, continuous casting and slow cooling of ingots

[0071] Example Argon blowing time / min RH vacuum degassing time / min Superheat / ℃ <![CDATA[Drawing speed / (m·min -1 )]]> Electromagnetic stirring current intensity / A Continuous casting billet reduction / mm Secondary cooling water volume / (L / kg) Pit entry temperature / ℃ Slow cooling temperature / ℃ Slow cooling time / h Outlet temperature / ℃ 1 28 28 17 0.9 120 36 1.6 620 630 50 130 2 25 25 23 1.3 140 33 2.0 615 640 70 150 3 26 27 25 1.2 135 39 1.4 620 635 48 145 4 32 30 21 1.0 150 45 1.8 605 645 65 110 5 30 32 24 1.1 140 35 1.9 640 650 72 120 6 33 28 20 0.8 125 38 1.7 630 640 50 130

[0072] Table 3 Heating process parameters of ingot

[0073]

[0074] Table 4 Rolling process parameters of steel plates

[0075] Example Rough rolling start temperature / ℃ Rough rolling and final rolling temperature / ℃ Rough rolling pass First pass reduction rate in rough rolling stage / % Second pass reduction rate in rough rolling stage / % Finish rolling start temperature / ℃ Finish rolling temperature / ℃ Finishing rolling pass First pass reduction rate in finishing rolling stage / % Second pass reduction rate in finishing rolling stage / % 2-pass descaling time / min Descaling water pressure / MPa Intermediate billet thickness / mm Rolling speed / m / s 1 1130 1012 4 18 20 910 840 5 22 24 1.0、1.6 18、20 200 1.5 2 1125 1015 5 16 18 900 820 6 22 25 1.2、1.8 15、19 140 1.3 3 1120 1025 6 16 20 885 825 5 22 23 1.3、2.0 16、18 180 1.6 4 1120 1005 5 16 18 880 830 5 22 23 1.2、1.8 15、18 200 1.7 5 1135 996 4 17 19 900 840 6 22 25 1.7、1.9 16、20 150 1.2 6 1135 985 5 18 16 890 845 5 22 25 1.2、1.6 18、20 150 1.8

[0076] Table 5 Process parameters of hot straightening and stacking slow cooling of steel plates

[0077] Example Heat correction temperature / ℃ Straightening force / kN Roll bending amount / mm Tilt value / mm Stacking temperature / ℃ Stacking time / h 1 750 3200 1.2 3.6 500 50 2 785 4200 1.6 5.5 520 52 3 770 4500 1.7 4.8 560 50 4 780 3500 1.5 4.5 530 49 5 775 3600 1.8 3.8 525 60 6 760 4300 1.3 5.3 570 48

[0078] Table 6 Steel plate heat treatment process parameters

[0079] Example Low temperature section temperature / ℃ Low temperature section in furnace time / min / mm High temperature section temperature / ℃ High temperature section in furnace time / min / mm Cooling section temperature / ℃ Cooling time in furnace / min / mm Average cooling rate / ℃ / s Quenching end temperature / ℃ Tempering temperature / ℃ Tempering time / min / mm 1 660 2.8 880 1.7 780 0.6 25 200 160 2.5 2 680 3.2 905 1.5 800 0.8 30 230 180 3.0 3 630 3.3 910 1.5 770 0.9 35 185 170 3.3 4 650 2.1 920 1.8 790 0.7 28 190 160 3.1 5 670 2.6 885 1.6 810 0.8 40 220 150 2.2 6 665 2.8 890 1.7 805 0.7 36 230 165 2.6

[0080] Table 7 Steel plate cutting process parameters and surface conditions after cutting

[0081] Example Plate thickness / mm Preheating temperature / ℃ Welding line energy / kJ / cm Number of days Whether there are cracks 1 60 150 18 65 none 2 40 180 15 80 none 3 70 200 19 60 none 4 80 180 16 70 none 5 45 178 18 100 none 6 50 190 17 120 none

[0082] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preventing delayed cracking of low alloy high strength steel plate after cutting, characterized in that: Including controlling the chemical composition of the steel plate and controlling the production process of the steel plate; the chemical composition of the steel plate includes by weight percentage: C 0.14%~0.19%, Si 0.15%~0.35%, Mn 1.05%~1.45%, P≤0.02%, S≤0.005%, Nb 0.010%~0.040%, Ti0.010%~0.025%, Mo 0.5%~0.8%, Als 0.02%~0.05%, Ca 0.005%~0.010%, B 0.0008%~0.0018%, Cr 0.3%~0.5%, Ni 0.3%~0.5%, the balance is Fe and unavoidable impurities, and the total amount of impurity elements is less than 0.05%; the production process of steel plate includes: molten steel smelting, refining outside the furnace + RH vacuum degassing, micro-Ti treatment, B alloying, continuous casting, heating and slow cooling of ingots into the pit, ingot reheating, controlled rolling and controlled cooling, hot straightening, slow cooling of steel plate stacking, quenching, tempering and cutting; The production process of the steel plate is as follows: 1) Molten steel smelting to casting billet heating and slow cooling: During the pretreatment of molten iron, the S content is controlled to be less than 0.015%, during the converter smelting, the P content is controlled to be ≤0.02%, and the C content at the end of the converter smelting is controlled to be 0.14%-0.19%; argon is blown for 25-35 minutes when the converter is tapped; during the LF refining process, Si-Ca wire is fed for refining outside the furnace; RH vacuum degassing is maintained for more than 25 minutes, and Al is added according to the Als content requirements after the degassing treatment is completed, and Ti-Fe is added for micro-Ti treatment, and B-Fe alloy is added for B alloying; during continuous casting The superheat is controlled at 15-25℃, and the continuous casting billet drawing rate is 0.8-1.3m / min; the electromagnetic stirring current intensity in the secondary cooling zone during the continuous casting stage is 100-150A, and the secondary cooling water volume is 1.3-2.0L / kg; the billet is pressed down by 30-45mm under heavy pressure at the horizontal fan-shaped section, i.e., the end of solidification; the billet is put into the pit for slow cooling after it comes off the line, and the pit temperature is not less than 600℃, the slow cooling temperature is 600-650℃, and the slow cooling time is 48-72h. The billet is cooled down to below 150℃ in the pit before leaving the pit; 2) Reheating of ingot: the temperature of preheating section is 900-1050℃, the temperature of soaking section and heating section are both 1225-1250℃, the total heating time of soaking section and heating section is 4-5.5h, and the total time in furnace is 6-8h; 3) Controlled rolling and cooling: Rolling is carried out in two stages: the starting temperature of rough rolling is ≥1120℃, and the final rolling temperature of rough rolling is 980~1025℃; the rough rolling is not more than 6 passes, and the reduction rate of at least the first 2 passes is more than 15%; during the intermediate billet waiting for temperature, at least 2 passes of descaling water are sprayed, and the descaling time of each pass is 1~2min, and the descaling water pressure is 15~20MPa; the starting temperature of finishing rolling is 860~920℃, and the final rolling temperature of finishing rolling is 820~850℃; the finishing rolling is not more than 6 passes, and the reduction rate of at least the first 2 passes is more than 20%; slow rolling is adopted in the finishing rolling stage, and the rolling speed is 1~2m / s; the straightening temperature of hot straightening is 750~800℃, the straightening force is 3000~4500kN, the bending roll amount is 1.2~1.8mm, and the tilting value is 3.5~5.5mm; 4) Steel plates are stacked and slowly cooled: After hot straightening, they are immediately stacked and slowly cooled. The stacking temperature is not less than 400°C and the slow cooling time is not less than 48 hours. 5) Quenching; quenching heating includes low temperature section, high temperature section and cooling section; the temperature of low temperature section is 620~680℃, the time of low temperature section in furnace is 2.0~3.5min / mm; the temperature of high temperature section is 880~920℃, the time of high temperature section in furnace is 1.5~1.8min / mm; the temperature of cooling section is 760~810℃, the time of cooling section in furnace is 0.5~0.9min / mm; the average cooling rate of quenching is 20~45℃ / s; the final temperature of quenching is 180~250℃; 6) Tempering: The tempering heating temperature is 150-180°C, and the tempering holding time is 2.0-3.5min / mm; 7) Cutting: The preheating temperature of the steel plate is 100℃~200℃, and the cutting is carried out at room temperature. The welding line energy is controlled below 20kJ / cm during cutting. After cutting, the cutting edge and heat-affected zone are covered with asbestos cloth insulation blanket and slowly cooled to room temperature.

2. A method for preventing delayed cracking of low alloy high strength steel plate after cutting according to claim 1, characterized in that: The finished steel plate is above 1000MPa grade.

3. The method for preventing delayed cracking of low alloy high strength steel plate after cutting according to claim 1, characterized in that: The thickness of the finished steel plate is 40-80 mm; the thickness of the ingot is 250-300 mm; the thickness of the intermediate ingot is 2.5-3.5 times the thickness of the finished steel plate.

4. The method for preventing delayed cracking of low alloy high strength steel plate after cutting according to claim 1, characterized in that: In the step 7), the steel plate is preheated by using a flame burner, an electronic heating pad or a heating furnace.