A nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof

By combining modified nylon staple fiber with nano-zirconium carbide particles and components such as silver nitrate and citric acid, a high adhesion and uniform silver plating layer is formed, which solves the problem of easy falling off of traditional silver-plating fiber plating and significantly improves electromagnetic Shielding performance and durability.

CN118653299BActive Publication Date: 2024-11-08潍坊瑞银纺织科技有限公司
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411143970.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-08
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

Traditional silver-plated fibers show significant performance in the field of electromagnetic shielding, but their coating adhesion is insufficient, resulting in the silver layer falling off after repeated washing or long-term use, affecting the service life and shielding performance of the material.

Method used

Modified nylon staple fiber is combined with chitosan and nano-zirconium carbide particles, combined with silver nitrate, citric acid and succinate sulfonate wetting agent, and a uniform silver plating is formed through ultrasonic dispersion and impregnation reaction, which enhances the coating. Adhesion and stability.

Benefits of technology

It significantly improves the electromagnetic shielding efficiency and durability of nylon silver-plated staple fiber, enhances the adhesion and uniformity of the silver-plated layer, and extends the service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of electromagnetic shielding, and in particular to a nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof. The nylon silver-plated staple fiber comprises the following components: 1-3 parts by weight of modified nylon staple fiber, 1.5-3 parts by weight of silver nitrate, 0.2-1 parts by weight of sodium citrate, 0.01-0.05 parts by weight of a succinate sulfonate wetting agent, and 0.05-0.1 parts by weight of a sodium adipate inhibitor, wherein the modified nylon staple fiber is formed by composite modification of chitosan and nano zirconium carbide particles, and the nylon silver-plated staple fiber is modified by nano zirconium carbide and chitosan to prepare a nylon silver-plated staple fiber with electromagnetic shielding, the electromagnetic shielding effect of the nylon silver-plated staple fiber is improved by nano zirconium carbide, the interface bonding between silver ions and the nylon staple fiber is enhanced by chitosan, the adhesion of the silver-plated layer is improved, and the durability of the nylon silver-plated staple fiber is improved, the wetting agent is added to reduce bubbles and gaps, and the inhibitor slows down the silver ion plating rate, so that the silver plating is more uniform and the silver plating effect is better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electromagnetic shielding, and in particular to a nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof. Background Art

[0002] In today's highly information-based and electronic society, electromagnetic radiation is everywhere. From wireless communication networks, radar systems, microwave ovens to various electronic devices, electromagnetic waves permeate our living and working environment. Although electromagnetic waves have brought convenience to modern technology, they have also brought potential health risks and equipment interference problems. Long-term exposure to high-intensity electromagnetic radiation will have adverse effects on human health, such as nervous system disorders, sleep disorders, immune system suppression, etc. Therefore, the preparation of clothing with electromagnetic shielding effect has become increasingly important. Silver-plated fibers have become an ideal choice for electromagnetic shielding materials due to their excellent conductivity and relatively light weight. Through chemical plating, electroplating, spraying or dipping, a thin metal film can be formed on the surface of non-conductive fibers, thereby giving the fibers good electromagnetic shielding capabilities. When they are woven into fabrics, they can effectively block or absorb electromagnetic waves, thereby providing necessary protection.

[0003] Although traditional silver-plated fibers have shown remarkable performance in the field of electromagnetic shielding, they also have some inherent limitations and challenges, which restrict their widespread use in certain applications. For example, the adhesion of the silver plating layer is often insufficient, which means that after repeated washing or long-term use, the silver layer is easy to fall off, resulting in a gradual decrease in shielding effectiveness and affecting the service life of the material. How can the fiber have both excellent electromagnetic shielding performance and better durability? In view of this, we propose a nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof. Summary of the invention

[0004] The object of the present invention is to provide a nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0005] To achieve the above-mentioned purpose, the present invention provides a nylon silver-plated staple fiber with electromagnetic shielding, comprising the following components: 1-3 parts by weight of modified nylon staple fiber, 1.5-3 parts by weight of silver nitrate, 0.2-1 parts by weight of sodium citrate, 0.01-0.05 parts by weight of succinate sulfonate wetting agent and 0.05-0.1 parts by weight of sodium adipate inhibitor, wherein the modified nylon staple fiber is composite-modified by chitosan and nano zirconium carbide particles.

[0006] Preferably, the preparation method of the modified nylon staple fiber is as follows:

[0007] S1.1. Use ethanol solvent to clean the nylon staple fibers to remove grease and impurities on the surface, and dry them in an oven at 60-80℃;

[0008] S1.2. Use dilute acetic acid as solvent, weigh an appropriate amount of chitosan to prepare a solution, heat and stir at 60-80°C for 2-3h until completely dissolved;

[0009] S1.3, weigh a certain amount of nano zirconium carbide particles, use the above chitosan solution as a dispersion medium, add the nano zirconium carbide particles to the chitosan solution, and use an ultrasonic instrument to disperse the nano zirconium carbide particles in the medium to avoid agglomeration, to obtain a mixed solution of chitosan and nano zirconium carbide;

[0010] S1.4, immerse the pretreated nylon staple fiber into the mixed solution at room temperature for 20-30 minutes, take out the fiber and place it at 1-2kg / cm 2 The fiber is dipped and pressed under pressure, and finally dried at 50-60°C for 1-1.5h to obtain modified nylon staple fiber.

[0011] Nano zirconium carbide is a high-performance nanomaterial belonging to transition metal carbides. It combines the unique properties of carbides and zirconium elements, and has high melting point, high hardness, good high temperature stability, corrosion resistance and good conductivity. Therefore, when it is applied to nylon staple fibers, it can greatly improve the electromagnetic shielding effect of nylon silver-plated staple fibers. First, since the nano zirconium carbide particles themselves have a certain electronic conductivity, when the zirconium carbide nanoparticles are compounded on the nylon staple fibers, they can form a conductive network to enhance the conductivity of the entire fabric. We know that the stronger the conductivity, the more electromagnetic waves are reflected and absorbed on the fabric. Therefore, the compounding of nano zirconium carbide particles makes the nylon silver-plated staple fibers greatly improve the electromagnetic shielding effectiveness. Secondly, the dielectric properties and size effect of zirconium carbide nanoparticles can lead to increased scattering and absorption of electromagnetic waves in fabrics. That is to say, due to the high conductivity and dielectric loss of nano zirconium carbide particles, when electromagnetic waves pass through the material, the free charges in the nanoparticles vibrate under the action of the alternating electromagnetic field, resulting in ohmic loss and polarization loss, and part of the energy will be converted into Thermal energy increases the absorption of electromagnetic waves in fabrics. In addition, since the size of the nanoparticles is comparable to the wavelength of the incident electromagnetic waves, they scatter electromagnetic waves like small antennas, causing the energy distribution of electromagnetic waves to change. Part of the energy is scattered in other directions, reducing the energy of electromagnetic waves that penetrate in a straight line, increasing the scattering of electromagnetic waves in fabrics, thereby enhancing the shielding effect. Then, when the nano zirconium carbide particles are compounded with the nylon silver-plated staple fibers, it is equivalent to forming a multi-layer structure. When electromagnetic waves pass through each layer, they encounter different dielectric constants and conductivity, thereby increasing the energy dissipation of electromagnetic waves and enhancing multiple reflections and absorption of electromagnetic waves. In addition, since the nanoparticles provide a larger surface area and more contact points, the physical and chemical bonding between the coating and the fiber is enhanced, making the coating more uniform and firm. Finally, since the nano zirconium carbide particles have good high-temperature stability and corrosion resistance, the composite nylon silver-plated staple fibers can still maintain their electromagnetic shielding performance in harsh environments, greatly improving the electromagnetic shielding effect and durability of the nylon silver-plated staple fibers.

[0012] Chitosan is a natural polysaccharide composed of N-acetylglucosamine units and deacetylated glucosamine units, containing a large number of amino groups (-NH2) and hydroxyl groups (-OH). On the one hand, these functional groups can combine with the carboxyl or amide groups on the surface of nylon staple fibers through hydrogen bonds or electrostatic attraction, so that they are adsorbed on the surface of nylon fibers to form a chitosan film. This film can serve as an intermediate layer to improve the adhesion between the fiber and the metallic silver coating, thereby enhancing the affinity of chitosan to nylon staple fibers. On the other hand, these functional groups can form chelates with metallic silver ions (Ag⁺) under appropriate pH conditions. When the pH of the amino groups in the chitosan molecules is low, the amino groups exist more in the form of protonated -NH3⁺, and the coordination ability with silver ions is weak at this time. When the pH is high, the unprotonated amino groups -NH2, which form chelates with silver ions, However, when the pH is high, silver ions will react with hydroxide ions (OH⁻) in water to form insoluble silver oxide (Ag2O), so a suitable pH value needs to be selected. In addition, hydroxyl groups can be partially dissociated into -O⁻ in aqueous solution. This negatively charged oxygen atom can also form a coordination bond with silver ions, so that the silver ions are attached to the nylon staple fiber, enhancing the adhesion of the silver plating. In addition, in an acidic or neutral environment, the -NH2 in the chitosan molecule receives an H⁺ and turns into a positively charged -NH3⁺, and its surface charge properties change. The positively charged chitosan can form a stronger electrostatic interaction with the negatively charged dye, thereby improving the dyeing depth and dye uptake rate. Chitosan itself also has certain antibacterial properties. When it is fixed on nylon fibers, it can give nylon fibers antibacterial properties.

[0013] Preferably, the mass fraction of the dilute acetic acid is 0.8-1%.

[0014] Preferably, the chitosan is prepared by dilute acetic acid into a solution with a mass fraction of 1-5%.

[0015] Preferably, the nano zirconium carbide particles account for 5-7% of the total chitosan solution mass.

[0016] Preferably, the frequency range of the ultrasonic instrument is 20-40 kHz, and the ultrasonic time is 20-30 min.

[0017] On the other hand, the present invention provides a method for preparing nylon silver-plated staple fibers with electromagnetic shielding, which is used for any one of the above-mentioned nylon silver-plated staple fibers with electromagnetic shielding, comprising the following steps:

[0018] The modified nylon staple fiber is placed in a silver nitrate solution, a sodium adipate inhibitor and a succinate sulfonate wetting agent are added to the silver nitrate solution, stirred evenly, a citric acid solution is added and the pH is adjusted, and the mixture is immersed in the reaction at 30-50°C for 50-60 minutes, and finally the surface precipitate is cleaned and dried at 60-80°C to obtain a nylon silver-plated staple fiber with electromagnetic shielding.

[0019] Citric acid, with the chemical formula C6H8O7, is an organic weak acid. First, as a reducing agent, citric acid promotes the reduction of silver ions and helps the deposition and distribution of silver ions on the surface of modified nylon staple fibers. This is because the carboxyl group (-COOH) in the citric acid molecule can provide electrons to silver ions, reducing them from a +1 valence state to a 0 valence state, and depositing them on the surface of the modified nylon staple fibers to form a silver-plated layer. Secondly, citric acid can also be used as a cross-linking agent to improve the adhesion and durability of chitosan on the surface of nylon staple fibers. This is because the amino group (-NH2) in the chitosan molecule can react with the carboxyl group (-COOH) in the citric acid molecule to produce an ammonium salt through an acid-base neutralization reaction, and the hydroxyl group (-OH) in the chitosan molecule can also react with the carboxyl group (-COOH) in the citric acid molecule to produce an ester bond (-O-CO-), thereby enhancing the stability of the nylon silver-plated staple fiber structure.

[0020] As a surfactant, succinate sulfonate wetting agent has good emulsifying, wetting and penetrating properties, which can reduce the surface tension of the silver plating solution, improve the wettability of the silver plating solution on the fiber surface, and help the coating to be more evenly distributed; sodium adipate, with the molecular formula C6H8Na2O4, can be used as an inhibitor in the silver plating process to achieve a uniform silver coating. This is because sodium adipate can form a complex with silver ions, which helps to control the effective concentration of silver ions, thereby affecting the growth rate and uniformity of the coating.

[0021] Preferably, the acid silver solution is prepared by mixing silver nitrate and deionized water in a mass ratio of 1:95-100.

[0022] Preferably, the citric acid solution is prepared by mixing sodium citrate and deionized water in a mass ratio of 1:50-55.

[0023] Preferably, the pH value is adjusted to 5-6 by citric acid solution.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] In the nylon silver-plated staple fiber with electromagnetic shielding and the preparation method thereof, nano zirconium carbide and chitosan are used to modify the nylon staple fiber to prepare the nylon silver-plated staple fiber with electromagnetic shielding. Since the nano zirconium carbide itself has high electronic conductivity, dielectric properties and size effect, the electromagnetic shielding effect of the nylon silver-plated staple fiber is greatly improved, and the binding force between chitosan and nylon staple fiber and the chelating force of silver ions are utilized to enhance the interface bonding between silver ions and nylon staple fiber, and improve the adhesion of the silver-plated layer. At the same time, citric acid is added to reduce silver ions so that silver is deposited on the modified nylon staple fiber, and chitosan is further solidified, thereby improving the durability of the nylon silver-plated staple fiber. A wetting agent is added to reduce bubbles and voids, and an inhibitor is added to slow down the silver ion plating rate, so that the silver plating is more uniform and the silver plating effect is better. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0027] The invention discloses a nylon silver-plated staple fiber with electromagnetic shielding, comprising the following components: 1-3 parts by weight of modified nylon staple fiber, 1.5-3 parts by weight of silver nitrate, 0.2-1 parts by weight of sodium citrate, 0.01-0.05 parts by weight of succinate sulfonate wetting agent and 0.05-0.1 parts by weight of sodium adipate inhibitor, wherein the modified nylon staple fiber is formed by composite modification of chitosan and nano zirconium carbide particles.

[0028] Embodiment 1: A nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof, comprising the following steps:

[0029] S1.1. Prepare components: 2 parts by weight of modified nylon staple fiber, 1.5 parts by weight of silver nitrate, 0.5 parts by weight of sodium citrate, 0.01 parts by weight of succinate sulfonate wetting agent, and 0.05 parts by weight of sodium adipate inhibitor;

[0030] S1.2. Pretreatment of nylon staple fibers: Use ethanol solvent to clean the nylon staple fibers to remove grease and impurities on the surface, and dry them in an oven at 70°C;

[0031] S1.3, prepare chitosan solution: use 1% dilute acetic acid as solvent, weigh an appropriate amount of chitosan to prepare a 1% solution, heat and stir at 80°C for 2h until completely dissolved;

[0032] S1.4, dispersing nano zirconium carbide particles: weigh a certain amount of nano zirconium carbide particles, wherein the nano zirconium carbide particles account for 5% of the total chitosan solution mass, use the chitosan solution as a dispersion medium, add the nano zirconium carbide particles into the chitosan solution, and use an ultrasonic instrument to disperse the nano zirconium carbide particles in the medium to avoid agglomeration, the ultrasonic frequency is set to 30 kHz, and the ultrasonic time is 30 min;

[0033] S1.5, Preparation of modified nylon staple fiber: Immerse the pretreated nylon staple fiber into the mixed solution at room temperature, soak for 20 minutes, take out the fiber and place it at 1kg / cm 2 The modified nylon staple fibers were obtained by dipping and rolling under the pressure of , and finally drying at 50℃ for 1h.

[0034] S1.6. Prepare a nylon silver-plated staple fiber with electromagnetic shielding: prepare a silver nitrate solution by mixing silver nitrate and deionized water in a mass ratio of 1:100, place the modified nylon staple fiber in the silver nitrate solution, add a sodium adipate inhibitor and a succinate sulfonate wetting agent to the silver nitrate solution, stir evenly, then add a citric acid solution prepared by mixing sodium citrate and deionized water in a mass ratio of 1:50, adjust the pH to 5, immerse and react at 40°C for 60 minutes, finally clean the surface precipitate, and dry at 75°C to obtain a nylon silver-plated staple fiber with electromagnetic shielding.

[0035] Embodiment 2: A nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof, comprising the following steps:

[0036] S1.1. Prepare components: 2 parts by weight of modified nylon staple fiber, 1.5 parts by weight of silver nitrate, 0.5 parts by weight of sodium citrate, 0.01 parts by weight of succinate sulfonate wetting agent, and 0.05 parts by weight of sodium adipate inhibitor;

[0037] S1.2. Pretreatment of nylon staple fibers: Use ethanol solvent to clean the nylon staple fibers to remove grease and impurities on the surface, and dry them in an oven at 70°C;

[0038] S1.3, prepare chitosan solution: use 1% dilute acetic acid as solvent, weigh an appropriate amount of chitosan to prepare a 3% solution, heat and stir at 80°C for 2h until completely dissolved;

[0039] S1.4, dispersing nano zirconium carbide particles: weigh a certain amount of nano zirconium carbide particles, wherein the nano zirconium carbide particles account for 5% of the total chitosan solution mass, use the chitosan solution as a dispersion medium, add the nano zirconium carbide particles into the chitosan solution, and use an ultrasonic instrument to disperse the nano zirconium carbide particles in the medium to avoid agglomeration, the ultrasonic frequency is set to 30 kHz, and the ultrasonic time is 30 min;

[0040] S1.5, Preparation of modified nylon staple fiber: Immerse the pretreated nylon staple fiber into the mixed solution at room temperature, soak for 20 minutes, take out the fiber and place it at 1kg / cm 2 The modified nylon staple fiber was obtained by dipping and pressing under pressure and finally drying at 50°C for 1h.

[0041] S1.6. Prepare a nylon silver-plated staple fiber with electromagnetic shielding: prepare a silver nitrate solution by mixing silver nitrate and deionized water in a mass ratio of 1:100, place the modified nylon staple fiber in the silver nitrate solution, add a sodium adipate inhibitor and a succinate sulfonate wetting agent to the silver nitrate solution, stir evenly, then add a citric acid solution prepared by mixing sodium citrate and deionized water in a mass ratio of 1:50, adjust the pH to 5, immerse and react at 40°C for 60 minutes, finally clean the surface precipitate, and dry at 75°C to obtain a nylon silver-plated staple fiber with electromagnetic shielding.

[0042] Embodiment 3: A nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof, comprising the following steps:

[0043] S1.1. Prepare components: 2 parts by weight of modified nylon staple fiber, 1.5 parts by weight of silver nitrate, 0.5 parts by weight of sodium citrate, 0.01 parts by weight of succinate sulfonate wetting agent, and 0.05 parts by weight of sodium adipate inhibitor;

[0044] S1.2. Pretreatment of nylon staple fibers: Use ethanol solvent to clean the nylon staple fibers to remove grease and impurities on the surface, and dry them in an oven at 70°C;

[0045] S1.3, prepare chitosan solution: use 1% by mass dilute acetic acid as solvent, weigh an appropriate amount of chitosan to prepare a 5% by mass solution, heat and stir at 80°C for 2h until completely dissolved;

[0046] S1.4, dispersing nano zirconium carbide particles: weigh a certain amount of nano zirconium carbide particles, wherein the nano zirconium carbide particles account for 5% of the total chitosan solution mass, use the chitosan solution as a dispersion medium, add the nano zirconium carbide particles into the chitosan solution, and use an ultrasonic instrument to disperse the nano zirconium carbide particles in the medium to avoid agglomeration, the ultrasonic frequency is set to 30 kHz, and the ultrasonic time is 30 min;

[0047] S1.5, Preparation of modified nylon staple fiber: Immerse the pretreated nylon staple fiber into the mixed solution at room temperature, soak for 20 minutes, take out the fiber and place it at 1kg / cm 2 The modified nylon staple fiber was obtained by dipping and pressing under pressure and finally drying at 50°C for 1h.

[0048] S1.6. Prepare a nylon silver-plated staple fiber with electromagnetic shielding: prepare a silver nitrate solution by mixing silver nitrate and deionized water in a mass ratio of 1:100, place the modified nylon staple fiber in the silver nitrate solution, add a sodium adipate inhibitor and a succinate sulfonate wetting agent to the silver nitrate solution, stir evenly, then add a citric acid solution prepared by mixing sodium citrate and deionized water in a mass ratio of 1:50, adjust the pH to 5, immerse and react at 40°C for 60 minutes, finally clean the surface precipitate, and dry at 75°C to obtain a nylon silver-plated staple fiber with electromagnetic shielding.

[0049] Embodiment 4: A nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof, comprising the following steps:

[0050] S1.1. Prepare components: 2 parts by weight of modified nylon staple fiber, 1.5 parts by weight of silver nitrate, 0.5 parts by weight of sodium citrate, 0.01 parts by weight of succinate sulfonate wetting agent, and 0.05 parts by weight of sodium adipate inhibitor;

[0051] S1.2. Pretreatment of nylon staple fibers: Use ethanol solvent to clean the nylon staple fibers to remove grease and impurities on the surface, and dry them in an oven at 70°C;

[0052] S1.3, prepare chitosan solution: use 1% dilute acetic acid as solvent, weigh an appropriate amount of chitosan to prepare a 3% solution, heat and stir at 80°C for 2h until completely dissolved;

[0053] S1.4, dispersing nano zirconium carbide particles: weigh a certain amount of nano zirconium carbide particles, wherein the nano zirconium carbide particles account for 6% of the total chitosan solution mass, use the chitosan solution as a dispersion medium, add the nano zirconium carbide particles into the chitosan solution, and use an ultrasonic instrument to disperse the nano zirconium carbide particles in the medium to avoid agglomeration, the ultrasonic frequency is set to 30 kHz, and the ultrasonic time is 30 min;

[0054] S1.5, Preparation of modified nylon staple fiber: Immerse the pretreated nylon staple fiber into the mixed solution at room temperature, soak for 20 minutes, take out the fiber and place it at 1kg / cm 2 The modified nylon staple fiber was obtained by dipping and pressing under pressure and finally drying at 50°C for 1h.

[0055] S1.6. Prepare a nylon silver-plated staple fiber with electromagnetic shielding: prepare a silver nitrate solution by mixing silver nitrate and deionized water in a mass ratio of 1:100, place the modified nylon staple fiber in the silver nitrate solution, add a sodium adipate inhibitor and a succinate sulfonate wetting agent to the silver nitrate solution, stir evenly, then add a citric acid solution prepared by mixing sodium citrate and deionized water in a mass ratio of 1:50, adjust the pH to 5, immerse and react at 40°C for 60 minutes, finally clean the surface precipitate, and dry at 75°C to obtain a nylon silver-plated staple fiber with electromagnetic shielding.

[0056] Embodiment 5: A nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof, comprising the following steps:

[0057] S1.1. Prepare components: 2 parts by weight of modified nylon staple fiber, 1.5 parts by weight of silver nitrate, 0.5 parts by weight of sodium citrate, 0.01 parts by weight of succinate sulfonate wetting agent, and 0.05 parts by weight of sodium adipate inhibitor;

[0058] S1.2. Pretreatment of nylon staple fibers: Use ethanol solvent to clean the nylon staple fibers to remove grease and impurities on the surface, and dry them in an oven at 70°C;

[0059] S1.3, prepare chitosan solution: use 1% dilute acetic acid as solvent, weigh an appropriate amount of chitosan to prepare a 3% solution, heat and stir at 80°C for 2h until completely dissolved;

[0060] S1.4, dispersing nano zirconium carbide particles: weigh a certain amount of nano zirconium carbide particles, wherein the nano zirconium carbide particles account for 7% of the total chitosan solution mass, use the chitosan solution as a dispersion medium, add the nano zirconium carbide particles into the chitosan solution, and use an ultrasonic instrument to disperse the nano zirconium carbide particles in the medium to avoid agglomeration, the ultrasonic frequency is set to 30 kHz, and the ultrasonic time is 30 min;

[0061] S1.5, Preparation of modified nylon staple fiber: Immerse the pretreated nylon staple fiber into the mixed solution at room temperature, soak for 20 minutes, take out the fiber and place it at 1kg / cm 2 The modified nylon staple fiber was obtained by dipping and pressing under pressure and finally drying at 50°C for 1h.

[0062] S1.6. Prepare a nylon silver-plated staple fiber with electromagnetic shielding: prepare a silver nitrate solution by mixing silver nitrate and deionized water in a mass ratio of 1:100, place the modified nylon staple fiber in the silver nitrate solution, add a sodium adipate inhibitor and a succinate sulfonate wetting agent to the silver nitrate solution, stir evenly, then add a citric acid solution prepared by mixing sodium citrate and deionized water in a mass ratio of 1:50, adjust the pH to 5, immerse and react at 40°C for 60 minutes, finally clean the surface precipitate, and dry at 75°C to obtain a nylon silver-plated staple fiber with electromagnetic shielding.

[0063] Embodiment 6: A nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof, comprising the following steps:

[0064] S1.1. Prepare components: 2 parts by weight of modified nylon staple fiber, 2 parts by weight of silver nitrate, 0.5 parts by weight of sodium citrate, 0.01 parts by weight of succinate sulfonate wetting agent, and 0.05 parts by weight of sodium adipate inhibitor;

[0065] S1.2. Pretreatment of nylon staple fibers: Use ethanol solvent to clean the nylon staple fibers to remove grease and impurities on the surface, and dry them in an oven at 70°C;

[0066] S1.3, prepare chitosan solution: use 1% dilute acetic acid as solvent, weigh an appropriate amount of chitosan to prepare a 3% solution, heat and stir at 80°C for 2h until completely dissolved;

[0067] S1.4, dispersing nano zirconium carbide particles: weigh a certain amount of nano zirconium carbide particles, wherein the nano zirconium carbide particles account for 6% of the total chitosan solution mass, use the chitosan solution as a dispersion medium, add the nano zirconium carbide particles into the chitosan solution, and use an ultrasonic instrument to disperse the nano zirconium carbide particles in the medium to avoid agglomeration, the ultrasonic frequency is set to 30 kHz, and the ultrasonic time is 30 min;

[0068] S1.5, Preparation of modified nylon staple fiber: Immerse the pretreated nylon staple fiber into the mixed solution at room temperature, soak for 20 minutes, take out the fiber and place it at 1kg / cm 2 The modified nylon staple fiber was obtained by dipping and pressing under pressure and finally drying at 50°C for 1h.

[0069] S1.6. Prepare a nylon silver-plated staple fiber with electromagnetic shielding: prepare a silver nitrate solution by mixing silver nitrate and deionized water in a mass ratio of 1:100, place the modified nylon staple fiber in the silver nitrate solution, add a sodium adipate inhibitor and a succinate sulfonate wetting agent to the silver nitrate solution, stir evenly, then add a citric acid solution prepared by mixing sodium citrate and deionized water in a mass ratio of 1:50, adjust the pH to 5, immerse and react at 40°C for 60 minutes, finally clean the surface precipitate, and dry at 75°C to obtain a nylon silver-plated staple fiber with electromagnetic shielding.

[0070] Embodiment 7: A nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof, comprising the following steps:

[0071] S1.1. Prepare components: 2 parts by weight of modified nylon staple fiber, 3 parts by weight of silver nitrate, 0.5 parts by weight of sodium citrate, 0.01 parts by weight of succinate sulfonate wetting agent, and 0.05 parts by weight of sodium adipate inhibitor;

[0072] S1.2. Pretreatment of nylon staple fibers: Use ethanol solvent to clean the nylon staple fibers to remove grease and impurities on the surface, and dry them in an oven at 70°C;

[0073] S1.3, prepare chitosan solution: use 1% dilute acetic acid as solvent, weigh an appropriate amount of chitosan to prepare a 3% solution, heat and stir at 80°C for 2h until completely dissolved;

[0074] S1.4, dispersing nano zirconium carbide particles: weigh a certain amount of nano zirconium carbide particles, wherein the nano zirconium carbide particles account for 6% of the total chitosan solution mass, use the chitosan solution as a dispersion medium, add the nano zirconium carbide particles into the chitosan solution, and use an ultrasonic instrument to disperse the nano zirconium carbide particles in the medium to avoid agglomeration, the ultrasonic frequency is set to 30 kHz, and the ultrasonic time is 30 min;

[0075] S1.5, Preparation of modified nylon staple fiber: Immerse the pretreated nylon staple fiber into the mixed solution at room temperature, soak for 20 minutes, take out the fiber and place it at 1kg / cm 2 The modified nylon staple fiber was obtained by dipping and pressing under pressure and finally drying at 50°C for 1h.

[0076] S1.6. Prepare a nylon silver-plated staple fiber with electromagnetic shielding: prepare a silver nitrate solution by mixing silver nitrate and deionized water in a mass ratio of 1:100, place the modified nylon staple fiber in the silver nitrate solution, add a sodium adipate inhibitor and a succinate sulfonate wetting agent to the silver nitrate solution, stir evenly, then add a citric acid solution prepared by mixing sodium citrate and deionized water in a mass ratio of 1:50, adjust the pH to 5, immerse and react at 40°C for 60 minutes, finally clean the surface precipitate, and dry at 75°C to obtain a nylon silver-plated staple fiber with electromagnetic shielding.

[0077] Embodiment 8: A nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof, comprising the following steps:

[0078] S1.1. Prepare components: 2 parts by weight of modified nylon staple fiber, 3 parts by weight of silver nitrate, 0.2 parts by weight of sodium citrate, 0.01 parts by weight of succinate sulfonate wetting agent, and 0.05 parts by weight of sodium adipate inhibitor;

[0079] S1.2. Pretreatment of nylon staple fibers: Use ethanol solvent to clean the nylon staple fibers to remove grease and impurities on the surface, and dry them in an oven at 70°C;

[0080] S1.3, prepare chitosan solution: use 1% dilute acetic acid as solvent, weigh an appropriate amount of chitosan to prepare a 3% solution, heat and stir at 80°C for 2h until completely dissolved;

[0081] S1.4, dispersing nano zirconium carbide particles: weigh a certain amount of nano zirconium carbide particles, wherein the nano zirconium carbide particles account for 6% of the total chitosan solution mass, use the chitosan solution as a dispersion medium, add the nano zirconium carbide particles into the chitosan solution, and use an ultrasonic instrument to disperse the nano zirconium carbide particles in the medium to avoid agglomeration, the ultrasonic frequency is set to 30 kHz, and the ultrasonic time is 30 min;

[0082] S1.5, Preparation of modified nylon staple fiber: Immerse the pretreated nylon staple fiber into the mixed solution at room temperature, soak for 20 minutes, take out the fiber and place it at 1kg / cm 2 The modified nylon staple fiber was obtained by dipping and pressing under pressure and finally drying at 50°C for 1h.

[0083] S1.6. Prepare a nylon silver-plated staple fiber with electromagnetic shielding: prepare a silver nitrate solution by mixing silver nitrate and deionized water in a mass ratio of 1:100, place the modified nylon staple fiber in the silver nitrate solution, add a sodium adipate inhibitor and a succinate sulfonate wetting agent to the silver nitrate solution, stir evenly, then add a citric acid solution prepared by mixing sodium citrate and deionized water in a mass ratio of 1:50, adjust the pH to 5, immerse and react at 40°C for 60 minutes, finally clean the surface precipitate, and dry at 75°C to obtain a nylon silver-plated staple fiber with electromagnetic shielding.

[0084] Embodiment 9: A nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof, comprising the following steps:

[0085] S1.1. Prepare components: 2 parts by weight of modified nylon staple fiber, 3 parts by weight of silver nitrate, 1 part by weight of sodium citrate, 0.01 parts by weight of succinate sulfonate wetting agent, and 0.05 parts by weight of sodium adipate inhibitor;

[0086] S1.2. Pretreatment of nylon staple fibers: Use ethanol solvent to clean the nylon staple fibers to remove grease and impurities on the surface, and dry them in an oven at 70°C;

[0087] S1.3, prepare chitosan solution: use 1% dilute acetic acid as solvent, weigh an appropriate amount of chitosan to prepare a 3% solution, heat and stir at 80°C for 2h until completely dissolved;

[0088] S1.4, dispersing nano zirconium carbide particles: weigh a certain amount of nano zirconium carbide particles, wherein the nano zirconium carbide particles account for 6% of the total chitosan solution mass, use the chitosan solution as a dispersion medium, add the nano zirconium carbide particles into the chitosan solution, and use an ultrasonic instrument to disperse the nano zirconium carbide particles in the medium to avoid agglomeration, the ultrasonic frequency is set to 30 kHz, and the ultrasonic time is 30 min;

[0089] S1.5, Preparation of modified nylon staple fiber: Immerse the pretreated nylon staple fiber into the mixed solution at room temperature, soak for 20 minutes, take out the fiber and place it at 1kg / cm 2 The modified nylon staple fiber was obtained by dipping and pressing under pressure and finally drying at 50°C for 1h.

[0090] S1.6. Prepare a nylon silver-plated staple fiber with electromagnetic shielding: prepare a silver nitrate solution by mixing silver nitrate and deionized water in a mass ratio of 1:100, place the modified nylon staple fiber in the silver nitrate solution, add a sodium adipate inhibitor and a succinate sulfonate wetting agent to the silver nitrate solution, stir evenly, then add a citric acid solution prepared by mixing sodium citrate and deionized water in a mass ratio of 1:50, adjust the pH to 5, immerse and react at 40°C for 60 minutes, finally clean the surface precipitate, and dry at 75°C to obtain a nylon silver-plated staple fiber with electromagnetic shielding.

[0091] Embodiment 10: A nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof, comprising the following steps:

[0092] S1.1. Prepare components: 1 part by weight of modified nylon staple fiber, 3 parts by weight of silver nitrate, 1 part by weight of sodium citrate, 0.01 part by weight of succinate sulfonate wetting agent and 0.05 part by weight of sodium adipate inhibitor;

[0093] S1.2. Pretreatment of nylon staple fibers: Use ethanol solvent to clean the nylon staple fibers to remove grease and impurities on the surface, and dry them in an oven at 70°C;

[0094] S1.3, prepare chitosan solution: use 1% dilute acetic acid as solvent, weigh an appropriate amount of chitosan to prepare a 3% solution, heat and stir at 80°C for 2h until completely dissolved;

[0095] S1.4, dispersing nano zirconium carbide particles: weigh a certain amount of nano zirconium carbide particles, wherein the nano zirconium carbide particles account for 6% of the total chitosan solution mass, use the chitosan solution as a dispersion medium, add the nano zirconium carbide particles into the chitosan solution, and use an ultrasonic instrument to disperse the nano zirconium carbide particles in the medium to avoid agglomeration, the ultrasonic frequency is set to 30 kHz, and the ultrasonic time is 30 min;

[0096] S1.5, Preparation of modified nylon staple fiber: Immerse the pretreated nylon staple fiber into the mixed solution at room temperature, soak for 20 minutes, take out the fiber and place it at 1kg / cm 2 The modified nylon staple fiber was obtained by dipping and pressing under pressure and finally drying at 50°C for 1h.

[0097] S1.6. Prepare a nylon silver-plated staple fiber with electromagnetic shielding: prepare a silver nitrate solution by mixing silver nitrate and deionized water in a mass ratio of 1:100, place the modified nylon staple fiber in the silver nitrate solution, add a sodium adipate inhibitor and a succinate sulfonate wetting agent to the silver nitrate solution, stir evenly, then add a citric acid solution prepared by mixing sodium citrate and deionized water in a mass ratio of 1:50, adjust the pH to 5, immerse and react at 40°C for 60 minutes, finally clean the surface precipitate, and dry at 75°C to obtain a nylon silver-plated staple fiber with electromagnetic shielding.

[0098] Embodiment 11: A nylon silver-plated staple fiber with electromagnetic shielding and a preparation method thereof, comprising the following steps:

[0099] S1.1. Prepare components: 3 parts by weight of modified nylon staple fiber, 3 parts by weight of silver nitrate, 1 part by weight of sodium citrate, 0.01 parts by weight of succinate sulfonate wetting agent, and 0.05 parts by weight of sodium adipate inhibitor;

[0100] S1.2. Pretreatment of nylon staple fibers: Use ethanol solvent to clean the nylon staple fibers to remove grease and impurities on the surface, and dry them in an oven at 70°C;

[0101] S1.3, prepare chitosan solution: use 1% dilute acetic acid as solvent, weigh an appropriate amount of chitosan to prepare a 3% solution, heat and stir at 80°C for 2h until completely dissolved;

[0102] S1.4, dispersing nano zirconium carbide particles: weigh a certain amount of nano zirconium carbide particles, wherein the nano zirconium carbide particles account for 6% of the total chitosan solution mass, use the chitosan solution as a dispersion medium, add the nano zirconium carbide particles into the chitosan solution, and use an ultrasonic instrument to disperse the nano zirconium carbide particles in the medium to avoid agglomeration, the ultrasonic frequency is set to 30 kHz, and the ultrasonic time is 30 min;

[0103] S1.5, Preparation of modified nylon staple fiber: Immerse the pretreated nylon staple fiber into the mixed solution at room temperature, soak for 20 minutes, take out the fiber and place it at 1kg / cm 2 The modified nylon staple fiber was obtained by dipping and pressing under pressure and finally drying at 50°C for 1h.

[0104] S1.6. Prepare a nylon silver-plated staple fiber with electromagnetic shielding: prepare a silver nitrate solution by mixing silver nitrate and deionized water in a mass ratio of 1:100, place the modified nylon staple fiber in the silver nitrate solution, add a sodium adipate inhibitor and a succinate sulfonate wetting agent to the silver nitrate solution, stir evenly, then add a citric acid solution prepared by mixing sodium citrate and deionized water in a mass ratio of 1:50, adjust the pH to 5, immerse and react at 40°C for 60 minutes, finally clean the surface precipitate, and dry at 75°C to obtain a nylon silver-plated staple fiber with electromagnetic shielding.

[0105] Comparative Example 1: The method of Example 6 was adopted to silver-plate unmodified nylon staple fibers.

[0106] Comparative Example 2: The method of Example 6 was adopted, only chitosan was used to modify the nylon staple fibers, nano zirconium carbide particles were not added, and other conditions remained unchanged.

[0107] Comparative Example 3: The method of Example 6 was adopted, only single nano zirconium carbide particles were used to modify the nylon staple fibers, chitosan was not added, and other conditions remained unchanged.

[0108] Comparative Example 4: The method of Example 6 was adopted, and an equal amount of polyethyleneimine was used instead of chitosan. After compounding with nano zirconium carbide particles, the nylon staple fibers were modified, and other conditions remained unchanged.

[0109] Comparative Example 5: The method of Example 6 was adopted without adding the sodium adipate inhibitor.

[0110] Comparative Example 6: The method of Example 6 was adopted without adding succinate sulfonate wetting agent.

[0111] The present invention adopts modified nylon staple fiber to prepare a nylon silver-plated staple fiber with electromagnetic shielding, wherein the performance index inspection items and inspection standards of the nylon silver-plated staple fiber with electromagnetic shielding are as follows:

[0112] Impact strength refers to the ability of nylon silver-plated fiber to resist damage under rapid impact load when processed into fabric. It reflects the ability of the material to absorb energy and resist crack propagation under instantaneous stress. First, prepare a specimen of 80mm×10mm×4mm (L×W×T), fix the specimen in the appropriate position of the pendulum impact tester, set the release height of the pendulum to ensure the same conditions for each test, perform the impact test, record the fracture energy of each specimen, and calculate the impact velocity based on the release height of the pendulum of 0.5m and the mass of 2kg. The potential energy of the pendulum is converted into kinetic energy at the moment of impact, which is the impact energy. By measuring the energy difference of the pendulum before and after the impact, the energy absorbed by the specimen is calculated, which is the impact strength.

[0113] The flexural strength is the ability of nylon silver-plated fiber to resist fracture when subjected to bending load when processed into fabric. It is a measure of the maximum ability of a material to withstand stress until failure when bent. Prepare a specimen of 125mm×12.7mm×3.2mm (L×W×T). Use a three-point bending test fixture to place the specimen on a universal material testing machine. Adjust the support spacing according to the thickness of the specimen. Set the loading rate to 10mm / min, start loading until the specimen breaks, and record the maximum load and deformation when the specimen breaks to calculate the flexural strength and modulus.

[0114] GB / T 30142-2013 "Measurement Method for Shielding Effectiveness of Planar Electromagnetic Shielding Materials" is a standard applicable to measuring the electromagnetic shielding effectiveness of planar electromagnetic shielding materials. It covers the electromagnetic shielding effectiveness measurement of electromagnetic shielding fabrics, electromagnetic shielding metal meshes, electromagnetic shielding glass, electromagnetic shielding films, electromagnetic shielding plastics, electromagnetic shielding rubber and other materials. As a conductive composite material, the silver-plated layer on the surface of nylon silver-plated staple fiber can provide electromagnetic shielding effect. Therefore, this standard can be used to test the electromagnetic shielding effectiveness of nylon silver-plated staple fiber.

[0115] According to the above standards, the nylon silver-plated staple fibers with electromagnetic shielding prepared in the above Examples 1-11 and Comparative Examples 1-6 were tested, and the obtained data are shown in Table 1:

[0116] Table 1 Performance data of Examples 1-11 and Comparative Examples 1-6

[0117]

[0118] The above data fully show that compared with comparative examples 1-6, examples 1-11 can fully show the effect of the modified nylon staple fiber on the mechanical and electromagnetic shielding properties of a nylon silver-plated staple fiber with electromagnetic shielding.

[0119] Since the present invention adopts modified nylon staple fiber to prepare a nylon silver-plated staple fiber with electromagnetic shielding, the performance of the nylon silver-plated staple fiber with electromagnetic shielding is effectively improved by modifying the nylon staple fiber, as follows:

[0120] It can be seen from Examples 1-3 that as the chitosan content continues to increase, the mechanical properties and electromagnetic shielding effectiveness first increase and then decrease. This is because chitosan contains a large number of amino and hydroxyl groups. These functional groups can be combined with the carboxyl or amide groups on the surface of the nylon staple fiber through hydrogen bonds or electrostatic attraction, so that it is adsorbed on the surface of the nylon fiber to form a layer of chitosan film. This film can be used as an intermediate layer to improve the adhesion of the fiber to the metal silver coating of other substances, thereby enhancing the affinity of chitosan and nylon staple fibers. This good interfacial bonding can effectively transfer stress, thereby improving the mechanical properties of the nylon silver-plated staple fibers. At the same time, because chitosan can chelate with silver ions and increase the content of silver ions deposited on the surface of the staple fibers, the conductivity of the obtained nylon silver-plated staple fibers is enhanced, thereby increasing the electromagnetic shielding effectiveness of the nylon silver-plated staple fibers; however, if the chitosan content is too high, It will lead to an increase in the porosity inside the material, which will make chitosan brittle and the fiber brittle, and its mechanical properties will decrease; excessive chitosan molecules will occupy more space and provide more coordination sites, so that silver ions have more opportunities to combine with the amino and hydroxyl groups on chitosan to form chitosan-silver complexes, rather than directly reacting with the reducing agent and depositing on the fiber surface. That is, the complexation reaction of chitosan molecules with silver ions becomes a competitive process, competing with the reduction reaction of the reducing agent on silver ions for silver ions. As a result of this competition, a part of the silver ions are consumed by chitosan, reducing the amount of silver ions available for deposition on the fiber surface, thereby reducing the efficiency of chemical silver plating. The reduction in silver plating efficiency means that the silver layer formed on the fiber surface may be thinner or discontinuous, affecting the conductivity of the silver-plated fiber, and thus the electromagnetic shielding effect is significantly reduced.

[0121] It can be seen from Examples 2, 4 and 5 that with the increase in the content of nano zirconium carbide particles, the mechanical properties of a nylon silver-plated staple fiber with electromagnetic shielding first increase and then decrease, and the electromagnetic shielding performance first increases and then changes little. This is because the size of zirconium carbide is at the nano level, so that the nano zirconium carbide particles can be evenly dispersed on the surface of the nylon silver-plated staple fiber as a reinforcing phase, which is beneficial to reduce stress concentration points, increase the material's resistance to crack propagation, and improve the material's mechanical properties. In addition, due to the dielectric properties and size effect of nano zirconium carbide itself, as well as a certain electronic conductivity, the scattering and absorption of electromagnetic waves in the fabric increase, the conductivity of the nylon silver-plated staple fiber is enhanced, and the electromagnetic shielding effectiveness of the nylon silver-plated staple fiber is enhanced; however, when the zirconium carbide content is high, the brittleness of the coating will increase, thereby reducing the mechanical properties of the nylon silver-plated staple fiber.

[0122] It can be seen from Examples 4, 6 and 7 that as the concentration of silver nitrate gradually increases, its electromagnetic shielding effect first increases and then decreases. This is because a lower silver nitrate concentration causes the coating to grow slowly and be thinner, which is prone to unevenness, thereby reducing the electromagnetic shielding effect. Although a higher silver nitrate concentration can accelerate the growth of the coating and make the coating reach the desired thickness faster, too high a concentration will cause the coating to be locally too thick, making the coating uneven and even causing dendritic crystals, affecting the appearance and quality. Therefore, selecting a silver nitrate solution of appropriate concentration will help form a coating with good bonding strength, ensure that the coating is evenly adsorbed and deposited on the substrate, enhance the adhesion between the coating and the substrate, and improve the electromagnetic shielding effect.

[0123] It can be seen from Examples 7-9 that with the increase of citric acid concentration, the electromagnetic shielding effect first increases and then decreases. This is because citric acid acts as a reducing agent in the silver plating process and can control the stability of silver ions. If the concentration is too high, the silver ions will be deposited unevenly on the surface of the staple fibers. The uneven thickness of the coating will affect the integrity and continuity of the coating, thereby reducing the electromagnetic shielding effectiveness. In addition, since chitosan will cross-link with citric acid, the degree of cross-linking of the modified nylon silver-plated staple fibers will increase, and the mechanical properties of the material will be further enhanced. However, when the citric acid concentration is too high, the polymer network will be too tight, making the nylon staple fibers fragile and the mechanical properties will decrease.

[0124] It can be seen from Examples 9-11 that with the continuous change of the content of modified nylon staple fibers, the mechanical properties and electromagnetic shielding effects of the nylon silver-plated staple fibers continue to change. This is because the increase in the content of modified nylon staple fibers is equivalent to an increase in the solid-liquid ratio of modified nylon staple fibers to silver nitrate solution. An excessively high solid-liquid ratio makes the silver ion concentration in the solution insufficient to completely cover the fibers, resulting in a thin and incomplete coating, affecting the electromagnetic shielding effect of the coating. For an excessively low solid-liquid ratio, the concentration of silver ions in the solution is relatively high, resulting in a thick and uneven coating, and even the formation of a dendritic structure, which greatly reduces the density and adhesion of the silver coating. Therefore, an appropriate solid-liquid ratio helps to control the expected thickness of the silver coating to ensure that it is neither too thick nor too thin.

[0125] According to the above test experiments, the nylon silver-plated staple fiber with electromagnetic shielding prepared according to Example 6 has the best performance, so Example 6 is taken as the best embodiment;

[0126] By comparing Example 6 with Comparative Examples 1-6, it can be seen that:

[0127] In comparative example 1, unmodified nylon staple fibers were used for silver plating, and the electromagnetic shielding performance of the prepared nylon silver-plated staple fibers with electromagnetic shielding was significantly reduced. The unmodified nylon staple fibers have a relatively smooth surface and lack sufficient roughness, which is not conducive to the physical adhesion of the metal silver plating, that is, the mechanical bite between the plating and the surface of the nylon staple fibers is insufficient, resulting in the plating being easy to fall off. In addition, the surface chemical properties of the unmodified nylon staple fibers are relatively stable, and the chemical reaction activity with the metal silver ions and reducing agents in the silver plating solution is relatively low, which affects the deposition efficiency of silver ions on the fiber surface and the quality of the plating. In addition, nylon is a hydrophilic fiber with polar groups such as amino and carboxyl groups on the surface, which makes its surface energy relatively high. This characteristic easily leads to nonspecific adsorption of the surface, affecting the uniformity of the silver plating layer, and thus the electromagnetic shielding effect is greatly reduced. It is also because the silver plating layer is not dense and uniform enough, and there are pores and cracks. These defects will become stress concentration points, resulting in a significant reduction in mechanical properties.

[0128] In Comparative Example 2, only chitosan was used to modify the nylon staple fiber, and the electromagnetic shielding performance of the prepared nylon silver-plated staple fiber with electromagnetic shielding was significantly reduced. This is because chitosan itself is non-conductive, while nano-zirconium carbide has a certain conductivity. Therefore, compared with the modified nylon silver-plated staple fiber, its electromagnetic shielding performance is worse. In addition, because nano-zirconium carbide has high rigidity and high modulus, it can significantly enhance the mechanical properties of the composite material. Therefore, the use of chitosan alone cannot enhance the mechanical properties of the nylon staple fiber. Therefore, nylon staple fibers modified with chitosan and nano-zirconium carbide particles should be used.

[0129] In Comparative Example 3, only nano-zirconium carbide particles are used to modify the nylon staple fiber, and the electromagnetic shielding performance of the prepared nylon silver-plated staple fiber with electromagnetic shielding is poor. This is because chitosan, as a natural polymer, can form a uniform film, which helps to improve the uniformity and density of the coating, while the nano-zirconium carbide particles cannot independently provide such a uniform base, which may cause the silver coating to become uneven, resulting in poor electromagnetic shielding performance. At the same time, only nano-zirconium carbide particles are used to modify the nylon staple fiber. Due to the high hardness of the nanoparticles, stress concentration points will be formed on the fiber surface. At this time, external forces will cause early formation and expansion of cracks, thereby reducing the mechanical properties of the material. Therefore, nylon staple fibers modified synergistically with chitosan and nano-zirconium carbide particles should be used.

[0130] In Comparative Example 4, polyethyleneimine was used to modify the nylon staple fiber, replacing chitosan. The performance of the prepared nylon silver-plated staple fiber with electromagnetic shielding deteriorated. This is because although polyethyleneimine can provide similar surface activity and metal ion complexing ability as chitosan, which helps to improve the adhesion and uniformity of the coating, the high molecular weight of polyethyleneimine makes it difficult to disperse evenly on the fiber surface, thereby affecting the coating effect.

[0131] In Comparative Example 5, no sodium adipate inhibitor is added, and the performance of the prepared nylon silver-plated staple fiber with electromagnetic shielding deteriorates. This is because the sodium adipate inhibitor can slow down the growth rate of the coating, make the coating more uniform, prevent the formation of a dendritic structure caused by excessive growth of the coating, refine the coating structure, reduce the pores in the coating, thereby improving the density, adhesion and uniformity of the coating, and further improving the electromagnetic shielding performance of the coating. In the absence of the inhibitor, the coating grows too fast, resulting in uneven coating, and thus poor performance.

[0132] In Comparative Example 6, no succinate sulfonate wetting agent is added, and the performance of the prepared nylon silver-plated staple fiber with electromagnetic shielding becomes worse. This is because the succinate sulfonate wetting agent can reduce the surface tension of water, improve the wettability of the plating solution to the fiber surface, reduce bubbles and pores in the coating, and enable the plating solution to spread better on the fiber surface, thereby improving the uniformity and continuity of the coating. In the absence of a wetting agent, the coating will be discontinuous, forming voids or weak areas, which will affect the conductivity and electromagnetic shielding performance of the coating.

[0133] In summary, by modifying nylon staple fibers with chitosan and nano-zirconium carbide particles, chitosan and nano-zirconium carbide work synergistically to promote the conductivity of nylon silver-plated staple fibers on the one hand, and improve the adhesion of silver plating on the other hand. At the same time, wetting agents are added to reduce bubbles and voids, and inhibitors slow down the silver ion plating rate and promote the uniformity of silver plating, thereby improving the electromagnetic shielding properties and mechanical properties of nylon silver-plated staple fibers.

[0134] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments, and the above embodiments and descriptions are only preferred examples of the present invention, and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A nylon silver-plated staple fiber with electromagnetic shielding, Features: The invention comprises the following components: 1-3 parts by weight of modified nylon staple fiber, 1.5-3 parts by weight of silver nitrate, 0.2-1 parts by weight of sodium citrate, 0.01-0.05 parts by weight of succinate sulfonate wetting agent and 0.05-0.1 parts by weight of sodium adipate inhibitor; Among them, the modified nylon staple fiber is made of chitosan and nano zirconium carbide particles. The preparation method of the modified nylon staple fiber is as follows: S1.

1. Use ethanol solvent to clean the nylon staple fibers to remove grease and impurities on the surface, and dry them in an oven at 60-80℃; S1.2, using dilute acetic acid as solvent, weigh chitosan to prepare a solution, heat and stir at 60-80°C for 2-3h until completely dissolved; S1.3, weigh a certain amount of nano zirconium carbide particles, use the chitosan solution as a dispersion medium, add the nano zirconium carbide particles to the chitosan solution, and use an ultrasonic instrument to disperse the nano zirconium carbide particles in the medium to obtain a mixed solution of chitosan and nano zirconium carbide; S1.4, immerse the pretreated nylon staple fibers into the mixed solution at room temperature for 20-30 minutes, take out the fibers and place them at 1-2 kg / cm 2 Under the pressure of , dipping and rolling, and finally drying at 50-60℃ for 1-1.5h to obtain modified nylon staple fiber; The chitosan is prepared into a solution with a mass fraction of 1-5% by dilute acetic acid, wherein the mass fraction of the dilute acetic acid is 0.8-1%; the nano zirconium carbide particles account for 5-7% of the total mass of the chitosan solution.

2. The nylon silver-plated staple fiber with electromagnetic shielding according to claim 1, Features: The frequency range of the ultrasonic instrument is 20-40kHz, and the ultrasonic time is 20-30min.

3. A method for preparing a nylon silver-plated staple fiber with electromagnetic shielding, used for preparing a nylon silver-plated staple fiber with electromagnetic shielding as claimed in any one of claims 1 to 2, Features: The steps include: 1-3 parts by weight of modified nylon staple fibers are placed in a silver nitrate solution, a sodium adipate inhibitor and a succinate sulfonate wetting agent are added to the silver nitrate solution, the mixture is stirred evenly, a citric acid solution is added and the pH value is adjusted, the mixture is immersed and reacted at 30-50°C for 50-60 minutes, the surface precipitate is finally cleaned, and the mixture is dried at 60-80°C to obtain a nylon silver-plated staple fiber with electromagnetic shielding. The silver nitrate solution is prepared by silver nitrate and deionized water in a mass ratio of 1:95-100; and the citric acid solution is prepared by sodium citrate and deionized water in a mass ratio of 1:50-55.

4. The method for preparing the nylon silver-plated staple fiber with electromagnetic shielding according to claim 3, Features: The pH value was adjusted to 5-6 by citric acid solution.

Citation Information

Patent Citations

  • Method for preparing nano alumina particles composite silver coating on surface of nylon fabric

    CN101876146A

  • Sensitization-free and activation-free chemical silvering method for polyamide base body

    CN104032564A

  • Method for chemical silver-plating of aramid conductive fibers

    CN104532553A

  • Nano silver in-situ formation silver-plating method based on plasma modification and silver-plated fabric

    CN104988720A

  • Zirconium carbide modified cloth and preparation method and application thereof

    CN112553888A