A back contact battery with improved back passivation effect and its preparation method and application
By setting the conductive film layer and alumina layer in the back contact battery and setting the silicon oxide and alumina passivation layers on the front, the opening structure is optimized, and the problem of low current density caused by the transparent conductive film layer on the back is solved, which improves the Battery filling factor and conversion efficiency.
Patent Information
- Application Number
- CN202411140292.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The transparent conductive film layer on the back of the existing back contact battery results in a low current density, failing to fully absorb the long wavelength of the front and incident light on the back, affecting the conversion efficiency of the battery.
The first and second semiconductor layers are alternately arranged on the back of the silicon wafer, and a conductive film layer is laid on its outer surface, combined with the alumina layer, forming an isolation groove, controlling the refractive index and thickness ratio of the alumina layer and the conductive film layer, and increasing the back surface The passivation effect is provided on the front, and the silicon oxide and aluminum oxide passivation layer are provided on the front, optimizing the opening structure to improve the electrode contact effect.
The passivation effect of the back semiconductor layer and the filling factor of the battery are significantly improved, and the current density and battery conversion efficiency are improved.
Smart Images

Figure CN118658902B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of back contact batteries, and in particular relates to a back contact battery with improved back passivation effect, and a preparation method and application thereof. Background Art
[0002] In the existing back contact battery, the first semiconductor layer and the second semiconductor layer are alternately arranged on the back side of the silicon wafer, and also include a front passivation layer and an anti-reflection layer sequentially arranged on the front side of the silicon wafer.
[0003] However, the anti-reflection layer on the back is generally only deposited with a transparent conductive film layer. The refractive index of the transparent conductive film layer, such as the ITO layer, is 1.8-1.9. The incident infrared light on the front and the scattered light on the back are generally not fully absorbed, resulting in a certain impact on the current density and a low current density of the battery.
[0004] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention
[0005] The purpose of the present invention is to overcome the defect of the prior art that the anti-reflection layer on the back side of the back-contact battery adopts a transparent conductive film layer but has a low current density, and to provide a back-contact battery with improved back passivation effect and a preparation method and application thereof, which can increase the absorption of long wavelength light on the front side and incident light on the back side, and increase the passivation effect of the back semiconductor layer; while improving the passivation effect, it is also beneficial to improve the fill factor of the battery, and improve the current density and conversion efficiency of the battery.
[0006] In order to achieve the above-mentioned purpose, in a first aspect, the present invention provides a back-contact battery with improved back-side passivation effect, comprising a silicon wafer, a front passivation layer and an anti-reflection layer sequentially arranged on the front side of the silicon wafer, a first semiconductor layer and a second semiconductor layer alternately arranged on the back side of the silicon wafer, a conductive film layer laid on the outer surfaces of the first semiconductor layer and the second semiconductor layer, and a metal electrode; the two ends of the second semiconductor layer respectively extend outward to the outside of the partial back side covering the adjacent first semiconductor layer, and a first semiconductor opening area not covering the second semiconductor layer is opened on the back side of the first semiconductor layer, a second semiconductor opening area is formed between the adjacent first semiconductor layers, the second semiconductor opening area is arranged at intervals from the first semiconductor opening area, and the corresponding semiconductor area therebetween is an overlapping area, and an isolation groove is opened on the portion of the conductive film layer located in the overlapping area; the metal electrode is arranged in the second The semiconductor opening region and the first semiconductor opening region each correspond to the outer surface of the conductive film layer; it also includes an aluminum oxide layer arranged on the outer surface of the conductive film layer, the isolation groove penetrates the aluminum oxide layer, and a first opening is opened on the portion of the aluminum oxide layer corresponding to the first semiconductor opening region, and a second opening is opened on the portion of the aluminum oxide layer corresponding to the second semiconductor opening region, the first opening and the second opening are for the metal electrode to contact the conductive film layer; wherein, the refractive index of the aluminum oxide layer is 1.5-1.7, the thickness of the aluminum oxide layer is 30-50nm, the refractive index of the conductive film layer is 1.8-1.9, and the thickness ratio of the aluminum oxide layer to the conductive film layer is 1: (1.0-2.6); and the front passivation layer comprises a combination of a silicon oxide passivation layer and an aluminum oxide passivation layer arranged in sequence from the front side of the silicon wafer to the outside, and the thickness ratio of the aluminum oxide passivation layer to the aluminum oxide layer is 1: (6-17).
[0007] In some preferred embodiments of the present invention, the thickness of the conductive film layer is 40-80 nm.
[0008] In some preferred embodiments of the present invention, the ratio of the width W31 of the first opening to the width W1 of the first semiconductor opening region is 1:(1.0-1.8), and / or the ratio of the width W32 of the second opening to the width W2 of the second semiconductor opening region is 1:(1.2-2.0).
[0009] In some preferred embodiments of the present invention, the width W31 of the first opening is 130-230 μm, and / or the width W32 of the second opening is 250-400 μm.
[0010] In some preferred embodiments of the present invention, the width W1 of the first semiconductor opening region is 200-300 μm, and / or the width W2 of the second semiconductor opening region is 400-550 μm.
[0011] In some preferred embodiments of the present invention, the first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer, and the second semiconductor layer is a stack including an intrinsic hydrogenated amorphous silicon layer and a second doped silicon layer or a stack including a second tunneling oxide layer and a second doped polysilicon layer.
[0012] In some preferred embodiments of the present invention, the silicon wafer front side and the silicon wafer region corresponding to the second semiconductor opening region are both texturing regions, and the silicon wafer region corresponding to the first semiconductor opening region is a polishing region.
[0013] In some preferred embodiments of the present invention, the thickness of the silicon oxide passivation layer is 1-2 nm, and the thickness of the aluminum oxide passivation layer is 3-4 nm.
[0014] In some preferred embodiments of the present invention, the anti-reflection layer is a combination of a silicon nitride layer and a silicon oxide layer sequentially arranged from the front side of the silicon wafer outward, the thickness of the silicon nitride layer is 50-100 nm, and the thickness of the silicon oxide layer is 80-150 nm.
[0015] In a second aspect, the present invention provides a method for preparing a back contact battery with improved back passivation effect, comprising the following steps:
[0016] S1, provide double-sided polished silicon wafers;
[0017] S2, forming a first semiconductor layer and an isolation layer in sequence on the back side of the silicon wafer;
[0018] S3, performing a first etching opening on the back surface obtained in S2 to form a second semiconductor opening region;
[0019] S4, then performing texturing cleaning, and then selecting whether to perform a step of removing the isolation layer outside the second semiconductor opening area on the back side of the silicon wafer through cleaning according to needs;
[0020] S5, depositing a second semiconductor layer on the back surface obtained in S4;
[0021] S6, forming a front passivation layer and an anti-reflection layer in sequence on the front side of the silicon wafer, wherein the front passivation layer comprises a combination of a silicon oxide passivation layer and an aluminum oxide passivation layer which are sequentially arranged from the front side of the silicon wafer outward;
[0022] S7, performing a second etching opening on a portion of the second semiconductor layer on the back side of the silicon wafer to form a first semiconductor opening region spaced apart from the second semiconductor opening region;
[0023] S8, depositing a conductive film layer on the back surface obtained in S7, and controlling the refractive index of the conductive film layer to be 1.8-1.9;
[0024] S9, depositing an aluminum oxide layer on the outer surface of the back conductive film layer, controlling the refractive index of the aluminum oxide layer to be 1.5-1.7, the thickness of the aluminum oxide layer to be 30-50 nm, the thickness ratio of the aluminum oxide layer to the conductive film layer to be 1:(1.0-2.6), and the thickness ratio of the aluminum oxide passivation layer to the aluminum oxide layer to be 1:(6-17);
[0025] S10, using a laser to remove a portion of the aluminum oxide layer corresponding to the first semiconductor opening region to form a first opening, and simultaneously removing a portion of the aluminum oxide layer corresponding to the second semiconductor opening region to form a second opening, wherein the first opening and the second opening expose the conductive film layers corresponding to the corresponding semiconductor opening regions;
[0026] and performing a third etching opening on a portion of the conductive film layer and its corresponding aluminum oxide layer located between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove;
[0027] S11, forming metal electrodes on the outer surfaces of the corresponding exposed conductive film layers in the areas where the first semiconductor opening region and the second semiconductor opening region are located.
[0028] In some preferred embodiments of the present invention, the aluminum oxide layer in S9 is deposited by an atomic layer deposition method, and the conditions of the atomic layer deposition method include: the process temperature is between 150-300°C; the reaction gases are trimethylaluminum and ozone, and the flow rate of trimethylaluminum introduced in the first stage is 3000sccm-8000sccm, the reaction time is 20-40s, and then nitrogen is used to purge the chamber and pipelines; then the second stage is carried out, and the flow rate of ozone introduced in the second stage is 3000sccm-6000sccm, the ozone introduction time is 15-30s, and then nitrogen is used to purge the chamber and pipelines; the first stage and the second stage are carried out in sequence as a cycle reaction, and a total of 100-200 cycle reactions are carried out.
[0029] In some preferred embodiments of the present invention, the laser used to remove part of the aluminum oxide layer in S10 is a flat-top picosecond green laser or a flat-top picosecond ultraviolet laser, and the power of the laser is 20kW-100kW and the frequency is 200kHZ-1000kHZ.
[0030] In a third aspect, the present invention provides a back-contact battery with improved back-side passivation effect, which is prepared by the preparation method of a back-contact battery with improved back-side passivation effect described in the second aspect.
[0031] In a fourth aspect, the present invention provides a photovoltaic module, which includes the back contact cell for improving back passivation effect as described in the first aspect, or includes the back contact cell for improving back passivation effect as described in the third aspect.
[0032] Beneficial effects:
[0033] The present invention adopts the above technical scheme, especially superimposing a passivation layer of aluminum oxide on the outer surface of the back conductive film layer. The aluminum oxide layer not only has the chemical passivation effect of passivating the dangling bonds, but also can provide an effective fixed charge enhanced field passivation effect, and the refractive index of the aluminum oxide layer is controlled to be 1.5-1.7, and the conductive film layer (refractive index is 1.8-1.9) forms an anti-reflection effect in which the refractive index gradually decreases from the inside to the outside, and the thickness ratio of the aluminum oxide layer to the conductive film layer is controlled in an appropriate range, which is conducive to forming an effective and significant anti-reflection effect on the back, which can increase the absorption of the front long wavelength and the incident light on the back, and can increase the passivation effect of the semiconductor layer on the back; and the aluminum oxide passivation layer on the front can further enhance the passivation effect, which is conducive to improving the conversion efficiency of the battery. Among them, controlling the thickness ratio of the aluminum oxide passivation layer to the aluminum oxide layer in an appropriate range is conducive to improving the passivation effect while achieving the best anti-reflection effect on both the front and back sides, and maximizing the current density of the battery.
[0034] In the preferred embodiment of the present invention, controlling the corresponding opening width ratio of the two semiconductor opening areas and the aluminum oxide layer is more conducive to improving the passivation effect while ensuring sufficient contact between the metal electrode and the conductive film layer, which is further beneficial to improving the battery's fill factor, current density and battery conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0036] Figure 1 It is a structural schematic diagram of a specific implementation mode of a back contact battery for improving the back passivation effect of the present invention.
[0037] Description of Reference Numerals
[0038] Silicon wafer 1, first tunneling silicon oxide layer 2, N-type doped polysilicon layer 3, second tunneling silicon oxide layer 5, P-type doped polysilicon layer 6, front passivation layer 7, silicon oxide passivation layer 7.1, aluminum oxide passivation layer 7.2, anti-reflection layer 8, transparent conductive film layer 9, aluminum oxide layer 10, metal electrode 11. DETAILED DESCRIPTION
[0039] In the present invention, unless otherwise specified, directional words such as "up, down, left, right" are generally understood in combination with the directions shown in the drawings and actual applications.
[0040] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0041] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0042] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).
[0043] In the present invention, the area close to the silicon wafer is referred to as the inside, and the area far from the silicon wafer is referred to as the outside.
[0044] In the present invention, the refractive index is obtained by testing with an ellipsometer at a corresponding film thickness.
[0045] In a first aspect, the present invention provides a back-contact battery for improving the back passivation effect, comprising a silicon wafer, a front passivation layer and an anti-reflection layer sequentially arranged on the front side of the silicon wafer, a first semiconductor layer and a second semiconductor layer alternately arranged on the back side of the silicon wafer, a conductive film layer laid on the outer surfaces of the first semiconductor layer and the second semiconductor layer, and a metal electrode; the two ends of the second semiconductor layer respectively extend outward to the outside of the partial back side covering the adjacent first semiconductor layer, and a first semiconductor opening area not covering the second semiconductor layer is opened on the back side of the first semiconductor layer, a second semiconductor opening area is formed between adjacent first semiconductor layers, the second semiconductor opening area is arranged at intervals with the first semiconductor opening area, and the corresponding semiconductor area therebetween is an overlapping area, an isolation groove is opened on the part of the conductive film layer located in the overlapping area; the metal electrode is arranged on the outer surface of the conductive film layer corresponding to each of the second semiconductor opening area and the first semiconductor opening area; and also includes an aluminum oxide layer arranged on the outer surface of the conductive film layer, the isolation groove penetrates the aluminum oxide layer, and a first opening is opened on the part of the aluminum oxide layer corresponding to the first semiconductor opening area, and a second opening is opened on the part of the aluminum oxide layer corresponding to the second semiconductor opening area, the first opening and the second opening are for the metal electrode to contact the conductive film layer.
[0046] Among them, the refractive index of the aluminum oxide layer is 1.5-1.7, the thickness of the aluminum oxide layer is 30-50nm, preferably 35-50nm, the refractive index of the conductive film layer is 1.8-1.9, the thickness ratio of the aluminum oxide layer to the conductive film layer is 1: (1.0-2.6), preferably 1: (1.0-2.0), and further preferably 1: (1.2-2.0); and the front passivation layer comprises a combination of a silicon oxide passivation layer and an aluminum oxide passivation layer arranged in sequence from the front of the silicon wafer to the outside, and the thickness ratio of the aluminum oxide passivation layer to the aluminum oxide layer is 1: (6-17), preferably 1: (8-17). The scheme of using this specific correlation parameter to cooperate with each other can increase the absorption of the front long wavelength and the back incident light, and can also increase the passivation effect of the back semiconductor layer; while improving the passivation effect, it can effectively improve the fill factor of the battery, improve the current density and battery conversion efficiency.
[0047] The thickness ratio of the aluminum oxide layer to the conductive film layer is 1:(1.0-2.6), for example, it can be 1:1, 1:1.3, 1:1.5, 1:2, 1:2.2, 1:2.5, 1:2.6, etc., and the range between any two point values.
[0048] The thickness of the aluminum oxide layer is 30-50 nm, for example, it can be 30, 33, 35, 38, 40, 42, 45, 48, 49, 50, etc. and the range between any two point values.
[0049] In some preferred embodiments of the present invention, the thickness of the conductive film layer is 40-80 nm.
[0050] The present invention uses an aluminum oxide layer and a conductive film layer of suitable thickness, which is more conducive to forming an effective anti-reflection effect on the back side, can increase the absorption of long wavelength light on the front side and incident light on the back side, and can increase the passivation effect of the back semiconductor layer.
[0051] The conductive film layer is preferably a transparent conductive film layer. Further preferably, the material of the transparent conductive film layer can be an indium oxide-based film doped with at least one of tin, tungsten, titanium, zinc, and gallium, or a zinc oxide-based film doped with at least one of aluminum, gallium, and boron.
[0052] In some preferred embodiments of the present invention, the ratio of the width W31 of the first opening to the width W1 of the first semiconductor opening region is 1: (1.0-1.8), preferably 1: (1.2-1.8), and / or the ratio of the width W32 of the second opening to the width W2 of the second semiconductor opening region is 1: (1.2-2.0), preferably 1: (1.4-2.0). The use of the first opening and the second opening with a suitable width ratio is more conducive to full contact between the metal electrode and the conductive film layer, ensuring the conductivity performance of the battery and the stability of the process.
[0053] The ratio of the width W31 of the first opening to the width W1 of the first semiconductor opening region is 1:(1.0-1.8), for example, it can be 1:1.0, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, etc. and the range between any two point values.
[0054] The ratio of the width W32 of the second opening to the width W2 of the second semiconductor opening region is 1:(1.2-2.0), for example, it can be 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:2.0, etc. and the range between any two point values.
[0055] In some preferred embodiments of the present invention, the width W31 of the first opening is 130-230 μm, preferably 130-220 μm, and / or the width W32 of the second opening is 250-400 μm. In the art, the width of the metal electrode fine grid is generally 30-60 μm, which is much smaller than the width of the first opening and the second opening. The metal electrode fine grid is generally printed in the middle of the opening width, and a slight deviation has little effect. The use of the first opening and the second opening of appropriate width can reduce the requirements for laser engraving accuracy and printing alignment accuracy, and is easier to control in the process, ensuring that the printed metal electrode fine grid is printed on the opening to prevent it from being biased onto the aluminum oxide, which is beneficial to improving the conductivity and the fill factor FF.
[0056] In some preferred embodiments of the present invention, the width W1 of the first semiconductor opening region is 200-300 μm, and / or the width W2 of the second semiconductor opening region is 400-550 μm.
[0057] Preferably, in the present invention, the width W3 of the isolation groove is 20-100 μm.
[0058] In some preferred embodiments of the present invention, the first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer, and the second semiconductor layer is a stack including an intrinsic hydrogenated amorphous silicon layer and a second doped silicon layer or a stack including a second tunneling oxide layer and a second doped polysilicon layer.
[0059] The thickness and corresponding doping concentration of the first tunneling oxide layer, the second tunneling oxide layer or the intrinsic hydrogenated amorphous silicon layer, the first doped polysilicon layer and the second doped silicon layer, and the second doped polysilicon layer of the present invention can refer to the range of the prior art, and can be used in the present invention. Exemplarily, the thickness of the first tunneling oxide layer and the second tunneling oxide layer is independently 1-2nm, and the thickness of the intrinsic hydrogenated amorphous silicon layer is 5-15nm; the thickness of the second doped silicon layer is 7-20nm, and the thickness of the second doped polysilicon layer is 60-100nm, and the effective doping concentration of the second doped silicon layer and the second doped polysilicon layer is independently 1e18cm -3 -9e19cm -3 The thickness of the first doped polysilicon layer is 70-120nm, and the effective doping concentration is greater than 1e19cm -3 The second doped silicon layer may be doped amorphous or doped microcrystalline.
[0060] In some specific embodiments, the first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer, and the second semiconductor layer is a stacked layer including an intrinsic hydrogenated amorphous silicon layer and a second doped silicon layer. The use of a combined passivation structure and a specific aluminum oxide layer is more conducive to improving the passivation effect and the open circuit voltage.
[0061] In some more preferred embodiments, the first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer, and the second semiconductor layer is a stacked layer including a second tunneling oxide layer and a second doped polysilicon layer. With this preferred passivation structure, since the second semiconductor layer uses a polycrystalline P layer, its crystallinity is improved and its conductivity is increased compared to the amorphous silicon P layer, which can further effectively reduce the series resistance; with a specific aluminum oxide layer, it is more conducive to improving the conductivity of the battery and improving the fill factor.
[0062] The above two passivation structures of the present invention have good corrosion resistance and will not be damaged by laser or solution grooving in the subsequent preparation process (such as side etching damage in strong alkali and strong acid in texturing), and the process stability is good.
[0063] In some preferred embodiments of the present invention, the silicon wafer front side and the silicon wafer region corresponding to the second semiconductor opening region are both texturing regions, and the silicon wafer region corresponding to the first semiconductor opening region is a polishing region.
[0064] Preferably, in the present invention, the thickness of the silicon oxide passivation layer is 1-2 nm, and the thickness of the aluminum oxide passivation layer is 3-4 nm.
[0065] The anti-reflection layer can be one or a combination of a silicon nitride layer, an aluminum oxide layer and a silicon oxide layer. In some preferred embodiments of the present invention, the anti-reflection layer is a combination of a silicon nitride layer and a silicon oxide layer sequentially arranged from the front side of the silicon wafer outward, the thickness of the silicon nitride layer is 50-100nm, and the thickness of the silicon oxide layer is 80-150nm.
[0066] In the present invention, in the overlapping region, an isolation layer is provided between the first semiconductor layer and the second semiconductor layer, or no isolation layer is provided.
[0067] The type and thickness of the isolation layer can refer to the prior art, for example, the type can be at least one of silicon nitride, silicon oxide, silicon oxynitride or nitrogen-containing polysilicon, preferably silicon nitride. The thickness of the isolation layer can be, for example, 40-90 nm.
[0068] In a second aspect, the present invention provides a method for preparing a back contact battery with improved back passivation effect, comprising the following steps:
[0069] S1, provide double-sided polished silicon wafers;
[0070] S2, forming a first semiconductor layer and an isolation layer in sequence on the back side of the silicon wafer;
[0071] S3, performing a first etching opening on the back surface obtained in S2 to form a second semiconductor opening region;
[0072] S4, then performing texturing cleaning, and then selecting whether to perform a step of removing the isolation layer outside the second semiconductor opening area on the back side of the silicon wafer through cleaning according to needs;
[0073] S5, depositing a second semiconductor layer on the back surface obtained in S4;
[0074] S6, forming a front passivation layer and an anti-reflection layer in sequence on the front side of the silicon wafer, wherein the front passivation layer comprises a combination of a silicon oxide passivation layer and an aluminum oxide passivation layer which are sequentially arranged from the front side of the silicon wafer outward;
[0075] S7, performing a second etching opening on a portion of the second semiconductor layer on the back side of the silicon wafer to form a first semiconductor opening region spaced apart from the second semiconductor opening region;
[0076] S8, depositing a conductive film layer on the back surface obtained in S7, and controlling the refractive index of the conductive film layer to be 1.8-1.9;
[0077] S9, depositing an aluminum oxide layer on the outer surface of the back conductive film layer, controlling the refractive index of the aluminum oxide layer to be 1.5-1.7, the thickness of the aluminum oxide layer to be 30-50 nm, the thickness ratio of the aluminum oxide layer to the conductive film layer to be 1:(1.0-2.6), and the thickness ratio of the aluminum oxide passivation layer to the aluminum oxide layer to be 1:(6-17);
[0078] S10, using a laser to remove a portion of the aluminum oxide layer corresponding to the first semiconductor opening region to form a first opening, and simultaneously removing a portion of the aluminum oxide layer corresponding to the second semiconductor opening region to form a second opening, wherein the first opening and the second opening expose the conductive film layers corresponding to the corresponding semiconductor opening regions;
[0079] and performing a third etching opening on a portion of the conductive film layer and its corresponding aluminum oxide layer located between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove;
[0080] S11, forming metal electrodes on the outer surfaces of the corresponding exposed conductive film layers in the areas where the first semiconductor opening region and the second semiconductor opening region are located.
[0081] It can be understood that the S4 texturing cleaning of the present invention can remove the residual isolation layer and the first semiconductor layer in the second semiconductor opening area, and at the same time form a texturing surface on the front side of the silicon wafer and the second semiconductor opening area.
[0082] In some preferred embodiments of the present invention, the aluminum oxide layer in S9 is deposited by an atomic layer deposition method, and the conditions of the atomic layer deposition method include: a process temperature between 150-300°C, for example, 150°C, 180°C, 200°C, 230°C, 250°C, 270°C, 300°C, etc. and a range between any two point values. Using a lower process temperature to deposit the aluminum oxide layer is more conducive to ensuring the passivation effect and light transmittance of the film layer.
[0083] In some preferred embodiments of the present invention, the aluminum oxide layer in S9 is deposited by an atomic layer deposition method, and the conditions of the atomic layer deposition method include: the reaction gases are trimethylaluminum and ozone, the flow rate of trimethylaluminum introduced in the first stage is 3000sccm-8000sccm, the reaction time is 20-40s, and then the chamber and pipeline are purged with nitrogen; then the second stage is carried out, the flow rate of ozone introduced in the second stage is 3000sccm-6000sccm, the ozone introduction time is 15-30s, and then the chamber and pipeline are purged with nitrogen; the first stage and the second stage are carried out in sequence as a cycle reaction, and a total of 100-200 cycle reactions are carried out. Using a suitable deposition process to deposit the aluminum oxide layer is more conducive to improving the density of the film layer and improving the passivation performance of the film layer.
[0084] The third etching opening of the isolation groove of the present invention is performed by laser.
[0085] In some preferred embodiments of the present invention, the laser used to remove part of the aluminum oxide layer in S10 is a flat-top picosecond green laser (wavelength 532 nm) or a flat-top picosecond ultraviolet laser (355 nm).
[0086] More preferably, the power of the laser is 20kW-100kW, and the frequency is 200kHZ-1000kHZ. Using appropriate laser parameters is more conducive to avoiding laser damage to the bottom film layer and ensuring the quality of the film layer.
[0087] In a third aspect, the present invention provides a back-contact battery with improved back-side passivation effect, which is prepared by the preparation method of a back-contact battery with improved back-side passivation effect described in the second aspect.
[0088] In a fourth aspect, the present invention provides a photovoltaic module, which includes the back contact cell for improving back passivation effect as described in the first aspect, or includes the back contact cell for improving back passivation effect as described in the third aspect.
[0089] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0090] Example 1
[0091] A back contact cell with improved back passivation effect, such as Figure 1 As shown, it is prepared by the following preparation method:
[0092] S1, double-sided polishing of silicon wafer 1:
[0093] S2, forming a first semiconductor layer and an isolation layer on the back side of the silicon wafer 1:
[0094] The first semiconductor layer comprises a first tunneling silicon oxide layer 2 and an N-type doped polysilicon layer 3. The isolation layer is silicon nitride. The first tunneling silicon oxide layer 2 has a thickness of 1.5 nm, the N-type doped polysilicon layer 3 has a thickness of 100 nm, and an effective doping concentration of 3e20 cm -3 , the thickness of the isolation layer is 70nm.
[0095] S3, etching an opening on the back side of the silicon wafer 1 for the first time to form a second semiconductor opening region; the width W2 of the formed second semiconductor opening region is 500 μm.
[0096] S4, texturing and cleaning the opening areas on the front and back of the silicon wafer 1:
[0097] The front and back opening areas of the silicon wafer 1 are subjected to texturing and cleaning. During the texturing process on the front side, the silicon nitride isolation layer on the back side of the silicon wafer 1 is also removed by the final cleaning solution.
[0098] S5, forming a second semiconductor layer on the back side of the silicon wafer 1;
[0099] The second semiconductor layer is a second tunneling silicon oxide layer 5 (1 nm thick) and a P-type doped polysilicon layer 6 (80 nm thick, with an effective doping concentration of 2e19 cm -3 ) stack.
[0100] S6, forming a front passivation layer 7 and an anti-reflection layer 8 on the front side of the silicon wafer 1:
[0101] The front passivation layer 7 is a combination of a silicon oxide passivation layer 7.1 and an aluminum oxide passivation layer 7.2. The thickness of the silicon oxide passivation layer 7.1 is 1.2 nm, and the thickness of the aluminum oxide passivation layer 7.2 is 4 nm.
[0102] The anti-reflection layer 8 is a combination of a silicon nitride layer and a silicon oxide layer, the thickness of the silicon nitride layer is 70 nm, and the thickness of the silicon oxide layer is 100 nm;
[0103] S7. Etching an opening on the back side of the silicon wafer 1 for the second time to form a first semiconductor opening region. The width W1 of the formed first semiconductor opening region is 230 μm.
[0104] S8. Deposit a transparent conductive film layer 9 on the back of the silicon wafer 1; the transparent conductive film layer 9 is a tin-doped indium oxide-based thin film ITO with a thickness of 70 nm.
[0105] S9, depositing an aluminum oxide layer 10 on the back side of the silicon wafer 1;
[0106] The aluminum oxide layer 10 is formed by an atomic layer deposition method, and the conditions of the atomic layer deposition method include: the process temperature is 180°C, the reaction gases are trimethylaluminum and ozone, the flow rate of trimethylaluminum in the first stage is 4000sccm, the reaction time is 30s, and then the chamber and pipeline are purged with nitrogen; then the second stage is carried out, the ozone flow rate in the second stage is 5000sccm, the ozone time is 20s, and then the chamber and pipeline are purged with nitrogen; the first stage and the second stage are carried out in sequence as a cycle reaction, and a total of 120 cycle reactions are carried out. The thickness of the aluminum oxide layer 10 is 40nm, and the refractive index of the aluminum oxide layer 10 is 1.67; the thickness ratio of the aluminum oxide layer 10 to the transparent conductive film layer 9 is 1:1.75, and controlling the thickness ratio of the two layers is conducive to forming an effective anti-reflection effect on the back.
[0107] S10, etching an opening for the third time on the back side of the silicon wafer 1, using a laser to remove a portion of the aluminum oxide layer 10 corresponding to the first semiconductor opening area to form a first opening, and simultaneously removing a portion of the aluminum oxide layer 10 corresponding to the second semiconductor opening area to form a second opening, the first opening and the second opening to expose the transparent conductive film layer 9 corresponding to the corresponding semiconductor opening area; and etching an opening on the corresponding transparent conductive film layer 9 and its corresponding aluminum oxide layer 10 in the overlapping area of the two semiconductor layers to form an isolation groove;
[0108] The purpose of removing the corresponding part of the aluminum oxide layer 10 on the two semiconductor opening regions is to expose the transparent conductive film layer 9 to contact the metal electrode 11, so as to facilitate the transmission of carriers. The aluminum oxide layer of the two semiconductor layers is removed by laser, and the laser is a flat-top picosecond green laser (wavelength 532nm), the power of the laser is 40kW, and the frequency is 400kHZ.
[0109] The widths of the first opening and the second opening satisfy: the ratio of the width W31 of the first opening to the width W1 of the first semiconductor opening region is 1:1.53, and the ratio of the width W32 of the second opening to the width W2 of the second semiconductor opening region is 1:1.80. W31 is 150 μm, and W32 is 278 μm;
[0110] The isolation groove process uses a laser method to etch an opening on the back of the silicon wafer 1 to form an isolation groove between the first semiconductor and the second semiconductor. The width W3 of the isolation groove is 80 μm, and the resistance between the first semiconductor and the second semiconductor after etching is greater than 1 kΩ.
[0111] S11 , metal electrodes 11 are formed on the outer surfaces of the exposed transparent conductive film layer 9 at the first semiconductor opening region and the second semiconductor opening region on the back side of the silicon wafer 1 .
[0112] Example 2
[0113] The method of Example 1 is followed, except that the thickness of the aluminum oxide layer is adjusted to 30 nm, so that the thickness ratio of the aluminum oxide layer to the conductive film layer is 1:2.3. The process parameters that need to be adjusted to meet the thickness adjustment are: reducing the number of cycle reactions by 25%.
[0114] Example 3
[0115] The method of Example 1 is referred to, except that the width W31 of the first opening is adjusted so that the ratio of W31 to the width W1 of the first semiconductor opening region is 1:1. The process parameters that need to be adjusted to meet the adjustment of the width W31 are: increasing the first opening width W31 to 230 μm.
[0116] Example 4
[0117] The method of Example 1 is referred to, except that the width W32 of the second opening is adjusted so that the ratio of W32 to the width W2 of the second semiconductor opening region is 1:1.25. The process parameters that need to be adjusted to meet the adjustment of the width W32 are: increasing the width W32 of the second opening to 400 μm.
[0118] Example 5
[0119] The method of Example 1 is followed, except that the second semiconductor layer is adjusted to be an intrinsic hydrogenated amorphous silicon layer (with a thickness of 10 nm) and a P-type doped amorphous silicon layer (with a thickness of 15 nm and an effective doping concentration of 2×10 19 cm -3 ) stack.
[0120] Comparative Example 1
[0121] The method of Example 1 is referred to, except that no aluminum oxide layer is provided.
[0122] Comparative Example 2
[0123] The method of Example 1 is referred to, except that the refractive index of the aluminum oxide layer is adjusted to 1.8, and the process parameters that need to be adjusted to meet the refractive index adjustment are: increasing the process temperature to 350°C.
[0124] Comparative Example 3
[0125] The method of Example 1 is referred to, except that the thickness of the aluminum oxide layer is adjusted to 80 nm, so that the thickness ratio of the aluminum oxide layer to the conductive film layer is 1:0.875. The process parameters that need to be adjusted to meet the thickness adjustment are: extending the number of cycle reactions by 1 times.
[0126] Comparative Example 4
[0127] The method of Example 1 is referred to, except that the thickness of the aluminum oxide passivation layer is adjusted so that the ratio of the thickness of the aluminum oxide passivation layer to the thickness of the aluminum oxide layer is 1:40.
[0128] Test Case
[0129] The back contact cells obtained in the above embodiments and comparative examples were subjected to performance tests, and the results are shown in Table 1. Among them, the performance indicators of each embodiment and comparative example were converted using embodiment 1 as a reference benchmark, the data of embodiment 1 is normalized benchmark 1, and other examples are converted based on embodiment 1, such as the battery conversion efficiency of comparative example 1 / battery conversion efficiency of embodiment 1 is 0.954. In the normalization process, the unit of current density is mA / cm², the unit of open circuit voltage is V, the unit of fill factor is %, and the unit of battery conversion efficiency is %.
[0130] Table 1
[0131]
[0132] It can be seen from the above results that, compared with the comparative example, the embodiment scheme of the present invention can increase the absorption of long wavelength light on the front side and incident light on the back side, and increase the passivation effect of the back semiconductor layer; while improving the passivation effect, it can effectively improve the fill factor of the battery, thereby improving the current density and battery conversion efficiency.
[0133] Furthermore, according to Example 1 and Examples 2-5, it can be seen that the preferred battery structure of the present invention is more conducive to improving the fill factor of the battery, and increasing the current density and battery conversion efficiency.
[0134] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A back contact cell for improving back passivation effect, comprising a silicon wafer, a front passivation layer and an anti-reflection layer sequentially arranged on the front side of the silicon wafer, a first semiconductor layer and a second semiconductor layer alternately arranged on the back side of the silicon wafer, a conductive film layer laid on the outer surfaces of the first semiconductor layer and the second semiconductor layer, and a metal electrode; the two ends of the second semiconductor layer respectively extend outward to the outside of the partial back side covering the adjacent first semiconductor layer, and a first semiconductor opening region not covering the second semiconductor layer is provided on the back side of the first semiconductor layer, a second semiconductor opening region is formed between adjacent first semiconductor layers, the second semiconductor opening region is arranged at intervals with the first semiconductor opening region, and the corresponding semiconductor region therebetween is a superposition region, and an isolation groove is provided on the portion of the conductive film layer located in the superposition region; the metal electrode is provided on the outer surfaces of the conductive film layers corresponding to the second semiconductor opening region and the first semiconductor opening region; the first semiconductor layer comprises a first tunneling oxide layer and a first doped polycrystalline silicon layer, and the second semiconductor layer is a stacked layer comprising an intrinsic hydrogenated amorphous silicon layer and a second doped silicon layer, or a stacked layer comprising a second tunneling oxide layer and a second doped polycrystalline silicon layer; It is characterized in that It also includes an aluminum oxide layer arranged on the outer surface of the conductive film layer, an isolation groove penetrates the aluminum oxide layer, and a first opening is opened on a portion of the aluminum oxide layer corresponding to the first semiconductor opening area, and a second opening is opened on a portion of the aluminum oxide layer corresponding to the second semiconductor opening area, and the first opening and the second opening are for the metal electrode to contact the conductive film layer; wherein, the refractive index of the aluminum oxide layer is 1.5-1.7, the thickness of the aluminum oxide layer is 30-50nm, the refractive index of the conductive film layer is 1.8-1.9, and the thickness ratio of the aluminum oxide layer to the conductive film layer is 1:(1.0-2.6); and the front passivation layer includes a combination of a silicon oxide passivation layer and an aluminum oxide passivation layer arranged in sequence from the front side of the silicon wafer to the outside, and the thickness ratio of the aluminum oxide passivation layer to the aluminum oxide layer is 1:(6-17).
2. The back contact cell with improved back passivation effect according to claim 1, characterized in that: The thickness of the conductive film layer is 40-80 nm.
3. The back contact cell with improved back passivation effect according to claim 1, characterized in that: The ratio of the width W31 of the first opening to the width W1 of the first semiconductor opening region is 1:(1.0-1.8), and / or the ratio of the width W32 of the second opening to the width W2 of the second semiconductor opening region is 1:(1.2-2.0).
4. The back contact cell with improved back passivation effect according to claim 1 or 3, characterized in that: The width W31 of the first opening is 130-230 μm, and the width W32 of the second opening is 250-400 μm; and / or, The width W1 of the first semiconductor opening region is 200-300 μm, and the width W2 of the second semiconductor opening region is 400-550 μm.
5. The back contact cell with improved back passivation effect according to claim 1, characterized in that: The front side of the silicon wafer and the silicon wafer region corresponding to the second semiconductor opening region are both texturing regions, and the silicon wafer region corresponding to the first semiconductor opening region is a polishing region.
6. The back contact cell with improved back passivation effect according to claim 1, characterized in that: The thickness of the silicon oxide passivation layer is 1-2nm, and the aluminum oxide passivation layer is 3-4nm; and / or, The anti-reflection layer is a combination of a silicon nitride layer and a silicon oxide layer arranged in sequence from the front side of the silicon wafer to the outside, the thickness of the silicon nitride layer is 50-100nm, and the thickness of the silicon oxide layer is 80-150nm.
7. A method for preparing a back contact battery with improved back passivation effect, characterized in that: The method is used for preparing a back contact battery with improved back passivation effect as claimed in any one of claims 1 to 6, and comprises the following steps: S1, provide double-sided polished silicon wafers; S2, forming a first semiconductor layer and an isolation layer in sequence on the back side of the silicon wafer; S3, performing a first etching opening on the back surface obtained in S2 to form a second semiconductor opening region; S4, then performing texturing cleaning, and then selecting whether to perform a step of removing the isolation layer outside the second semiconductor opening area on the back side of the silicon wafer through cleaning according to needs; S5, depositing a second semiconductor layer on the back surface obtained in S4; S6, forming a front passivation layer and an anti-reflection layer in sequence on the front side of the silicon wafer, wherein the front passivation layer comprises a combination of a silicon oxide passivation layer and an aluminum oxide passivation layer which are sequentially arranged from the front side of the silicon wafer outward; S7, performing a second etching opening on a portion of the second semiconductor layer on the back side of the silicon wafer to form a first semiconductor opening region spaced apart from the second semiconductor opening region; S8, depositing a conductive film layer on the back surface obtained in S7, and controlling the refractive index of the conductive film layer to be 1.8-1.9; S9, depositing an aluminum oxide layer on the outer surface of the back conductive film layer, controlling the refractive index of the aluminum oxide layer to be 1.5-1.7, the thickness of the aluminum oxide layer to be 30-50 nm, the thickness ratio of the aluminum oxide layer to the conductive film layer to be 1:(1.0-2.6), and the thickness ratio of the aluminum oxide passivation layer to the aluminum oxide layer to be 1:(6-17); S10, using a laser to remove a portion of the aluminum oxide layer corresponding to the first semiconductor opening region to form a first opening, and simultaneously removing a portion of the aluminum oxide layer corresponding to the second semiconductor opening region to form a second opening, wherein the first opening and the second opening expose the conductive film layers corresponding to the corresponding semiconductor opening regions; and performing a third etching opening on a portion of the conductive film layer and its corresponding aluminum oxide layer located between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove; S11, forming metal electrodes on the outer surfaces of the corresponding exposed conductive film layers in the areas where the first semiconductor opening region and the second semiconductor opening region are located.
8. The method for preparing a back contact battery with improved back passivation effect according to claim 7, characterized in that: The aluminum oxide layer in S9 is deposited by atomic layer deposition, and the conditions of the atomic layer deposition method include: the process temperature is between 150-300°C; the reaction gases are trimethylaluminum and ozone, and the flow rate of trimethylaluminum introduced in the first stage is 3000sccm-8000sccm, the reaction time is 20-40s, and then nitrogen is used to purge the chamber and pipelines; then the second stage is carried out, and the flow rate of ozone introduced in the second stage is 3000sccm-6000sccm, the ozone introduction time is 15-30s, and then nitrogen is used to purge the chamber and pipelines; the first stage and the second stage are carried out in sequence as a cycle reaction, and a total of 100-200 cycle reactions are carried out.
9. The method for preparing a back contact battery with improved back passivation effect according to claim 7 or 8, characterized in that: The laser used to remove part of the aluminum oxide layer in S10 is a flat-top picosecond green laser or a flat-top picosecond ultraviolet laser, the power of the laser is 20kW-100kW, and the frequency is 200kHZ-1000kHZ.
10. A photovoltaic module, characterized in that: It comprises a back contact cell with improved back passivation effect as claimed in any one of claims 1 to 6.