Photovoltaic waste recycling and interface regulation method for synthesizing silicon-carbon negative electrode materials

By recycling photovoltaic cutting waste silicon powder, it prepares silane-modified silicon particles and copolymerizes with polymers to form a stable silicon-carbon composite material, solving the problem of insufficient volume expansion and binding force of silicon-carbon anode material during charging and discharging, and realizing the material commercial application and long-term battery stability.

CN118658986BActive Publication Date: 2024-11-15FUYANG NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411139163.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-15
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

The existing silicon carbon negative electrode materials expand in the charging and discharging process lead to damage to the battery structure. The method of preparing small-grain silicon powder takes a long time, is costly and complex to operate, making it difficult to achieve a close bond between silicon and carbon, limiting the commercialization of materials. .

Method used

By recovering photovoltaic cutting waste silicon powder, ball milling, cleaning and surface treatment, silane-modified silicon particles are formed, and copolymerized with polymer monomers. After pyrolytic carbonization, a silicon-carbon composite material is formed, and electrode materials are prepared by combining conductive agents and binders. , a stable carbon-silicon bond is formed using a silane coupling agent and a polymer segment.

Benefits of technology

It realizes stress resistance of silicon-carbon composite materials during expansion and contraction, maintains electrical contact, is suitable for long-term lithium battery work, reduces preparation costs and complexity, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118658986B_ABST
    Figure CN118658986B_ABST
Patent Text Reader

Abstract

The present application relates to the field of electrode material technology, and specifically discloses a method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation. The present application utilizes photovoltaic cutting waste silicon powder to obtain silicon particles at a lower cost, avoiding the problems of complex silicon particle preparation process, difficult composition control, cumbersome subsequent processing, and unsuitability for industrial production in traditional processes, making it more suitable for commercial applications. The silicon-carbon composite material obtained according to the method of the present application can fully resist the stress generated during expansion and contraction, and the carbonized layer and silicon particles can maintain electrical contact for a long time, which is suitable for long-term operation in lithium batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electrode materials, and more specifically, to a method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation. Background Art

[0002] Lithium-ion batteries (LIBs) are one of the most important energy storage devices in modern times. They have been widely used in various new energy devices due to their advantages such as high energy density, low operating voltage, environmental friendliness, and long cycle life. Silicon-carbon anode materials have ultra-high theoretical capacity and low charge and discharge voltage window, and have great application potential in the field of lithium-ion batteries.

[0003] However, some studies have pointed out that the current silicon-carbon negative electrode materials generally experience dramatic volume expansion during the charging and discharging process, which can easily lead to damage to the battery structure and is not conducive to maintaining the stability of the battery structure. Although the use of small-particle silicon powder to prepare carbon-silicon negative electrode materials can overcome the influence of volume expansion to a certain extent, the current methods for preparing small-particle silicon powder (such as chemical vapor deposition and plasma evaporation condensation) generally have limitations such as long time consumption, high cost, complex operation, and immature large-scale production technology. In addition, how to achieve a close combination between silicon and carbon is still a difficult problem. If this problem is not solved, it will be difficult to ensure a stable electrode structure during a long cycle, which further limits the commercial application of silicon-carbon negative electrode materials.

[0004] Regarding the above-mentioned related technologies, the inventors believe that the silicon particles used to prepare silicon-carbon negative electrode materials currently have common problems such as complex preparation process, difficult to control composition, cumbersome subsequent processing, and unsuitability for industrial production. They are difficult to apply commercially, and it is difficult to ensure the bonding force between silicon and carbon with the current level of technology. This will cause the silicon particles to lose electrical contact with the carbon matrix due to repeated expansion and contraction during repeated charging and discharging, which will affect the conductivity of the material. Summary of the invention

[0005] In the related art, silicon particles used to prepare silicon-carbon negative electrode materials are difficult to commercialize, and it is difficult to fully ensure the bonding force between silicon and carbon with the current technical level, which will cause the silicon particles to lose electrical contact with the carbon matrix due to repeated expansion and contraction during repeated charging and discharging, affecting the conductivity of the material. In order to improve this defect, the present application provides a method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation.

[0006] The present application provides a method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation, which adopts the following technical scheme:

[0007] A method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation comprises the following steps:

[0008] (1) Adding photovoltaic waste silicon powder into a ball mill for ball milling to obtain silicon micro-nano particles, washing or burning the silicon micro-nano particles, and then flotation to obtain purified silicon particles; acid washing the purified silicon particles, and then using a silane coupling agent to perform surface treatment on the purified silicon particles to obtain silane-modified silicon particles; the surface of the silane-modified silicon particles has amino groups and vinyl groups;

[0009] (2) dispersing silane-modified silicon particles and polymer monomers in water, adding an initiator to initiate a reaction to obtain polymer-modified silicon particles; the polymer monomer used in this step includes acrylic acid;

[0010] (3) washing and drying the polymer-modified silicon particles, and obtaining a silicon-carbon composite material after pyrolysis and carbonization;

[0011] (4) The silicon-carbon composite material, the binder and the conductive agent are mixed, and water is added and stirred to obtain an electrode slurry. The electrode slurry is coated on a conductive copper foil, and the foil is vacuum dried and then cut to obtain a silicon-carbon negative electrode material.

[0012] By adopting the above technical scheme, the present application utilizes the cutting waste generated in the process of photovoltaic silicon wafer slicing - photovoltaic cutting waste silicon powder, and uses the photovoltaic cutting waste silicon powder as a silicon source for synthesizing silicon-carbon negative electrode materials. Due to the thin slice thickness in the photovoltaic silicon wafer slicing process, coupled with the huge production capacity of the photovoltaic industry, a large amount of photovoltaic cutting waste silicon powder will be generated. Due to the extremely high purity of photovoltaic silicon wafers, high-purity silicon particles can be obtained after simple separation, purification and crushing of photovoltaic cutting waste silicon powder, and the particle size can also meet the requirements for the production of silicon-carbon negative electrode materials. By utilizing photovoltaic cutting waste silicon powder, silicon particles can be obtained at a lower cost, avoiding the problems of complex silicon particle preparation process, difficult composition control, cumbersome subsequent processing, and unsuitability for industrial production in traditional processes, and more suitable for commercial applications. In the method of the present application, through the treatment of silane coupling agent, on the one hand, the surface of silicon particles can be organicized to reduce the agglomeration of silicon particles, and on the other hand, amino and vinyl groups can be introduced on the surface of silicon particles. In the subsequent step (2), the vinyl groups on the surface of the silicon particles can copolymerize with monomers such as acrylic acid, thereby introducing polymer segments on the surface of the silicon particles. These polymer segments are connected to the surface of the silicon particles through chemical bonds, and can form hydrogen bonds with groups such as amino groups on the surface of the silicon particles (i.e., amino groups introduced by silane coupling agents), so that a polymer coating with good bonding strength can be formed on the surface of the silicon particles. After pyrolysis and carbonization, the polymer coating undergoes carbonization and pyrolysis to obtain a silicon-carbon composite material with a relatively stable bond between carbon and silicon. The silicon-carbon composite material obtained according to the method of the present application can fully resist the stress generated during expansion and contraction, and the carbonized layer and the silicon particles can maintain electrical contact for a long time, which is suitable for long-term operation in lithium batteries.

[0013] Preferably, in step (1) of the method, the specific manner of surface treating the purified silicon particles is:

[0014] Purified silicon particles are added into anhydrous ethanol to obtain silicon particle dispersion after dispersion, which is set aside; a silane coupling agent is mixed with water, and a silane solution is obtained after stirring, which is set aside; the silane solution is added into the silicon particle dispersion to obtain a mixed solution, the mixed solution is stirred and heated, and condensed and refluxed at the same time, filtered after heating, and the filter cake is dried to obtain silane-modified silicon particles.

[0015] By adopting the above technical scheme, the present application separately prepares an anhydrous ethanol dispersion of silicon particles and an aqueous solution of a silane coupling agent, and then mixes the two and stirs and heats them to allow the silane to hydrolyze and condense with the silanol groups on the surface of the silicon particles, thereby grafting the silane segments onto the surface of the silicon particles to obtain silane-modified silicon particles.

[0016] Preferably, the silane coupling agent includes γ-aminopropyltriethoxysilane and vinyltriethoxysilane.

[0017] By adopting the above technical scheme, γ-aminopropyltriethoxysilane and vinyltriethoxysilane can introduce amino groups and vinyl groups on the surface of silicon particles respectively, and γ-aminopropyltriethoxysilane can promote the hydrolysis of the silane coupling agent, which helps to fully realize the surface modification of silicon particles.

[0018] Preferably, the silane coupling agent further comprises tetraethyl orthosilicate.

[0019] By adopting the above technical solution, the silica sol produced after the hydrolysis of ethyl orthosilicate can be bound to the surface of silicon particles, increasing the total amount of silanol groups on the surface of silicon particles, which is beneficial to fully realize the surface modification of silicon particles.

[0020] Preferably, in step (1) of the method, when surface treating the purified silicon particles, the silane solution and the aluminum sol are added together into the silicon particle dispersion.

[0021] By adopting the above technical solution, the aluminum sol and silicon particles have a good bonding effect, and the aluminum sol bonded to the surface of the silicon particles can be converted into aluminum oxide after high temperature treatment during the pyrolysis and carbonization process. The doping of aluminum oxide can enhance the resistance of the silicon-carbon electrode to expansion stress and help improve the cycle stability of the silicon-carbon negative electrode material.

[0022] Preferably, the aluminum sol is prepared as follows: an aluminum nitrate solution is stirred and heated, and then aluminum powder is added and reacted at 70-90° C. After the reaction is completed, insoluble impurities are removed by vacuum filtration to obtain an aluminum sol.

[0023] By adopting the above technical solution, the present application uses aluminum nitrate and aluminum powder as raw materials to prepare aluminum sol. The aluminum sol obtained according to the above method can be used in the surface modification of purified silicon particles.

[0024] Preferably, in step (2) of the method, nano-molybdenum trioxide, silane-modified silicon particles and polymer monomers are dispersed together in water.

[0025] By adopting the above technical solution, in step (2), the present application preferably uses nano molybdenum trioxide as an additive. Nano molybdenum trioxide can be loaded onto the surface of silicon particles together with polymer segments. In the subsequent pyrolysis and carbonization process, molybdenum trioxide can undergo a reduction reaction with the carbon element produced by the pyrolysis of the polymer. The molybdenum carbide produced by the reaction can promote the transfer of electrons and the diffusion of lithium ions, which helps to improve the cycle stability of the silicon-carbon negative electrode material.

[0026] Preferably, in step (2) of the method, nano-molybdenum trioxide is added in the form of a dispersion, and the solvent in the dispersion is a mixture of hydrogen peroxide and methanol.

[0027] By adopting the above technical solution, the present application optimizes the dispersion method of nano molybdenum trioxide, which can promote the uniform distribution of molybdenum carbide on the surface of the silicon-carbon negative electrode material, and help improve the cycle stability of the silicon-carbon negative electrode material.

[0028] Preferably, in step (2) of the method, unsaturated fatty acid, silane-modified silicon particles and polymer monomers are dispersed together in water, and the unsaturated fatty acid has 2-4 carbon-carbon double bonds in its molecule.

[0029] By adopting the above technical solution, the carbon-carbon double bonds in the unsaturated fatty acid molecules can copolymerize with monomers such as acrylic acid. After copolymerization with monomers, unsaturated fatty acids containing two or more carbon-carbon double bonds in the molecule can increase the number of polymer branches, help increase the coating density of the polymer on the surface of silicon particles, improve the bonding between silicon particles and carbides, and enhance the cycle stability of silicon-carbon negative electrode materials.

[0030] Preferably, the unsaturated fatty acid is selected from one of linoleic acid, linolenic acid and arachidonic acid.

[0031] By adopting the above technical solution, the present application has optimized the carbon-carbon double bond content within the range of 2-4, and obtained three unsaturated fatty acids, namely linoleic acid, linolenic acid, and arachidonic acid. By adding any one of the three unsaturated fatty acids to the copolymerization system of step (2), the number of polymer branches can be increased, and the coating density of the polymer on the surface of the silicon particles can be increased, which is helpful to improve the cycle stability of the silicon-carbon negative electrode material.

[0032] In summary, this application has the following beneficial effects:

[0033] 1. This application utilizes waste silicon powder from photovoltaic cutting to obtain silicon particles at a lower cost, avoiding the problems of complex silicon particle preparation process, difficult composition control, cumbersome subsequent processing, and unsuitability for industrial production in traditional processes, making it more suitable for commercial applications.

[0034] 2. The silicon-carbon composite material obtained according to the method of the present application can fully resist the stress generated during expansion and contraction, and the carbonized layer and silicon particles can maintain electrical contact for a long time, and is suitable for long-term operation in lithium batteries.

[0035] 3. The present application introduces aluminum oxide by adding aluminum sol, and introduces molybdenum carbide by adding nano molybdenum trioxide, thereby improving the cycle stability of the silicon-carbon negative electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a SEM image of waste silicon powder from photovoltaic cutting.

[0037] Figure 2 It is the SEM image of silicon micro-nanoparticles.

[0038] Figure 3 This is a SEM image of the silicon-carbon composite material.

[0039] Figure 4 This is the cycle performance curve of the silicon-carbon negative electrode material of Example 1 of the present application. DETAILED DESCRIPTION

[0040] The present application is further described in detail below in conjunction with embodiments, preparation examples and comparative examples. The raw materials involved in the present application can all be obtained commercially.

[0041] Preparation example of aluminum sol

[0042] The following is an explanation using Preparation Example 1.

[0043] Preparation Example 1

[0044] In this preparation example, aluminum sol was prepared according to the following method:

[0045] A 1 mol / L aluminum nitrate solution was stirred and heated while being refluxed to raise the temperature of the aluminum nitrate solution to 70°C. (铝粉) :n (硝酸铝) =2.1:1 molar ratio of aluminum powder to aluminum nitrate solution was added, and the reaction was continued at 70°C for 1 hour, then the temperature was raised to 90°C and kept for 5.5 hours, and then the insoluble impurities were removed by vacuum filtration to obtain aluminum sol. Example

[0046] Examples 1-5

[0047] The following description is given by taking Example 1 as an example.

[0048] Example 1

[0049] This embodiment provides a method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation, comprising the following steps:

[0050] (1) Adding photovoltaic cutting waste silicon powder and silicon carbide grinding balls into a ball mill for ball milling to obtain silicon micro-nano particles, washing the silicon micro-nano particles with ethanol, and then flotation to obtain purified silicon particles; using 2 mol / L hydrochloric acid to pickle the purified silicon particles, and then adding the purified silicon particles to anhydrous ethanol at a weight ratio of 1:10, and obtaining a silicon particle dispersion after ultrasonic dispersion for standby use; mixing a silane coupling agent with water at a weight ratio of 1:20, and obtaining a silane solution after stirring, and setting aside; measuring the silane solution and the silicon particle dispersion at a weight ratio of 5:1 between the silane coupling agent and the silicon dioxide, adding the silane solution to the silicon particle dispersion to obtain a mixed solution, stirring and heating the mixed solution at 70°C for 3h, and condensing and refluxing at the same time, filtering after the heating, and drying the filter cake to obtain silane-modified silicon particles; in this step, the silane coupling agent is prepared by mixing vinyl triethoxysilane and γ-aminopropyl triethoxysilane at a molar ratio of 3:1;

[0051] (2) Dispersing silane-modified silicon particles and polymer monomers in water to obtain a reaction solution with a silane-modified silicon particle content of 2.5 wt% and a monomer concentration of 7.5 wt%, adding an initiator azobisisobutylamidine hydrochloride to the reaction solution, and heating the reaction solution at 65° C. for 2 h to obtain polymer-modified silicon particles; in this step, the polymer monomer is composed of acrylic acid and acrylamide in a molar ratio of 4:1, and the amount of azobisisobutylamidine hydrochloride is 1% of the total weight of the polymer monomer;

[0052] (3) The polymer modified silicon particles were washed and dried, and then pyrolyzed and carbonized in a tube furnace. The pyrolysis and carbonization were divided into three stages. In the first stage, the temperature was raised from room temperature to 300 °C at a rate of 5 °C / min under argon protection, and then kept warm for 1 hour; in the second stage, the temperature was raised to 400 °C in 1 hour under argon protection, and then kept warm for 0.5 hour; in the third stage, hydrogen was introduced at a flow rate of 20 L / h, and the temperature was raised to 600 °C in 1 hour (referred to as the maximum carbonization temperature in Table 1), and then kept warm for 1 hour. After cooling to 25 °C in the furnace, a silicon-carbon composite material was obtained;

[0053] (4) A silicon-carbon composite material, a binder sodium hydroxymethyl cellulose, and a conductive agent carbon black were mixed in a weight ratio of 6:2:2 (referred to as the slurry ratio in Table 1), and water was added and stirred to obtain an electrode slurry with a solid content of 45%. The electrode slurry was coated on a conductive copper foil, and the mixture was vacuum dried at 80°C and then cut to obtain a silicon-carbon negative electrode material.

[0054] As shown in Table 1, the main difference between Examples 1-5 is that some of the process parameters selected in the method for synthesizing silicon-carbon negative electrode materials are different.

[0055] Table 1 Some process parameters

[0056]

[0057] Example 6

[0058] The difference between this embodiment and embodiment 5 is that in step (1), the silane coupling agent in the silane solution is a mixture of vinyl triethoxysilane, γ-aminopropyl triethoxysilane and ethyl orthosilicate in a molar ratio of 3:1:2. The weight ratio of the total weight of vinyl triethoxysilane and γ-aminopropyl triethoxysilane to the weight of silicon dioxide in the silicon particle dispersion is still 5:1.

[0059] Example 7

[0060] The difference between this embodiment and embodiment 6 is that in step (1), when surface treating the purified silicon particles, the silane solution and the aluminum sol are added to the silicon particle dispersion. The aluminum sol is prepared according to the method of preparation example 1, and the amount of aluminum sol used is 40% of the total weight of the silane solution.

[0061] Example 8

[0062] The difference between this embodiment and embodiment 7 is that in step (2), nano molybdenum trioxide, silane-modified silicon particles and polymer monomers are dispersed together in water, the nano molybdenum trioxide is added directly, the average particle size of the nano molybdenum trioxide is 18.6 nm, and the amount of nano molybdenum trioxide used is 1.5% of the total weight of the silane-modified silicon particles.

[0063] Example 9

[0064] The difference between this embodiment and embodiment 8 is that the method of adding nano molybdenum trioxide is as follows: first, nano molybdenum trioxide is added to a mixed solvent of hydrogen peroxide and methanol (volume ratio is 1:1) at a ratio of 1 g:35 mL, stirred at a rate of 200 r / min for 10 min to obtain a dispersion, and then nano molybdenum trioxide is added in the form of a dispersion.

[0065] Example 10

[0066] The difference between this embodiment and embodiment 9 is that in step (2) of the method, unsaturated fatty acid, silane-modified silicon particles and polymer monomers are dispersed together in water, the molar ratio of unsaturated fatty acid to acrylic acid is 1:10, and linoleic acid is selected as the unsaturated fatty acid.

[0067] Embodiment 11

[0068] The difference between this embodiment and embodiment 10 is that linolenic acid is used as the unsaturated fatty acid.

[0069] Example 12

[0070] The difference between this embodiment and embodiment 11 is that arachidonic acid is used as the unsaturated fatty acid.

[0071] Embodiment 13

[0072] The difference between this embodiment and embodiment 10 is that oleic acid is used as the unsaturated fatty acid. Comparative Example

[0073] Comparative Example 1

[0074] The difference between this comparative example and Example 1 is that the vinyltriethoxysilane in step (1) is replaced by methyltriethoxysilane.

[0075] Comparative Example 2

[0076] The difference between this comparative example and Example 1 is that the γ-aminopropyltriethoxysilane in step (1) is replaced by methyltriethoxysilane.

[0077] Comparative Example 3

[0078] The difference between this comparative example and Example 1 is that in step (1), no silane coupling agent is used to modify the surface of the purified silicon particles, and in step (2), the purified silicon particles and the polymer monomer are directly dispersed in water, and the subsequent steps are continued.

[0079] Performance testing methods

[0080] 1. Surface morphology

[0081] The surface morphology of photovoltaic waste silicon powder, silicon micro-nano particles, and silicon-carbon composites was observed using a scanning electron microscope (SEM). Figure 1-3 .

[0082] 2. Cycle stability

[0083] According to the process of each embodiment and comparative example, 2 mg / cm 2The slurry is coated on copper foil with a coating amount of 1 mol / L, and then cut after vacuum drying at 80°C to obtain a silicon-carbon negative electrode material. The silicon-carbon negative electrode material is assembled into a CR2032 button battery, and the electrolyte is prepared by dissolving LiPF6 at a concentration of 1 mol / L in a mixed solution of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1, and then adding 6 wt% of fluoroethylene carbonate. During the test, a charge and discharge tester (CT3001A) was used to test the cycle performance. The battery was first activated for 3 cycles at 100 mA / g, and then formally cycled for 50 cycles at 200 mA / g. The ratio between the specific capacity remaining after 200 cycles of formal circulation (the average value of the charge specific capacity and the discharge specific capacity, the same below) and the specific capacity before the start of the formal circulation (i.e. after 3 cycles of activation) was detected and calculated, and the ratio was recorded as the specific capacity remaining rate. The results are shown in Table 2. The cycle performance curve of the silicon-carbon negative electrode material of Example 1 is plotted as a reference, see Figure 4 .

[0084] Table 2

[0085]

[0086] Combination Figure 1-3 It can be seen that the silicon micro-nano particles prepared from photovoltaic cutting waste silicon powder have relatively ideal microscopic morphology and size, and are suitable for preparing silicon-carbon negative electrode materials. After the silicon particles are surface modified and pyrolyzed and carbonized, the obtained silicon-carbon composite material has been fully coated with carbides.

[0087] Combined with Examples 1-5 and Comparative Examples 1-3 and Tables 2 and Figure 4 It can be seen that the specific capacity residual rates measured in Examples 1-5 are all above 40%, and the remaining specific capacity of Example 1 is still around 1000mAh / g, which can fully meet the needs of actual use. The specific capacity residual rates of Comparative Examples 1-3 are significantly lower than those of Examples 1-5. Among them, the remaining specific capacity of Comparative Example 3 after cycling is even less than 20% of the initial capacity, indicating that a silicon-carbon composite material with a relatively stable bond between carbon and silicon can be obtained according to the method of the present application. The silicon-carbon composite material of the present application can fully resist the stress generated during expansion and contraction, and the carbonized layer and silicon particles can maintain electrical contact for a long time, which is more suitable for long-term operation in lithium batteries.

[0088] It can be seen from Example 5 and Example 6 and Table 2 that the addition of tetraethyl orthosilicate increases the total amount of silanol groups on the surface of silicon particles, which is beneficial to fully realize the surface modification of silicon particles, thereby obtaining a silicon-carbon negative electrode material with more ideal cycle stability.

[0089] It can be seen from Example 6 and Example 7 and Table 2 that due to the addition of aluminum sol, a certain amount of aluminum oxide is combined with the surface of the silicon-carbon negative electrode material, and the doping of aluminum oxide can enhance the resistance of the silicon-carbon electrode to expansion stress, thereby improving the cycle stability of the silicon-carbon negative electrode material.

[0090] It can be seen from Example 7 and Example 8 and Table 2 that after the reduction reaction between molybdenum trioxide and the carbon element produced by polymer pyrolysis, the molybdenum carbide produced promotes the transfer of electrons and the diffusion of lithium ions, thereby improving the cycle stability of the silicon-carbon negative electrode material.

[0091] It can be seen from Example 8 and Example 9 and Table 2 that the mixture of hydrogen peroxide and methanol improves the dispersion effect of nano-molybdenum trioxide and promotes the uniform distribution of molybdenum carbide on the surface of the silicon-carbon negative electrode material, thereby improving the cycle stability of the silicon-carbon negative electrode material.

[0092] It can be seen from Example 9, Examples 10-12 and Table 2 that since the carbon-carbon double bonds in the unsaturated fatty acid molecules can copolymerize with monomers such as acrylic acid, and the unsaturated fatty acids containing two or more carbon-carbon double bonds in the molecules can increase the number of polymer branches after copolymerization with the monomers, the coating density of the polymer on the surface of the silicon particles is increased, the bonding degree between the silicon particles and the carbide is improved, and the cycle stability of the silicon-carbon negative electrode material is enhanced.

[0093] It can be seen from Examples 10-13 and Table 2 that when the unsaturated fatty acid contains only one carbon-carbon double bond, the contribution of the unsaturated fatty acid to the cycle stability of the silicon-carbon negative electrode material is relatively small.

[0094] The above embodiments are merely explanations of the present application and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications to the embodiments of the present application without any creative contribution as needed. However, as long as they are within the scope of the claims of the present application, they are protected by the patent law.

Claims

1. A method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation, characterized in that: The following steps are involved: (1) adding photovoltaic waste silicon powder into a ball mill for ball milling to obtain silicon micro-nano particles, washing or burning the silicon micro-nano particles, and then flotation to obtain purified silicon particles; acid washing the purified silicon particles, and then using a silane coupling agent to perform surface treatment on the purified silicon particles to obtain silane-modified silicon particles; the surface of the silane-modified silicon particles has amino groups and vinyl groups; (2) dispersing silane-modified silicon particles and polymer monomers in water, adding an initiator to initiate a reaction to obtain polymer-modified silicon particles; the polymer monomer used in this step includes acrylic acid; (3) washing and drying the polymer-modified silicon particles, and obtaining a silicon-carbon composite material after pyrolysis and carbonization; (4) mixing a silicon-carbon composite material, a binder and a conductive agent, adding water and stirring to obtain an electrode slurry, coating the electrode slurry on a conductive copper foil, vacuum drying and cutting to obtain a silicon-carbon negative electrode material; In step (2) of the method, unsaturated fatty acid, silane-modified silicon particles and polymer monomers are dispersed together in water, wherein the unsaturated fatty acid has 2 to 4 carbon-carbon double bonds in its molecule.

2. The method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation according to claim 1, characterized in that: In step (1) of the method, the specific manner of surface treating the purified silicon particles is: Purified silicon particles are added into anhydrous ethanol to obtain silicon particle dispersion after dispersion, which is set aside; a silane coupling agent is mixed with water, and a silane solution is obtained after stirring, which is set aside; the silane solution is added into the silicon particle dispersion to obtain a mixed solution, the mixed solution is stirred and heated, and condensed and refluxed at the same time, filtered after heating, and the filter cake is dried to obtain silane-modified silicon particles.

3. The method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation according to claim 2, characterized in that: The silane coupling agent includes γ-aminopropyltriethoxysilane and vinyltriethoxysilane.

4. The method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation according to claim 3, characterized in that: The silane coupling agent also includes tetraethyl orthosilicate.

5. The method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation according to claim 3, characterized in that: In step (1) of the method, when surface treating the purified silicon particles, the silane solution and the aluminum sol are added together into the silicon particle dispersion.

6. The method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation according to claim 5, characterized in that: The aluminum sol is prepared by the following method: stirring and heating an aluminum nitrate solution, then adding aluminum powder and reacting at 70-90° C., and after the reaction is completed, removing insoluble impurities by vacuum filtration to obtain an aluminum sol.

7. The method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation according to claim 1, characterized in that: In step (2) of the method, nano-molybdenum trioxide, silane-modified silicon particles and polymer monomers are dispersed together in water.

8. The method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation according to claim 7, characterized in that: In step (2) of the method, nano molybdenum trioxide is added in the form of a dispersion, and the solvent in the dispersion is a mixture of hydrogen peroxide and methanol.

9. The method for recycling photovoltaic waste and synthesizing silicon-carbon negative electrode materials by interface regulation according to claim 1, characterized in that: The unsaturated fatty acid is selected from one of linoleic acid, linolenic acid and arachidonic acid.