Electrolyte, lithium battery and liquid injection formation method thereof
By adding sodium salt and organic film-forming additives to the lithium battery electrolyte, a porous and loose SEI film is formed, which solves the problem of easy interface damage during fast charging of the silicon-based negative electrode, and improves the cycle life and fast charging performance of the lithium battery .
Patent Information
- Application Number
- CN202411139342.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-19
AI Technical Summary
During the fast charging process of existing lithium batteries, silicon-based negative electrode solid electrolyte interface mask (SEI) is easily destroyed, affecting the battery's cycle life and fast charging performance, and it is difficult to take into account the battery's cycle life and fast charging performance.
Introduce an appropriate amount of sodium salt additives and organic film-forming additives to form a dense organic-inorganic SEI film, and dissolve the sodium compounds in the SEI film by standing at high temperature to form a porous, loose, and low-impedance SEI interface layer to alleviate silicon The volume of the base negative electrode changes to protect the negative electrode interface.
It effectively alleviates the volume change of the silicon-based negative electrode during charging and discharging, reduces the side reactions caused by SEI rupture, improves the cycle life and fast charging capacity of lithium batteries, and the low impedance of the porous and loose SEI film is conducive to ion transmission.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to an electrolyte, a lithium battery and a liquid injection formation method thereof. Background Art
[0002] Lithium-ion batteries have been widely used in electric vehicles, laptops, and energy storage due to their high energy density, long cycle life, and environmental friendliness. With the increasing demand for battery life and fast charging capabilities in electrical equipment, it is necessary to increase the energy density of batteries and reduce the internal resistance of batteries. In order to increase the energy density of batteries, high-energy-density silicon-based negative electrode active materials are often required. However, such silicon-based negative electrode materials will undergo huge volume changes during the battery charging and discharging process, especially under fast charging, where the volume ratio changes even more, which will cause the silicon-based negative electrode solid electrolyte interface film (SEI) to be destroyed, affecting the cycle life of the battery.
[0003] In this regard, the current main approach is to strengthen or thicken the SEI layer to protect the silicon-based interface, but this often increases the interface impedance, thus affecting the fast charging performance. In short, there is currently no better way to ensure both fast charging performance and the stability of the silicon-based negative electrode SEI under fast charging. Summary of the invention
[0004] To solve the above problems, the present invention provides an electrolyte, a lithium battery and a liquid injection formation method thereof. The present invention introduces an appropriate amount of sodium salt additive into the electrolyte, so that the sodium salt additive and the organic film-forming additive form a dense organic-inorganic SEI film during the small current charging stage at room temperature, and then stands and discharges at high temperature to dissolve the sodium-containing compounds in the SEI film in the electrolyte solvent to form a porous, loose and low-impedance SEI interface layer, which can effectively alleviate the volume change of the silicon-based negative electrode while ensuring the fast charging capability.
[0005] The present invention provides the following technical solutions:
[0006] A first aspect of the present invention provides an electrolyte, wherein the electrolyte comprises a sodium salt additive and an organic film-forming additive and satisfies the following relationship:
[0007] 0.3wt%≤X≤2wt%, 0.9wt%≤Y≤5wt%, and 1≤Y / X≤10;
[0008] Wherein, X is the mass percentage of the sodium salt additive in the electrolyte;
[0009] Y is the mass percentage of the organic film-forming additive in the electrolyte.
[0010] Furthermore, the sodium salt additive is preferably one or more of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium hexafluoroarsenate, sodium bis(oxalatoborate), sodium difluorooxalatoborate, sodium difluorophosphate, sodium bis(fluorosulfonyl)imide, and sodium bis(trifluoromethylsulfonyl)imide.
[0011] Furthermore, the organic film-forming additive is preferably one or more of vinylene carbonate, vinyl ethylene carbonate, 1,3-propylene sultone, triphenyl phosphite, acrylamide, N,N-dimethylacrylamide, ethoxylated trimethylolpropane triacrylate, and pentaerythritol triacrylate.
[0012] Furthermore, the mass ratio of the sodium salt additive to the organic film-forming additive in the electrolyte is more preferably 2≤Y / X≤5.
[0013] Furthermore, the electrolyte further comprises an electrolyte lithium salt; the mass percentage of the electrolyte lithium salt in the electrolyte is Z, preferably, satisfying 10wt%≤X+Z≤17wt%; the electrolyte lithium salt is preferably one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium difluorophosphate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, and lithium difluorobis(oxalatophosphate).
[0014] Furthermore, the electrolyte further comprises an organic solvent; the organic solvent is selected from one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, fluoroethylene carbonate, fluoropropylene carbonate, and fluoroethyl methyl carbonate.
[0015] The second aspect of the present invention provides a lithium battery, comprising a negative electrode plate and an electrolyte; the electrolyte is the electrolyte described in the first aspect; the negative electrode plate comprises a current collector and a negative electrode active layer arranged on at least one side of the current collector along the thickness direction, the negative electrode active layer comprises a negative electrode active material, and the negative electrode active material comprises a silicon-based negative electrode material; the silicon-based negative electrode material comprises one or more of silicon element, silicon-carbon material, and silicon-oxygen material.
[0016] The third aspect of the present invention provides a liquid injection formation method for the lithium battery according to the second aspect, comprising the following steps:
[0017] S1, liquid injection: injecting electrolyte into the shell of the lithium battery;
[0018] S2, formation: at temperature T1, charge the lithium battery after injection with a constant current of I1 to the upper limit voltage U1; then place it at temperature T2 for 12-24 hours, and then discharge it at temperature T2 with a constant current of I2 to the lower limit voltage U2; wherein, T1≤45℃, 45℃≤T2≤60℃; I1≤0.1℃, I2≤0.1℃; 3.2V≤U1≤3.7V, 2.0V≤U2≤2.8V;
[0019] S3, repeat the charge and discharge cycle of S2 1-3 times.
[0020] Furthermore, 25 ℃ ≤ T1 ≤ 35 ℃.
[0021] Furthermore, 0.05 C≤I1≤0.1 C and / or 0.05 C≤I2≤0.1 C; more preferably, I1=I2.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention provides an electrolyte, comprising an appropriate amount of a sodium salt additive and an organic film-forming additive, which can form a dense organic-inorganic SEI film in a small current charging stage at room temperature. The organic-inorganic SEI film comprises a sodium compound with low Lewis acidity, which can be dissolved in a carbonate solvent at high temperature to form an SEI interface layer with a loose porous structure, which can effectively alleviate the volume change of the negative electrode material during the charging and discharging process, protect the negative electrode interface, and reduce side reactions; and the porous and loose SEI interface has low impedance, which is conducive to accelerating ion transmission.
[0024] The present invention also provides a liquid injection formation method, which, in conjunction with the above-mentioned electrolyte, can effectively construct a loose, porous and low-impedance SEI film on the surface of the battery negative electrode, so that the lithium battery based on the silicon-based negative electrode has excellent charge and discharge cycle performance while having a lower DCR. DETAILED DESCRIPTION
[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items. The "include" or "comprising" described in the present invention means that in addition to the components described, other components may also be included or contained. The "include" or "comprising" described in the present invention may also be replaced by the closed "for" or "consisting of...".
[0026] Silicon-based negative electrode materials will undergo huge volume changes during the battery charging and discharging process, especially under fast charging, the volume ratio changes even more, which will cause the silicon-based negative electrode solid electrolyte interface film (SEI) to be destroyed, affecting the battery's cycle life. Currently, the main approach is to strengthen or thicken the SEI layer to protect the silicon-based interface, but this often causes an increase in interface impedance, thereby affecting fast charging performance. Therefore, it is difficult to take into account both the battery's cycle life and fast charging performance.
[0027] To solve the above problems, the embodiments of the present invention provide an electrolyte solution, which includes a sodium salt additive and an organic film-forming additive and satisfies the following relationship:
[0028] 0.3wt%≤X≤2wt%, 0.9wt%≤Y≤5wt%, and 1≤Y / X≤10;
[0029] Wherein, X is the mass percentage of the sodium salt additive in the electrolyte; Y is the mass percentage of the organic film-forming additive in the electrolyte.
[0030] In the present invention, the sodium salt additive can be selected from one or more of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium hexafluoroarsenate, sodium bisoxalate borate, sodium difluorooxalate borate, sodium difluorophosphate, sodium bisfluorosulfonyl imide, and sodium bis(trifluoromethylsulfonyl)imide; the organic film-forming additive can be selected from one or more of vinylene carbonate, vinyl ethylene carbonate, propylene-1,3-sultone, triphenylphosphite, acrylamide, N,N-dimethylacrylamide, ethoxylated trimethylolpropane triacrylate, and pentaerythritol triacrylate. The types of sodium salt additives and organic film-forming additives include but are not limited to the types listed above, and other sodium salt additives and organic film-forming additives that can form an organic-inorganic SEI film during low-current charging at room temperature can also be used.
[0031] The present invention provides an electrolyte containing both a sodium salt additive and an organic film-forming additive to solve the problem that it is difficult to balance the battery cycle life and fast charging performance in high-density lithium-ion batteries currently prepared with silicon-based negative electrode materials as negative electrode active materials. The electrolyte can form a dense SEI film containing inorganic sodium-containing compounds (such as sodium fluoride, sodium carbonate, sodium nitride, etc.) and organic compounds on the surface of the negative electrode during the low-current charging process in the formation stage of the lithium battery. The Lewis acidity of the inorganic sodium-containing compound is low, and the SEI film composed of it is unstable. The sodium-containing compound in the SEI film will dissolve in the electrolyte solvent (such as a carbonate solvent), thereby converting the original high-impedance, dense SEI film into a low-impedance, loose and porous SEI film. During the battery charging and discharging process, the porous and loose SEI film can effectively alleviate the volume change of the silicon-based negative electrode, protect the negative electrode interface, and reduce the occurrence of side reactions caused by SEI rupture and the consumption of active lithium.
[0032] In addition, it should be noted that the mass proportion of the sodium salt additive and the organic film-forming additive in the electrolyte and the mass ratio of the two will affect the porosity of the SEI film finally formed and its interfacial resistance. For example, the porosity of the SEI film will increase with the increase of the sodium salt additive content in the electrolyte, and the SEI interfacial resistance will increase with the increase of the organic film-forming additive content in the electrolyte; if the sodium salt additive content is too high (X>2wt%), the organic film-forming additive content is too low (Y<0.9wt%) or the Y / X ratio is <1, the interfacial resistance of the formed SEI film is low, but the porosity of the SEI film is too large and the integrity is poor. During the battery charge and discharge cycle, the side reactions increase, which deteriorates the battery's cycle performance; but if the sodium salt additive content is too low (X<0.3wt%), the organic film-forming additive content is too high (Y>5wt%) or the Y / X ratio is >10, the constructed SEI film has a high density, low porosity and high interfacial impedance. Although the integrity of the film is high, it cannot effectively alleviate the volume change of the silicon-based negative electrode, resulting in continuous damage to the SEI film during the charge and discharge cycle, which deteriorates the cycle performance. Based on this, in order to ensure that the SEI film constructed on the surface of the negative electrode has an appropriate porosity to alleviate the volume change of the silicon-based negative electrode while ensuring stability, and at the same time has a relatively low interface resistance, preferably, the mass percentage X of the sodium salt additive in the electrolyte is controlled in the range of 0.3wt%-2wt%, and the mass percentage Y of the organic film-forming additive in the electrolyte is controlled in the range of 0.9wt%-5wt%, and the ratio Y / X of the two is controlled in the range of 1-10; more preferably, Y / X is controlled in the range of 2-5 to obtain a lithium battery with both excellent cycle performance and low DCR.
[0033] In the present invention, the electrolyte further comprises an electrolyte lithium salt, and the content of the electrolyte lithium salt in the electrolyte needs to be controlled within a suitable range. If the content is too low, it will affect the ionic conductivity of the electrolyte, while if the content is too high, it will not only increase the cost, but also increase the viscosity of the electrolyte, which is not conducive to ion transmission; preferably, the mass percentage of the electrolyte lithium salt in the electrolyte is Z, satisfying 10wt%≤X+Z≤17wt%; wherein the electrolyte lithium salt includes but is not limited to one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium difluorophosphate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, and lithium difluorobis(oxalatophosphate).
[0034] In the present invention, the electrolyte further comprises an organic solvent, preferably a carbonate solvent, which can be selected from one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, fluoroethylene carbonate, fluoropropylene carbonate, and fluoromethyl ethyl carbonate. It has good solubility for sodium-containing compounds at high temperatures and is beneficial to the formation of a porous and loose structure of the SEI membrane.
[0035] The present invention also provides a lithium battery in the embodiment part, which includes a negative electrode plate and the above-mentioned electrolyte, the negative electrode plate includes a current collector and a negative electrode active layer arranged on at least one side of the current collector along the thickness direction, the negative electrode active layer includes a negative electrode active material, and the negative electrode active material includes a silicon-based negative electrode material; the silicon-based negative electrode material includes one or more of silicon element, silicon-carbon material, and silicon-oxygen material.
[0036] In addition, the embodiments of the present invention provide a liquid injection formation method suitable for the above lithium battery, comprising the following steps:
[0037] S1, liquid injection: injecting electrolyte into the shell of the lithium battery;
[0038] S2, formation: at temperature T1, charge the lithium battery after injection with a constant current of I1 to the upper limit voltage U1; then place it at temperature T2 for 12-24 hours, and then discharge it at temperature T2 with a constant current of I2 to the lower limit voltage U2; wherein, T1≤45℃, 45℃≤T2≤60℃; I1≤0.1℃, I2≤0.1℃; 3.2V≤U1≤3.7V, 2.0V≤U2≤2.8V;
[0039] S3, repeat S2 charge and discharge cycle 1-3 times
[0040] The present invention charges a lithium battery containing the above electrolyte at a relatively low temperature T1 (T1≤45°C) with a small current, so that the sodium salt additive and the organic film-forming additive in the electrolyte form a dense organic-inorganic SEI film on the surface of the negative electrode, and then places it at a high temperature T2 for 12-24 hours and discharges it at this temperature. Since the Lewis acidity of the inorganic sodium-containing compound in the formed organic-inorganic SEI film is low, it will dissolve in the electrolyte solvent at the temperature T2, thereby converting the original dense SEI film into an SEI film with a loose porous structure. The above film formation and inorganic sodium salt dissolution operations are repeated 1-3 times to form a complete SEI interface layer with a loose porous structure on the surface of the negative electrode. It should be noted here that the temperature of the film-forming stage T1 should not be too high, otherwise the sodium-containing compounds will dissolve during the film-forming stage, and the formed SEI film with a high organic content will be dense and have high impedance. Therefore, the temperature of T1 needs to be controlled below 45°C; at the same time, the temperature of T2 should not be too low or too high. If the temperature of T2 is too low, it will affect the dissolution of the sodium-containing compounds and fail to effectively form a loose porous SEI film. However, if the temperature of T2 is too low, it will lead to the dissolution of organic components and the stability of the formed SEI film will be poor. In order to obtain a stable, complete and loose porous SEI interface film layer, T2 needs to be controlled at 45-60°C.
[0041] In the present invention, the temperature of the formation charging process affects the rate of SEI formation and the dissolution rate of sodium-containing compounds in the SEI film. If the temperature is too low, the SEI film formation rate is too slow, and if the temperature is too high, the sodium-containing compounds in the SEI film will dissolve during the formation process, resulting in an increase in the content of organic components in the SEI film and an increase in the interface impedance; therefore, preferably, the temperature T1 of the charging process is controlled in the range of 25°C-35°C to increase the SEI film formation rate while forming a SEI film with low impedance and a complete, porous and loose structure.
[0042] In the present invention, the current size in the formation stage will affect the density of the film. For example, if the current is too high, the early film will be loose. When left to stand under subsequent high temperature conditions, as the sodium-containing compounds dissolve, the SEI film structure will be easily damaged, thereby deteriorating the cycle performance of the battery. Therefore, the present invention controls the charging current I1 and the discharging current I2 to be below 0.1 C. To promote the reaction efficiency, preferably, 0.05 C≤I1≤0.1 C, 0.05 C≤I2≤0.1 C, and more preferably, I1=I2.
[0043] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention. Example 1
[0044] This embodiment relates to the preparation of a lithium ion battery, and the specific preparation process is as follows:
[0045] Preparation of positive electrode sheets: positive electrode active material NCM (811), binder polyvinylidene fluoride (PVDF), conductive carbon black and single-walled carbon nanotubes are mixed in a weight ratio of 97.2:1.5:1.2:0.1, N-methylpyrrolidone (NMP) is added, and the mixture is stirred under the action of a vacuum mixer until the mixed system becomes a positive electrode slurry with uniform fluidity; the positive electrode slurry is evenly coated on the current collector aluminum foil, and the desired positive electrode sheets are obtained by drying, rolling and cutting.
[0046] Preparation of negative electrode sheets: negative electrode active material silicon oxide, thickener sodium carboxymethyl cellulose (CMC-Na), binder styrene-butadiene rubber, and conductive agent acetylene black are mixed in a weight ratio of 97:1:1:1, deionized water is added, and negative electrode slurry is obtained under the action of a vacuum mixer. The negative electrode slurry is evenly coated on a high-strength carbon-coated aluminum foil to obtain a sheet, and the obtained sheet is dried, rolled, and cut to obtain a negative electrode sheet.
[0047] Preparation of electrolyte: In a glove box filled with inert gas (H2O <10 ppm, O2 <5 ppm), fluoroethylene carbonate, ethyl methyl carbonate and diethyl carbonate were mixed in a mass ratio of FEC:EMC:DEC=3:5:2, and then 15 wt% LiPF6, 0.30 wt% NaFSI and 1 wt% VC based on the total weight of the electrolyte were slowly added to the mixed solution, where the mass ratio Y / X of the organic film-forming additive to the sodium salt additive was 3.33.
[0048] Diaphragm: 9 micron thick PP film;
[0049] Preparation of battery: stack the prepared positive electrode, separator and negative electrode in order, ensure that the separator is between the positive and negative electrodes to play an isolating role, place the bare battery cell in an aluminum plastic film outer package to obtain a battery, dry, inject (inject the prepared electrolyte into the dried battery), package, stand, form and divide the capacity to obtain a lithium-ion battery. Among them, the formation stage is divided into two parts: Formation stage 1, at T1 (25 ℃), charge to U1 (3.3 V) with current I1 (0.1 C); Formation stage 2: at T2 (45 ℃), stand for t (24 h), and continue to discharge to U2 (2.5 V) at T2 (45 ℃) with current I2 (0.1 C); Formation stage 1-2 is repeated 3 times to complete the formation. Then the capacity division is carried out, which is a conventional process step. The battery is charged to 4.25 V at 0.33 C at 25 °C, and then discharged to 2.5 V at 0.33 C to end the capacity division. Example 2
[0050] This embodiment relates to the preparation of a lithium ion battery, which is different from Example 1 only in that the mass proportion of LiPF6 in the electrolyte is 15 wt%, the mass proportion of NaFSI is 0.5 wt%, the mass proportion of VC is 2 wt%, the mass ratio Y / X of the organic film-forming additive to the sodium salt additive is 4, and other operations are the same to prepare a lithium ion battery. Example 3
[0051] This embodiment relates to the preparation of a lithium ion battery, which is different from Example 1 only in that the mass proportion of LiPF6 in the electrolyte is 15 wt%, the mass proportion of NaFSI is 2 wt%, the mass proportion of VC is 4 wt%, the mass ratio Y / X of the organic film-forming additive to the sodium salt additive is 2, and other operations are the same to prepare a lithium ion battery. Example 4
[0052] This embodiment relates to the preparation of a lithium ion battery, which is different from Example 1 only in that the mass proportion of LiPF6 in the electrolyte is 15 wt%, the mass proportion of NaFSI is 0.5 wt%, the mass proportion of VC is 5 wt%, the mass ratio Y / X of the organic film-forming additive to the sodium salt additive is 10, and other operations are the same to prepare a lithium ion battery. Example 5
[0053] This embodiment relates to the preparation of a lithium-ion battery, which is different from Example 1 only in that the mass proportion of LiPF6 in the electrolyte is 15 wt%, the mass proportion of NaFSI is 0.5 wt%, the mass proportion of VC is 0.5 wt%, the mass ratio Y / X of the organic film-forming additive to the sodium salt additive is 1, and other operations are the same to prepare a lithium-ion battery. Example 6
[0054] This embodiment relates to the preparation of a lithium ion battery, and the only difference from Embodiment 2 is that an equal amount of NaBF4 is used to replace NaFSI in the electrolyte, and other operations are the same to prepare a lithium ion battery. Example 7
[0055] This embodiment relates to the preparation of a lithium ion battery, and the only difference from Embodiment 2 is that an equal amount of PS is used to replace VC in the electrolyte, and other operations are the same to prepare a lithium ion battery. Example 8
[0056] This embodiment relates to the preparation of a lithium ion battery, which is different from Example 2 only in that: in the formation stage 1, T1 is 35°C, the current I1 is 0.05°C, and in the formation stage 2, the current I2 is 0.05°C. Other operations are the same, and a lithium ion battery is prepared. Example 9
[0057] This embodiment relates to the preparation of a lithium ion battery, which is different from the embodiment 2 only in that T2 in the formation stage 2 is 60° C., the standing time t is 12 h, and the other operations are the same, and a lithium ion battery is prepared. Example 10
[0058] This embodiment relates to the preparation of a lithium-ion battery, which is different from Embodiment 2 only in that the negative electrode main material is replaced by silicon dioxide with a silicon-carbon negative electrode, and other operations are the same to prepare a lithium-ion battery. Embodiment 11
[0059] This embodiment relates to the preparation of a lithium ion battery, and the only difference from Example 2 is that the electrolyte solvent system is replaced with fluoroethylene carbonate, propylene carbonate, ethyl methyl carbonate and diethyl carbonate in a mass ratio of FEC:PC:EMC:DEC=2:1:5:2, and other operations are the same to prepare a lithium ion battery. Example 12
[0060] This embodiment relates to the preparation of a lithium-ion battery, and the only difference from Example 2 is that 15 wt% of LiPF6 lithium salt in the electrolyte is replaced by 9 wt% LiPF6+7 wt% LiFSI, and other operations are the same to prepare a lithium-ion battery. Embodiment 13
[0061] This embodiment relates to the preparation of a lithium-ion battery, and the only difference from Embodiment 2 is that 15 wt% of LiPF6 lithium salt in the electrolyte is adjusted to 10 wt% of LiPF6, and other operations are the same to prepare a lithium-ion battery. Embodiment 14
[0062] This embodiment relates to the preparation of a lithium-ion battery, and the only difference from Embodiment 2 is that 15 wt% of LiPF6 lithium salt in the electrolyte is adjusted to 16.5 wt% of LiPF6, and other operations are the same to prepare a lithium-ion battery. Comparative Example 1
[0063] This comparative example relates to the preparation of a lithium-ion battery, which is different from Example 1 only in that the electrolyte does not contain the sodium salt additive NaFSI, and other operations are the same to prepare a lithium-ion battery. Comparative Example 2
[0064] This comparative example relates to the preparation of a lithium-ion battery, which is different from Example 1 only in that the mass proportion of NaFSI in the electrolyte is 3 wt %, and other operations are the same, and a lithium-ion battery is prepared. Comparative Example 3
[0065] This comparative example relates to the preparation of a lithium ion battery, which is different from Example 2 only in that the electrolyte does not contain the organic film-forming additive VC, and other operations are the same to prepare a lithium ion battery. Comparative Example 4
[0066] This comparative example relates to the preparation of a lithium-ion battery, which is different from Example 2 only in that the mass proportion of VC in the electrolyte is 6 wt %, and other operations are the same, and a lithium-ion battery is prepared. Comparative Example 5
[0067] This comparative example relates to the preparation of a lithium ion battery, and the only difference from Example 2 is: the formation method. This comparative example adopts a conventional formation process for formation, specifically: charging to 3.3 V with a current of 0.1 C, and ending the formation; other operations are the same, and a lithium ion battery is prepared. Comparative Example 6
[0068] This comparative example relates to the preparation of a lithium ion battery, which is different from Example 2 only in that the temperatures of I1 in formation stage 1 and I2 in formation stage 1 are both 0.3 C, and other operations are the same, thereby preparing a lithium ion battery. Comparative Example 7
[0069] This embodiment relates to the preparation of a lithium ion battery, which is different from the embodiment 2 only in that T1 in the formation stage 2 is 60° C., and other operations are the same, and a lithium ion battery is prepared. Comparative Example 8
[0070] This comparative example relates to the preparation of a lithium ion battery, which is different from Example 2 only in that T2 in the formation stage 2 is 80° C., and other operations are the same, thereby preparing a lithium ion battery. Comparative Example 9
[0071] This comparative example relates to the preparation of a lithium ion battery, which is different from Example 2 only in that T2 in the formation stage 2 is 25° C., and other operations are the same, thereby preparing a lithium ion battery. Comparative Example 10
[0072] This comparative example relates to the preparation of a lithium ion battery, which is different from Example 2 only in that the standing time t in the formation stage 2 is 48 h, and the other operations are the same, and a lithium ion battery is prepared. Comparative Example 11
[0073] This comparative example relates to the preparation of a lithium ion battery, which is different from Example 2 only in that the standing time t in the formation stage 2 is 6 h, and the other operations are the same, and a lithium ion battery is prepared.
[0074] The electrolyte parameters and formation process parameters of the sodium ion batteries prepared in the above examples and comparative examples are shown in Table 1 below:
[0075] Table 1
[0076]
[0077] Performance Testing
[0078] The lithium-ion batteries prepared in the above embodiments and comparative examples were subjected to a normal temperature discharge DCR test and a normal temperature high rate cycle test. The specific test methods are as follows:
[0079] Normal temperature discharge DCR test: Set the temperature to 25 ℃, perform charge and discharge operations in the voltage range of 2.5-4.5 V, first charge to 4.25 V at a constant current of 1 C, then discharge to 50% SOC at a constant current of 1C, record the discharge voltage when the discharge capacity reaches 50% SOC as V1, then perform a 2 C constant current discharge for 30 s at a current I, record the discharge voltage at this time as V2, calculate the discharge DCR value, and the calculation method is DCR discharge = |V1-V2| / I;
[0080] Room temperature high-rate cycle performance test: set the temperature to 25 ℃, charge to 4.25 V at 2 C constant current, and then discharge to 2.5 V at 1 C constant current, which is recorded as the initial discharge capacity; the test is terminated when the capacity drops to 80% of the initial capacity, and the number of cycles is recorded.
[0081] The test results are shown in Table 2 below:
[0082] Table 2
[0083]
[0084] As can be seen from Table 1, the present invention adopts an electrolyte containing an appropriate amount of sodium salt additives and an organic film-forming agent to coordinate the cyclic small battery charge and discharge operation of room temperature charging and high temperature static discharge, so that the lithium battery prepared in Examples 1-14 has both excellent cycle performance and a low DCR value. Among them, Example 10 uses a silicon-carbon negative electrode material as the negative electrode active material of the lithium battery. Since the kinetics of the silicon-carbon negative electrode is slightly better than that of the silicon-oxygen system, the performance of the lithium battery prepared therefrom is slightly better than that of Example 2; different types of electrolyte lithium salts or solvents are used to prepare lithium batteries (Examples 11 and 12), which have little effect on the performance of the battery; relative to Example 2, Example 13 reduces the content of lithium salt in the electrolyte. If the content of lithium salt is too little, the conductivity of the electrolyte is low, resulting in relatively poor performance of the lithium battery, while Example 14 increases the amount of lithium salt in the electrolyte relative to Example 2, and the performance of the lithium battery is reduced instead. This is because the excessive lithium salt in the electrolyte causes a large increase in the viscosity of the electrolyte, which is not conducive to ion transmission, thereby resulting in relatively deteriorated battery performance.
[0085] It can be seen from Examples 2, 4, 5 and Comparative Examples 1 and 3 that when Y / X is too small or too large, the cycle life of the battery will be significantly reduced, and when Y / X is too large, the DCR value of the battery is relatively large. When 1≤Y / X≤10, the lithium batteries prepared in Examples 1-9 are cycled and discharged until the capacity drops to 80% of the initial capacity, and the corresponding number of cycles is not less than 1500 cycles, and the DCR is less than 33 mΩ; 2≤Y / X≤5 corresponding to Examples 2, 3 and Examples 6-9 has a cycle performance of not less than 1600 cycles, and the number of cycles of Examples 2 and 6-9, where the Y / X value is 4, is not less than 1700 cycles, and the DCR value is less than 30 mΩ.
[0086] It can be seen from Example 2 and Comparative Examples 1 and 2 that, compared with Comparative Example 1 in which no sodium salt additive is added, adding an appropriate amount of sodium salt additive in Example 2 can significantly improve the cycle performance of the battery and reduce the battery impedance; and as the content of the sodium salt additive increases, the battery impedance is reduced, but the cycle life of the battery is greatly reduced. This is because the sodium salt additive is excessive, and the SEI film formed in the early stage contains a large amount of sodium-containing inorganic components. After standing at high temperature, as the sodium-containing compounds dissolve, the SEI integrity is greatly reduced. Although the DCR is reduced, the side reactions are serious during the cycle, which deteriorates the cycle performance.
[0087] It can be seen from Example 2 and Comparative Examples 3 and 4 that the lithium battery prepared in Comparative Example 3 without adding organic film-forming additives has low battery impedance, but the cycle performance is greatly reduced. The number of cycles corresponding to the capacity dropping to 80% of the initial capacity during cyclic charge and discharge is only 1281. This is because the main component of the SEI film is a sodium-containing compound. As the sodium-containing compound dissolves during subsequent high-temperature standing, the integrity of the SEI film is low, affecting the cycle performance of the battery. However, when an excessive amount of organic film-forming additives is included, the organic component content in the SEI film formed in the early stage is relatively high, and the porosity of the SEI film after high-temperature standing is low, resulting in a high battery impedance, and the volume expansion of the negative electrode cannot be effectively alleviated, affecting the cycle performance of the battery.
[0088] As can be seen from Comparative Example 5, the conventional chemical formation method is used for chemical formation treatment. Due to the lack of high-temperature standing process, the sodium-containing compounds in the SEI film cannot be effectively dissolved to form a porous loose structure, resulting in a high initial DCR of the prepared lithium battery, and the expansion and contraction of the negative electrode cannot be effectively alleviated, resulting in the continuous damage of the SEI film during the cyclic charge and discharge process, deteriorating the cycle performance. In addition, Comparative Example 6 uses a large current for charge and discharge cycles, and the prepared battery cycle performance is low. This is because the SEI film formed under a large current is relatively loose, and the dissolution of inorganic components under subsequent high-temperature standing will cause the destruction of the SEI, increase side reactions, and deteriorate the battery cycle performance.
[0089] It can be seen from Example 2 and Comparative Examples 7-9 that the temperature of the charging process in the formation stage and the temperature of the standing and discharging process will affect the impedance and cycle performance of the battery. For example, the temperature of the charging process in Comparative Example 7 is 60°C. At this temperature, during the formation of the SEI film, the inorganic components in the SEI film will be dissolved, resulting in a high content of organic components in the SEI film and a large impedance; while the temperature of the standing and discharging process in Comparative Example 8 is 80°C. Due to the high temperature, the organic and inorganic components in the SEI film are dissolved or decomposed, resulting in serious damage to the SEI film, resulting in poor cycle performance of the prepared lithium battery. However, if the temperature of the standing and discharging process is too low, for example, in Comparative Example 9, the standing and discharging operations are performed at 25°C. Due to the low temperature, the inorganic components in the SEI film cannot be fully dissolved, resulting in an increase in the interface impedance. At the same time, the SEI film with a low porosity cannot effectively alleviate the change in the volume of the negative electrode.
[0090] In addition, if the high-temperature standing time is too long (Comparative Example 10) or too short (Comparative Example 11), it will also affect the dissolution of inorganic and organic components, thereby affecting the impedance and cycle performance of the battery.
[0091] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. An electrolyte, characterized in that: The electrolyte comprises an electrolyte lithium salt, a sodium salt additive and an organic film-forming additive, and satisfies the following relationship: 0.3wt%≤X≤2wt%, 0.9wt%≤Y≤5wt%, and 1≤Y / X≤10, 10wt%≤X+Z≤17wt%; Wherein, X is the mass percentage of the sodium salt additive in the electrolyte; Y is the mass percentage of the organic film-forming additive in the electrolyte; Z is the mass percentage of the electrolyte lithium salt in the electrolyte; The sodium salt additive is selected from one or more of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium hexafluoroarsenate, sodium bis(oxalatoborate), sodium difluorooxalatoborate, sodium difluorophosphate, sodium bis(fluorosulfonyl)imide, and sodium bis(trifluoromethylsulfonyl)imide; The organic film-forming additive is selected from one or more of vinylene carbonate, vinyl ethylene carbonate, 1,3-propylene sultone, triphenyl phosphite, acrylamide, N,N-dimethylacrylamide, ethoxylated trimethylolpropane triacrylate, and pentaerythritol triacrylate.
2. The electrolyte according to claim 1, characterized in that 2≤Y / X≤5.
3. The electrolyte according to claim 1, characterized in that The electrolyte lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium difluorophosphate, lithium bisoxalatoborate, lithium difluorooxalatoborate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, and lithium difluorobis(oxalatophosphate).
4. The electrolyte according to claim 1, characterized in that The electrolyte further comprises an organic solvent; the organic solvent is selected from one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, fluoroethylene carbonate, fluoropropylene carbonate, and fluoroethyl methyl carbonate.
5. A lithium battery, characterized in that: The lithium battery comprises the electrolyte according to any one of claims 1 to 4; The lithium battery also includes a negative electrode plate, which includes a current collector and a negative electrode active layer arranged on at least one side of the current collector along the thickness direction, the negative electrode active layer includes a negative electrode active material, and the negative electrode active material includes a silicon-based negative electrode material; the silicon-based negative electrode material includes one or more of silicon element, silicon-carbon material, and silicon-oxygen material.
6. A method for liquid injection formation of a lithium battery as claimed in claim 5, characterized in that: The following steps are involved: S1, liquid injection: injecting electrolyte into the shell of the lithium battery; S2, formation: at temperature T1, charge the lithium battery after injection with a constant current of I1 to the upper limit voltage U1; then place it at temperature T2 for 12-24 hours, and then discharge it at temperature T2 with a constant current of I2 to the lower limit voltage U2; wherein, T1≤45℃, 45℃≤T2≤60℃; I1≤0.1℃, I2≤0.1℃; 3.2V≤U1≤3.7V, 2.0V≤U2≤2.8V; S3, repeat the charge and discharge cycle of S2 1-3 times.
7. The liquid injection formation method according to claim 6, characterized in that: 25 ℃≤T1≤35 ℃。 8. The liquid injection formation method according to claim 6, characterized in that: 0.05 C ≤ I1 ≤ 0.1 C and / or 0.05 C ≤ I2 ≤ 0.1 C.
9. The liquid injection formation method according to claim 8, characterized in that: I1=I2.