Negative electrode material loaded with nano silicon porous carbon and preparation method of negative electrode material

Hollow porous structures were prepared by synergistic enzymatic hydrolysis of starch using maltotriase and amyloglucosidase. Combined with treatment with ammonium chloride and sodium carboxymethyl cellulose, the volume expansion and conductivity issues of nano-silicon anode materials were solved, resulting in anode materials with high cycle stability and rapid lithium-ion transport.

CN119008893APending Publication Date: 2024-11-22GANZHOU RUIFUTE TECHNOLOGY CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411105207.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Nano-silicon, as an anode material in lithium-ion batteries, suffers from problems such as huge volume expansion, structural instability, and poor electronic conductivity, leading to decreased cycle performance and pulverization of electrode materials, which affects battery capacity and safety.

Method used

Hollow porous starch was prepared by synergistic enzymatic hydrolysis of starch using maltotriase and amyloglucosidase. Ammonium chloride was used as a protective agent and nitrogen source. After high-temperature carbonization, sodium carboxymethyl cellulose was coated and doped with cerium to form a supported nano-silicon porous carbon structure.

Benefits of technology

It effectively suppresses the volume expansion of nano-silicon, improves cycle stability and electronic conductivity, enhances lithium-ion transport rate, and improves the cycle performance and safety of anode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008893A_ABST
    Figure CN119008893A_ABST
Patent Text Reader

Abstract

The invention provides a nano-silicon-loaded porous carbon negative electrode material and a preparation method thereof, and belongs to the technical field of preparation of negative electrode materials. The preparation process comprises the following steps: preparing hollow porous starch; preparing a porous carbon loaded nano silicon precursor; and preparing the negative electrode material. According to the preparation method disclosed by the invention, the starch emulsion is firstly subjected to enzymolysis by using the maltotriase and then is subjected to enzymolysis by using the amyloglucosidase, and a hydrolysis mode of the maltotriase from inside to outside is cooperated with the amyloglucosidase to promote the formation of an internal cavity structure of starch granules, so that the starch with a relatively large internal cavity structure and a relatively large size can be prepared. According to the hollow porous starch with relatively complete particle structure and better pore structure, the nano silicon particles are loaded in the hollow porous starch, and volume expansion of silicon in an electrochemical cycle process can be greatly buffered through a starch skeleton and the pore structure, so that pulverization of the material is effectively inhibited, and the cycle performance of the negative electrode material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of negative electrode material preparation, and in particular to a negative electrode material loaded with nano-silicon porous carbon and a preparation method thereof. Background Art

[0002] As the global demand for sustainable energy continues to grow, the optimization and improvement of the performance of lithium-ion batteries, as one of the key technologies for energy storage, has received widespread attention. Especially in application fields such as electric vehicles and energy storage systems, high energy density, long cycle life and fast charge and discharge capabilities have become important indicators for evaluating the performance of lithium-ion batteries. In lithium-ion batteries, the choice of negative electrode materials directly affects the overall performance of the battery.

[0003] Traditional commercial lithium-ion battery negative electrode materials mainly rely on graphite, which has a theoretical specific capacity of about 372mAh / g. However, in order to meet the growing demand for energy density, it is particularly important to explore new negative electrode materials with higher specific capacity. Nanosilicon is regarded as one of the ideal candidates for the next generation of lithium-ion battery negative electrode materials due to its extremely high theoretical specific capacity. Compared with graphite, nanosilicon can absorb more lithium ions during the lithium ion embedding process, thereby significantly improving the energy density of the battery. However, nanosilicon faces major challenges in practical applications, mainly including huge volume expansion, structural instability and poor electronic conductivity. These factors lead to a sharp decline in cycle performance and pulverization of electrode materials, destroying the contact between electrode materials and current collectors, causing active materials to detach from the pole pieces, causing rapid attenuation of battery capacity, and expansion will also generate large stress inside the battery, squeezing the pole pieces and increasing the risk of pole piece fracture.

[0004] Therefore, we proposed a negative electrode material loaded with nano-silicon porous carbon, which can inhibit the expansion of nano-silicon and has high cycle stability, and a preparation method thereof. Summary of the invention

[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide a negative electrode material loaded with nano-silicon porous carbon and a preparation method thereof.

[0006] A method for preparing a negative electrode material loaded with nano-silicon porous carbon comprises the following steps:

[0007] S1: Preparation of hollow porous starch

[0008] Hollow porous starch can be prepared by first enzymatically hydrolyzing starch with maltotriase and then enzymatically hydrolyzing starch with amyloglucosidase;

[0009] S2: Preparation of porous carbon-supported nanosilicon precursor

[0010] The ammonium chloride and the hollow porous starch are mixed and then added with deionized water and stirred. During the stirring process, nano silicon powder is added, and after being stirred evenly, gelation and aging are performed, and then freezing and soaking are performed to obtain a porous carbon-loaded nano silicon precursor;

[0011] S3: Preparation of negative electrode materials

[0012] Sodium carboxymethyl cellulose is dissolved in deionized water, and then a porous carbon-loaded nano-silicon precursor is added, followed by high-temperature carbonization under vacuum to obtain a negative electrode material.

[0013] Furthermore, the preparation of the hollow porous starch in step S1 specifically comprises the following steps:

[0014] S1.1: Weigh 30-40 parts by weight of corn starch, prepare a starch emulsion with a concentration of 10-12% (w / v) with 0.1 mol / L disodium hydrogen phosphate-citric acid buffer solution, and swell the starch emulsion in a constant temperature water bath with a magnetic stirrer at 60-65°C for 0.5-1h to obtain a starch emulsion;

[0015] S1.2: The temperature of the starch emulsion is adjusted to 50-55°C, and maltotriose enzyme is added to react for 5-6 hours. After the reaction is completed, the starch emulsion is immediately placed in ice water for 10-15 minutes to rapidly cool down and reduce the reaction rate of the enzyme. Then, the pH is adjusted to 11-12 with 2 mol / L sodium hydroxide solution and reacted for 8-10 minutes to obtain the starch emulsion after enzyme inactivation;

[0016] S1.3: The temperature of the starch emulsion after enzyme inactivation is adjusted to 50-55°C, and amyloglucosidase is added for enzymatic hydrolysis for 5-6 hours. After the reaction is completed, the starch emulsion is immediately placed in ice water for 10-15 minutes for rapid cooling to reduce the reaction rate of the enzyme, and then the pH is adjusted to 11-12 with 2 mol / L sodium hydroxide solution for reaction for 8-10 minutes to obtain a starch emulsion after enzyme inactivation again;

[0017] S1.4: The pH of the starch emulsion after enzyme inactivation is adjusted to neutral with 2 mol / L hydrogen chloride solution, the neutral starch emulsion is centrifuged to obtain a precipitate, the precipitate is repeatedly washed with distilled water for 5-6 times, and then dried in an oven at 45-50°C for 40-48 hours, and then ground and crushed and passed through a 100-120 mesh sieve to obtain hollow porous starch.

[0018] Furthermore, step S2 of preparing the porous carbon-supported nano-silicon precursor specifically comprises the following steps:

[0019] S2.1: Weigh 1-2 parts by weight of ammonium chloride and 2-3 parts by weight of hollow porous starch, add 20-30 parts by weight of deionized water after mixing, and stir magnetically for 2-3 hours. During the magnetic stirring process, add 0.2-0.5 parts by weight of nano silicon powder with a particle size of 20-30 nm, and stir evenly to obtain a starch complex suspension;

[0020] S2.2: The starch complex suspension is placed in a water bath and heated at 80-90°C while being stirred continuously for 30-50 minutes to obtain a gelatinized starch complex suspension. The gelatinized starch complex suspension is further heated at 80-90°C for 10-12 minutes and then aged at room temperature for 10-12 hours to obtain an aged starch complex suspension.

[0021] S2.3: The aged starch complex suspension is frozen at -25°C to -20°C for 10-12 hours, then cooled to room temperature in air, and then soaked in acetone for 20-30 minutes to obtain a porous carbon-loaded nano-silicon precursor.

[0022] Furthermore, step S3 of preparing the negative electrode material specifically includes the following steps:

[0023] S3.1: dissolving 1-2 parts by weight of sodium carboxymethyl cellulose in 200-300 parts by weight of deionized water, and stirring evenly to obtain a gel solution, and then adding the porous carbon-supported nano-silicon precursor to the gel solution, stirring evenly to obtain a mixed gel solution;

[0024] S3.2: Add 0.01-0.02 parts by weight of cerium nitrate solution dropwise to the mixed gel solution, stir evenly, and freeze-dry to obtain a silicon / starch@cerium / sodium carboxymethyl cellulose precursor;

[0025] S3.3: Place the silicon / starch@cerium / sodium carboxymethyl cellulose precursor in a tubular resistance furnace with an inert gas as the protective atmosphere, carbonize it at high temperature under vacuum, cool it naturally to room temperature, wash it repeatedly with deionized water 2-3 times, and dry it to obtain the negative electrode material.

[0026] Furthermore, in step S1.2, the amount of maltotriosidase added is: the mass ratio of starch to maltotriosidase is 50-100:1.

[0027] Furthermore, the amount of amyloglucosidase added in step S1.3 is: the mass ratio of starch to amyloglucosidase is 50-100:1.

[0028] Furthermore, the starch in step S1.1 is specifically one or more of corn starch, wheat starch, potato starch and tapioca starch.

[0029] Furthermore, in step S3.3, the inert gas is nitrogen.

[0030] Furthermore, in step S3.3, the inert gas flow rate is 75-80 mL / min, the carbonization heating rate is 2-3°C / min, the temperature is 700-800°C, the carbonization vacuum is 10-15 Pa, and the carbonization time is 3-4 h.

[0031] A negative electrode material loaded with nano silicon porous carbon is prepared by a method for preparing a negative electrode material loaded with nano silicon porous carbon.

[0032] Compared with the prior art, the present invention has at least the following beneficial effects:

[0033] 1. The present invention first enzymatically hydrolyzes the starch emulsion with maltotriase and then with amyloglucosidase. The maltotriase can hydrolyze starch granules to generate holes and cavities on the surface and inside of the starch granules, and the maltotriase has an "inside-out" centripetal hydrolysis mechanism, so that a larger cavity is generated inside the granules, and the amyloglucosidase has an "outside-in" mode of action, which can effectively increase the number and pore size of the starch granule pores. By first enzymatically hydrolyzing with maltotriase and then with amyloglucosidase, the "inside-out" hydrolysis mode of maltotriase cooperates with amyloglucosidase to promote the formation of the internal cavity structure of the starch granules, and can prepare a hollow porous starch with a larger internal cavity structure of the starch, a relatively complete particle structure, and a better pore structure. The nano-silicon particles are loaded in the hollow porous starch, and the volume expansion of silicon during the electrochemical cycle can be greatly buffered by the starch skeleton and the pore structure, effectively inhibiting the pulverization of the material and improving the cycle performance of the negative electrode material.

[0034] 2. The ammonium chloride added in the present invention is both a protective agent and a nitrogen source. The added ammonium chloride plays a dual role in the carbonization process. The HCl generated by the thermal decomposition of ammonium chloride can promote the chemical dehydration of the hollow porous starch molecular chain, thereby slowly destroying the crystalline structure inside the hollow porous starch particles at a relatively low temperature. The melting phenomenon of the crystalline structure no longer occurs during high-temperature carbonization, which is beneficial to the maintenance of the original morphology and pore structure of the hollow porous starch. In addition, the NH3 generated by the thermal decomposition of ammonium chloride can undergo a dehydration condensation reaction with the hydroxyl groups on the hollow porous starch molecular chain to form a bond, thereby achieving nitrogen doping. The doping of nitrogen elements provides more active sites for the adsorption of lithium ions, which can accelerate the ion transmission rate of the negative electrode material and promote the transfer of electrons and ions, thereby achieving stable cycle performance.

[0035] 3. The outer layer of the sodium carboxymethyl cellulose coated in the present invention is coated on the porous carbon-supported nano-silicon after vacuum high-temperature carbonization, and a relatively dense carbon layer can be carbonized on the surface of the porous carbon-supported nano-silicon, isolating the rich specific surface area inside the negative electrode material from direct contact with the electrolyte, preventing the formation of excessive SEI film to ensure the reversible capacity of the negative electrode material, and enhancing the cycle stability of the negative electrode material.

[0036] 4. The present invention dopes cerium into the outer coated sodium carboxymethyl cellulose. After high-temperature calcination, the cerium ions doped into the carbon layer are converted into cerium oxides, and the cerium oxides are interspersed in the carbon layer. The doping of cerium can reduce the oxygen content of the carbon layer and reduce the occurrence of side reactions, thereby reducing the impedance and increasing the lithium ion diffusion coefficient. In addition, the doping of cerium improves the lithium ion conductivity and ion transfer rate of the negative electrode material, while enhancing the toughness of the carbon layer, further improving the cycle performance of the negative electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the present disclosure and, together with the description, further serve to explain the principles of the present disclosure and to enable those skilled in the relevant art to make and use the present disclosure.

[0038] Figure 1 This is a flow chart of a method for preparing a negative electrode material loaded with nano-silicon porous carbon used in an embodiment of the present invention. DETAILED DESCRIPTION

[0039] The following is a detailed description of a negative electrode material loaded with nano-silicon porous carbon and a preparation method thereof provided by the present invention in conjunction with the accompanying drawings and specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternative methods to implement some known technologies; and the accompanying drawings are only for a more specific description of the embodiments, and are not intended to specifically limit the present invention.

[0040] Example 1

[0041] A negative electrode material loaded with nano-silicon porous carbon and a preparation method thereof, such as Figure 1 As shown, the following steps are included:

[0042] S1: Preparation of hollow porous starch

[0043] S1.1: Weigh 30 parts by weight of corn starch and prepare a starch emulsion with a concentration of 10% (w / v) using 0.1 mol / L disodium hydrogen phosphate-citric acid buffer solution, and swell the starch emulsion in a 60°C constant temperature water bath with a magnetic stirrer for 0.5 h to obtain a starch emulsion;

[0044] S1.2: The temperature of the starch emulsion was adjusted to 50°C, and maltotriosidase was added to react for 5 hours. The mass ratio of starch to maltotriosidase was 50:1. After the reaction, the starch emulsion was immediately placed in ice water for 10 minutes to rapidly cool down and reduce the reaction rate of the enzyme. The pH was then adjusted to 11 with 2 mol / L sodium hydroxide solution and reacted for 8 minutes to obtain the enzyme-inactivated starch emulsion.

[0045] S1.3: The temperature of the starch emulsion after enzyme inactivation was adjusted to 50°C, and amyloglucosidase was added for enzymatic hydrolysis for 5 hours. The mass ratio of starch to amyloglucosidase was 50:1. After the reaction was completed, the starch emulsion was immediately placed in ice water for 10 minutes for rapid cooling to reduce the reaction rate of the enzyme. The pH was then adjusted to 1 with 2 mol / L sodium hydroxide solution and reacted for 8 minutes to obtain a starch emulsion after enzyme inactivation again.

[0046] S1.4: The pH of the starch emulsion after the enzyme is inactivated again is adjusted to neutral with a 2 mol / L hydrogen chloride solution, the neutral starch emulsion is centrifuged to obtain a precipitate, the precipitate is repeatedly washed with distilled water for 5 times, and then dried in an oven at 45°C for 40 hours, and then ground and crushed and passed through a 100-mesh sieve to obtain a hollow porous starch;

[0047] S2: Preparation of porous carbon-supported nanosilicon precursor

[0048] S2.1: Weigh 1 part by weight of ammonium chloride and 2 parts by weight of hollow porous starch, add 20 parts by weight of deionized water after mixing, and stir magnetically for 2 hours. During the magnetic stirring process, add 0.2 parts by weight of nano silicon powder with a particle size of 20 nm, and stir evenly to obtain a starch complex suspension;

[0049] S2.2: The starch complex suspension is placed in a water bath and heated at 80°C while being stirred continuously for 30 minutes to obtain a gelatinized starch complex suspension. The gelatinized starch complex suspension is further heated at 80°C for 10 minutes and then aged at room temperature for 10 hours to obtain an aged starch complex suspension.

[0050] S2.3: The aged starch complex suspension was frozen at -25°C for 10 hours, then cooled to room temperature in air, and then soaked in acetone for 20 minutes to obtain a porous carbon-supported nano-silicon precursor;

[0051] S3: Preparation of negative electrode materials

[0052] S3.1: Dissolve 1 part by weight of sodium carboxymethyl cellulose in 200 parts by weight of deionized water, and stir evenly to obtain a gel solution, then add the porous carbon-supported nano-silicon precursor to the gel solution, stir evenly to obtain a mixed gel solution;

[0053] S3.2: Add 0.01 parts by weight of cerium nitrate solution dropwise to the mixed gel solution, stir evenly, and freeze-dry to obtain a silicon / starch@cerium / sodium carboxymethyl cellulose precursor;

[0054] S3.3: Place the silicon / starch@cerium / sodium carboxymethyl cellulose precursor in a tubular resistance furnace, use nitrogen as the protective atmosphere with a flow rate of 75 mL / min, heat to 700°C at a heating rate of 2°C / min, carbonize and keep warm for 3 hours at a high temperature under a vacuum of 10 Pa, then cool naturally to room temperature, wash repeatedly with deionized water twice, and obtain the negative electrode material after drying.

[0055] Example 2

[0056] A negative electrode material loaded with nano-silicon porous carbon and a preparation method thereof, such as Figure 1 As shown, the following steps are included:

[0057] S1: Preparation of hollow porous starch

[0058] S1.1: Weigh 30 parts by weight of corn starch and prepare a starch emulsion with a concentration of 10% (w / v) using 0.1 mol / L disodium hydrogen phosphate-citric acid buffer solution. Place the starch emulsion in a constant temperature water bath with a magnetic stirrer at 65°C for swelling for 1 hour to obtain a starch emulsion;

[0059] S1.2: The temperature of the starch emulsion was adjusted to 55°C, and maltotriosidase was added to react for 6 hours. The mass ratio of starch to maltotriosidase was 50:1. After the reaction, the starch emulsion was immediately placed in ice water for 15 minutes to rapidly cool down and reduce the reaction rate of the enzyme. The pH was then adjusted to 11 with 2 mol / L sodium hydroxide solution and reacted for 10 minutes to obtain the enzyme-inactivated starch emulsion.

[0060] S1.3: The temperature of the starch emulsion after enzyme inactivation was adjusted to 55°C, and amyloglucosidase was added for enzymatic hydrolysis for 6 hours. The mass ratio of starch to amyloglucosidase was 50:1. After the reaction was completed, the starch emulsion was immediately placed in ice water for 15 minutes for rapid cooling to reduce the reaction rate of the enzyme. The pH was then adjusted to 11 with 2 mol / L sodium hydroxide solution and reacted for 10 minutes to obtain a starch emulsion after enzyme inactivation again.

[0061] S1.4: The pH of the starch emulsion after the enzyme is inactivated again is adjusted to neutral with a 2 mol / L hydrogen chloride solution, the neutral starch emulsion is centrifuged to obtain a precipitate, the precipitate is repeatedly washed with distilled water for 6 times, and then dried in an oven at 50°C for 48 hours, and then ground and crushed and passed through a 120-mesh sieve to obtain a hollow porous starch;

[0062] S2: Preparation of porous carbon-supported nanosilicon precursor

[0063] S2.1: Weigh 1 part by weight of ammonium chloride and 2 parts by weight of hollow porous starch, add 20 parts by weight of deionized water after mixing, and stir magnetically for 3 hours. During the magnetic stirring process, add 0.2 parts by weight of nano silicon powder with a particle size of 20 nm, and stir evenly to obtain a starch complex suspension;

[0064] S2.2: The starch complex suspension is placed in a water bath and heated at 90°C while being stirred continuously for 50 minutes to obtain a gelatinized starch complex suspension. The gelatinized starch complex suspension is further heated at 90°C for 12 minutes and then aged at room temperature for 12 hours to obtain an aged starch complex suspension.

[0065] S2.3: The aged starch complex suspension was frozen at -20°C for 12 hours, then cooled to room temperature in air, and then soaked in acetone for 30 minutes to obtain a porous carbon-supported nano-silicon precursor;

[0066] S3: Preparation of negative electrode materials

[0067] S3.1: Dissolve 1 part by weight of sodium carboxymethyl cellulose in 200 parts by weight of deionized water, and stir evenly to obtain a gel solution, then add the porous carbon-supported nano-silicon precursor to the gel solution, stir evenly to obtain a mixed gel solution;

[0068] S3.2: Add 0.01 parts by weight of cerium nitrate solution dropwise to the mixed gel solution, stir evenly, and freeze-dry to obtain a silicon / starch@cerium / sodium carboxymethyl cellulose precursor;

[0069] S3.3: Place the silicon / starch@cerium / sodium carboxymethyl cellulose precursor in a tubular resistance furnace, use nitrogen as the protective atmosphere with a flow rate of 80 mL / min, heat to 800°C at a heating rate of 3°C / min, carbonize and keep warm for 4 hours at a high temperature under a vacuum of 15 Pa, cool naturally to room temperature, and then wash repeatedly with deionized water for 3 times. After drying, the negative electrode material is obtained.

[0070] Example 3

[0071] A negative electrode material loaded with nano-silicon porous carbon and a preparation method thereof, such as Figure 1 As shown, the following steps are included:

[0072] S1: Preparation of hollow porous starch

[0073] S1.1: Weigh 40 parts by weight of corn starch and prepare a starch emulsion with a concentration of 12% (w / v) using 0.1 mol / L disodium hydrogen phosphate-citric acid buffer solution, and swell the starch emulsion in a 60°C constant temperature water bath with a magnetic stirrer for 0.5 h to obtain a starch emulsion;

[0074] S1.2: The temperature of the starch emulsion was adjusted to 50°C, and maltotriosidase was added to react for 5 hours. The mass ratio of starch to maltotriosidase was 100:1. After the reaction was completed, the starch emulsion was immediately placed in ice water for 10 minutes to rapidly cool down and reduce the reaction rate of the enzyme. The pH was then adjusted to 12 with 2 mol / L sodium hydroxide solution and reacted for 8 minutes to obtain an enzyme-inactivated starch emulsion.

[0075] S1.3: The temperature of the starch emulsion after enzyme inactivation was adjusted to 50°C, and amyloglucosidase was added for enzymatic hydrolysis for 5 hours. The mass ratio of starch to amyloglucosidase was 100:1. After the reaction was completed, the starch emulsion was immediately placed in ice water for 10 minutes for rapid cooling to reduce the reaction rate of the enzyme. The pH was then adjusted to 12 with 2 mol / L sodium hydroxide solution and reacted for 8 minutes to obtain a starch emulsion after enzyme inactivation again.

[0076] S1.4: The pH of the starch emulsion after the enzyme is inactivated again is adjusted to neutral with a 2 mol / L hydrogen chloride solution, the neutral starch emulsion is centrifuged to obtain a precipitate, the precipitate is repeatedly washed with distilled water for 5 times, and then dried in an oven at 45°C for 40 hours, and then ground and crushed and passed through a 100-mesh sieve to obtain a hollow porous starch;

[0077] S2: Preparation of porous carbon-supported nanosilicon precursor

[0078] S2.1: Weigh 2 parts by weight of ammonium chloride and 3 parts by weight of hollow porous starch, add 30 parts by weight of deionized water after mixing, and stir magnetically for 2 hours. During the magnetic stirring process, add 0.5 parts by weight of nano silicon powder with a particle size of 30 nm, and stir evenly to obtain a starch complex suspension;

[0079] S2.2: The starch complex suspension is placed in a water bath and heated at 80°C while being stirred continuously for 30 minutes to obtain a gelatinized starch complex suspension. The gelatinized starch complex suspension is further heated at 80°C for 10 minutes and then aged at room temperature for 10 hours to obtain an aged starch complex suspension.

[0080] S2.3: The aged starch complex suspension was frozen at -25°C for 10 hours, then cooled to room temperature in air, and then soaked in acetone for 20 minutes to obtain a porous carbon-supported nano-silicon precursor;

[0081] S3: Preparation of negative electrode materials

[0082] S3.1: dissolving 2 parts by weight of sodium carboxymethyl cellulose in 300 parts by weight of deionized water, and stirring evenly to obtain a gel solution, and then adding the porous carbon-supported nano-silicon precursor to the gel solution, stirring evenly to obtain a mixed gel solution;

[0083] S3.2: Add 0.02 parts by weight of cerium nitrate solution dropwise to the mixed gel solution, stir evenly, and freeze-dry to obtain a silicon / starch@cerium / sodium carboxymethyl cellulose precursor;

[0084] S3.3: Place the silicon / starch@cerium / sodium carboxymethyl cellulose precursor in a tubular resistance furnace, use nitrogen as the protective atmosphere with a flow rate of 75 mL / min, heat to 700°C at a heating rate of 2°C / min, carbonize and keep warm for 3 hours at a high temperature under a vacuum of 10 Pa, then cool naturally to room temperature, wash repeatedly with deionized water twice, and obtain the negative electrode material after drying.

[0085] Comparative Example 1

[0086] Compared with Example 1, the difference of Comparative Example 1 is that Comparative Example 1 removes step S1.2, replaces the starch emulsion after enzyme inactivation in step S1.3 with starch emulsion of equal mass, and prepares the negative electrode material without changing the other steps, which is recorded as Comparative Example 1.

[0087] Comparative Example 2

[0088] Compared with Example 1, the difference of Comparative Example 2 is that Comparative Example 2 removes step S1.3, replaces the starch emulsion after enzyme inactivation in step S1.4 with starch emulsion after enzyme inactivation of the same mass, and prepares the negative electrode material without changing the other steps, which is recorded as Comparative Example 2.

[0089] Comparative Example 3

[0090] Compared with Example 1, the difference of Comparative Example 3 is that step S1 is removed in Comparative Example 3, and the hollow porous starch in step S2.1 is replaced with corn starch of equal mass, and the other steps remain unchanged to prepare the negative electrode material, which is recorded as Comparative Example 3.

[0091] Comparative Example 4

[0092] Compared with Example 1, the difference of Comparative Example 4 is that in Comparative Example 4, the maltotriase in step S1.2 is replaced by an equal mass of amyloglucosidase, and the amyloglucosidase in step S1.3 is replaced by an equal mass of maltotriase, and the remaining steps remain unchanged to prepare the negative electrode material, which is recorded as Comparative Example 4.

[0093] Cycle performance test:

[0094] The negative electrode materials prepared in Examples 1-3 and Comparative Examples 1-4 were assembled into button-type battery samples to test the electrochemical performance: the positive electrode of the battery was a sodium sheet, and the negative electrode materials prepared in Examples 1-3 and Comparative Examples 1-4 were respectively mixed with the conductive agent acetylene black and the binder polytetrafluoroethylene emulsion in an aqueous solution at a weight ratio of 80:15:5, and then pressed on a copper foil to obtain a negative electrode sheet, a 1 mol / L lithium hexafluorophosphate solution of ethylene carbonate and dimethyl carbonate was used as an electrolyte, and Celgard2400 polypropylene microporous membrane was used as a diaphragm, and assembled into a CR2025 type button lithium ion battery for charge and discharge. The battery charge and discharge test was carried out on the LAND battery system, and the charge and discharge voltage range was 0-2V. The cycle performance test results refer to Table 1.

[0095] Table 1. Cyclic performance test results of negative electrode materials prepared in Examples 1-3 and Comparative Examples 1-4

[0096] Capacity retention after 200 cycles (%) Example 1 92.32 Example 2 92.13 Example 3 92.18 Comparative Example 1 88.34 Comparative Example 2 88.43 Comparative Example 3 80.45 Comparative Example 4 85.23

[0097] It can be seen from Table 1 that the negative electrode material prepared in the embodiment has excellent cycle stability. It can be seen from the data of comparative examples 1-3 that the cycle performance of comparative examples 1-2 is higher than that of comparative example 3 but lower than that of the embodiment, indicating that the pore structure of the hollow porous starch prepared by enzymatic hydrolysis of starch by maltotriosidase and amyloglucosidase is better than the effect of enzymatic hydrolysis by a single enzyme, reflecting that maltotriosidase and amyloglucosidase have a synergistic effect on the enzymatic hydrolysis of starch, which is beneficial to promote the formation of the cavity structure inside the starch granules.

[0098] The cycle performance of Comparative Example 4 is worse than that of the embodiment, indicating that the pore structure of the hollow porous starch prepared by first performing maltotriase hydrolysis and then performing amyloglucosidase hydrolysis is better than that prepared by first performing amyloglucosidase hydrolysis and then performing maltotriase hydrolysis, indicating that first hydrolyzing the starch emulsion with maltotriase and then hydrolyzing the starch emulsion with amyloglucosidase is beneficial to improving the cycle performance of the polar material.

[0099] Comparative Example 5

[0100] Compared with Example 1, the difference of Comparative Example 5 is that the ammonium chloride in step S2.1 is removed in Comparative Example 5, and the other steps remain unchanged to prepare the negative electrode material, which is recorded as Comparative Example 5.

[0101] The negative electrode material prepared in Comparative Example 5 was assembled into a CR2025 type button lithium ion battery according to the above method for charge and discharge. The battery charge and discharge test was carried out on a LAND battery system with a charge and discharge voltage range of 0-2 V. The cycle performance test results are shown in Table 2.

[0102] Table 2. Cyclic performance test results of Examples 1-3 and Comparative Example 5

[0103] Capacity retention after 200 cycles (%) Example 1 92.32 Example 2 92.13 Example 3 92.18 Comparative Example 5 83.45

[0104] It can be seen from the data in Table 2 that the data of Comparative Example 5 is lower than that of the embodiment, indicating that the cycle performance of the negative electrode material can be improved after adding ammonium chloride.

[0105] Comparative Example 6

[0106] Compared with Example 1, the difference of Comparative Example 6 is that, in Comparative Example 6, step S3.1 is replaced by freeze-drying the mixed gel solution to obtain a mixed gel precursor, and the silicon / starch@cerium / sodium carboxymethyl cellulose precursor in S3.3 is replaced by an equal mass of mixed gel precursor, and the remaining steps remain unchanged to prepare the negative electrode material, which is recorded as Comparative Example 6.

[0107] Comparative Example 7

[0108] Compared with Example 1, the difference of Comparative Example 7 is that Comparative Example 7 removes steps S3.1-S3.2, replaces the silicon / starch@cerium / sodium carboxymethyl cellulose precursor in S3.3 with an equal mass of porous carbon-loaded nano-silicon precursor, and prepares the negative electrode material without changing the other steps, which is recorded as Comparative Example 7.

[0109] The negative electrode materials prepared in Comparative Examples 6-7 were assembled into CR2025 type button lithium ion batteries according to the above method for charge and discharge. The battery charge and discharge test was carried out on the LAND battery system, and the charge and discharge voltage range was 0-2V. The electrochemical performance tests were carried out on Examples 1-3 and Comparative Examples 6-7, and the test results are shown in Table 3.

[0110] Table 3. Electrochemical performance test results of Examples 1-3 and Comparative Examples 6-7

[0111] First discharge capacity (mAh / g, 25℃) First coulombic efficiency (%) Capacity retention after 200 cycles (%) Example 1 428.2 90.3 92.32 Example 2 427.9 90.1 92.13 Example 3 427.2 89.8 92.18 Comparative Example 6 408.2 85.3 87.67 Comparative Example 7 392.5 83.8 84.97

[0112] From the data in Table 3, it can be seen that the data of Comparative Example 6 is worse than that of the embodiment, but slightly better than that of Comparative Example 7, indicating that the cycle stability of the negative electrode material is enhanced by coating the porous carbon-loaded nano-silicon with sodium carboxymethyl cellulose after vacuum high-temperature carbonization, the prepared negative electrode material has good electrochemical performance, and the cycle performance of the negative electrode material can be further improved after cerium doping.

[0113] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing a negative electrode material loaded with nano-silicon porous carbon, characterized in that: The steps include: S1: Preparation of hollow porous starch Hollow porous starch can be prepared by first enzymatically hydrolyzing starch with maltotriase and then enzymatically hydrolyzing starch with amyloglucosidase; S2: Preparation of porous carbon-supported nanosilicon precursor The ammonium chloride and the hollow porous starch are mixed and then added with deionized water and stirred. During the stirring process, nano silicon powder is added, and after being stirred evenly, gelation and aging are performed, and then freezing and soaking are performed to obtain a porous carbon-loaded nano silicon precursor; S3: Preparation of negative electrode materials Sodium carboxymethyl cellulose is dissolved in deionized water, and then a porous carbon-loaded nano-silicon precursor is added, followed by high-temperature carbonization under vacuum to obtain a negative electrode material.

2. The method for preparing a negative electrode material loaded with nano-silicon porous carbon according to claim 1, characterized in that: Step S1: Preparation of hollow porous starch, specifically comprising the following steps: S1.1: Weigh 30-40 parts by weight of starch, prepare a starch emulsion with a concentration of 10-12% (w / v) with 0.1 mol / L disodium hydrogen phosphate-citric acid buffer solution, and swell the starch emulsion in a constant temperature water bath with a magnetic stirrer at 60-65°C for 0.5-1h to obtain a starch emulsion; S1.2: The temperature of the starch emulsion is adjusted to 50-55°C, and maltotriose enzyme is added to react for 5-6 hours. After the reaction is completed, the starch emulsion is immediately placed in ice water for 10-15 minutes to rapidly cool down and reduce the reaction rate of the enzyme. Then, the pH is adjusted to 11-12 with 2 mol / L sodium hydroxide solution and reacted for 8-10 minutes to obtain the starch emulsion after enzyme inactivation; S1.3: The temperature of the starch emulsion after enzyme inactivation is adjusted to 50-55°C, and amyloglucosidase is added for enzymatic hydrolysis for 5-6 hours. After the reaction is completed, the starch emulsion is immediately placed in ice water for 10-15 minutes for rapid cooling to reduce the reaction rate of the enzyme, and then the pH is adjusted to 11-12 with 2 mol / L sodium hydroxide solution for reaction for 8-10 minutes to obtain a starch emulsion after enzyme inactivation again; S1.4: The pH of the starch emulsion after enzyme inactivation is adjusted to neutral with 2 mol / L hydrogen chloride solution, the neutral starch emulsion is centrifuged to obtain a precipitate, the precipitate is repeatedly washed with distilled water for 5-6 times, and then dried in an oven at 45-50°C for 40-48 hours, and then ground and crushed and passed through a 100-120 mesh sieve to obtain hollow porous starch.

3. The method for preparing a negative electrode material loaded with nano-silicon porous carbon according to claim 2, characterized in that: Step S2: Preparation of porous carbon-supported nano-silicon precursor, specifically comprising the following steps: S2.1: Weigh 1-2 parts by weight of ammonium chloride and 2-3 parts by weight of hollow porous starch, add 20-30 parts by weight of deionized water after mixing, and stir magnetically for 2-3 hours. During the magnetic stirring process, add 0.2-0.5 parts by weight of nano silicon powder with a particle size of 20-30 nm, and stir evenly to obtain a starch complex suspension; S2.2: The starch complex suspension is placed in a water bath and heated at 80-90°C while being stirred continuously for 30-50 minutes to obtain a gelatinized starch complex suspension. The gelatinized starch complex suspension is further heated at 80-90°C for 10-12 minutes and then aged at room temperature for 10-12 hours to obtain an aged starch complex suspension. S2.3: The aged starch complex suspension is frozen at -25°C to -20°C for 10-12 hours, then cooled to room temperature in air, and then soaked in acetone for 20-30 minutes to obtain a porous carbon-loaded nano-silicon precursor.

4. The method for preparing a negative electrode material loaded with nano-silicon porous carbon according to claim 3, characterized in that: Step S3: Preparation of negative electrode materials, specifically including the following steps: S3.1: dissolving 1-2 parts by weight of sodium carboxymethyl cellulose in 200-300 parts by weight of deionized water, and stirring evenly to obtain a gel solution, and then adding the porous carbon-supported nano-silicon precursor to the gel solution, stirring evenly to obtain a mixed gel solution; S3.2: Add 0.01-0.02 parts by weight of cerium nitrate solution dropwise to the mixed gel solution, stir evenly, and freeze-dry to obtain a silicon / starch@cerium / sodium carboxymethyl cellulose precursor; S3.3: Place the silicon / starch@cerium / sodium carboxymethyl cellulose precursor in a tubular resistance furnace with an inert gas as the protective atmosphere, carbonize it at high temperature under vacuum, cool it naturally to room temperature, wash it repeatedly with deionized water 2-3 times, and dry it to obtain the negative electrode material.

5. The method for preparing a negative electrode material loaded with nano-silicon porous carbon according to claim 2, characterized in that: The amount of maltotriosidase added in step S1.2 is: the mass ratio of starch to maltotriosidase is 50-100:

1.

6. The method for preparing a negative electrode material loaded with nano-silicon porous carbon according to claim 2, characterized in that: The amount of amyloglucosidase added in step S1.3 is: the mass ratio of starch to amyloglucosidase is 50-100:

1.

7. The method for preparing a negative electrode material loaded with nano-silicon porous carbon according to claim 2, characterized in that: The starch in step S1.1 is specifically one or more of corn starch, wheat starch, potato starch and tapioca starch.

8. The method for preparing a negative electrode material loaded with nano-silicon porous carbon according to claim 4, characterized in that: The inert gas in step S3.3 is nitrogen.

9. The method for preparing a negative electrode material loaded with nano-silicon porous carbon according to claim 4, characterized in that: In step S3.3, the inert gas flow rate is 75-80 mL / min, the carbonization heating rate is 2-3°C / min, the temperature is 700-800°C, the carbonization vacuum is 10-15 Pa, and the carbonization time is 3-4 h.

10. A negative electrode material loaded with nano-silicon porous carbon, characterized in that: It is prepared by the method for preparing a negative electrode material loaded with nano-silicon porous carbon as described in any one of claims 1 to 9.

Citation Information

Cited By

  • Novel silicon-carbon negative electrode material and preparation method thereof

    CN120328562A

  • A silicon-carbon anode material and its preparation method

    CN120328562B