A method for preparing a high-strength and high-conductivity rare earth copper alloy Cu-Cr-Zr plate
By adding rare earth elements Ce and La to the Cu-Cr-Zr alloy and adopting a specific process flow, high-strength and high conductivity rare earth copper alloy Cu-Cr-Zr plates are prepared, and the existing Cu-Cr- is solved by solving the problem of The problem of the contradiction between mechanics and electrical properties of Zr copper alloys meets the performance needs of high-end fields.
Patent Information
- Application Number
- CN202411140119.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The existing Cu-Cr-Zr-type copper alloys are difficult to achieve tensile strength of 600MPa and cannot meet the needs of high-strength and high-conducting copper alloys in the high-end field, and there is a problem of contradiction between mechanics and electrical properties.
The rare earth elements Ce and La are added to the Cu-Cr-Zr alloy, and the rare earth copper alloy Cu- with high strength and high conductivity are prepared through alloy ratio, smelting process, solid solution treatment, multiple rolling and alternating processing. Cr-Zr sheets ensure the comprehensive performance of the alloy.
The tensile strength of Cu-Cr-Zr sheet exceeds 620MPa and the relative conductivity is higher than 85% IACS, meeting the performance requirements of high-end fields. At the same time, the process is simple and suitable for large-scale production.
Smart Images

Figure CN118668088B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rare earth copper alloys, and in particular relates to a method for preparing a high-strength and high-conductivity rare earth copper alloy Cu-Cr-Zr plate. Background Art
[0002] Copper and copper alloys have a series of excellent properties such as high electrical conductivity, good thermal conductivity and high strength. They are a very important type of structural and functional integrated materials and are widely used in large-scale integrated circuits, high-speed rail transportation, aerospace, new energy vehicles and other fields. In recent years, with the rapid development of high-tech industries, especially the rapid development of microelectronics, new energy vehicles and other fields, higher and higher requirements have been placed on the performance of copper alloys. There is a contradictory relationship between the mechanical and electrical properties of high-strength and high-conductivity copper alloys. In engineering, it has always been hoped to obtain high-strength and high-conductivity copper alloys that have high conductivity, relative conductivity greater than 80% ICSA, high strength, and tensile strength exceeding 600MPa, which can meet the needs of large-scale production.
[0003] The high-strength and high-conductivity copper alloy systems mainly include Cu-Cr-Zr, Cu-Ni-Si, Cu-Fe-P, etc. Among them, Cu-Cr-Zr copper alloy has good mechanical and electrical properties, and the relative conductivity can reach more than 80% IACS, which is the most promising copper alloy material. However, the strength of Cu-Cr-Zr copper alloy is difficult to reach 600MPa, which is difficult to meet the growing product demand, which greatly limits the scope of use of Cu-Cr-Zr copper alloy. Therefore, the development of high-strength and high-conductivity Cu-Cr-Zr copper alloy that can meet large-scale production faces certain difficulties and challenges.
[0004] To this end, the present invention is proposed. Summary of the invention
[0005] The main purpose of the present invention is to provide a method for preparing a high-strength and high-conductivity rare earth copper alloy Cu-Cr-Zr plate. The rare earth copper alloy Cu-Cr-Zr plate prepared by the preparation method of the present invention can ensure an effective combination of high strength (≥620MPa) and high conductivity (≥85%IACS), and meet the use requirements of high-end fields.
[0006] In order to achieve the above objectives, the present invention provides the following technical solutions.
[0007] The present invention provides a method for preparing a high-strength and high-conductivity rare earth copper alloy Cu-Cr-Zr plate, the preparation method comprising the following steps:
[0008] The alloy ratio is made according to the alloy composition of the plate, and the metal single substance of each element and the master alloy are mixed and smelted, and cast to obtain an alloy ingot; wherein the alloy composition of the plate contains the following elements in percentage by mass: 0.58% to 0.62% Cr element, 0.13% to 0.17% Zr element, 0.09% to 0.11% rare earth element, and the balance is Cu element; the rare earth element is Ce element, or Ce and La element;
[0009] The alloy ingot is subjected to a solid solution treatment, and subjected to multiple rolling and multiple-step aging alternating and continuous processing to obtain the high-strength and high-conductivity rare earth copper alloy Cu-Cr-Zr plate;
[0010] During smelting, the Cr element is added in the form of a Cu-Cr master alloy, the Zr element is added in the form of a Cu-Zr master alloy, the rare earth element is added in the form of a Cu-rare earth element master alloy, and the Cu element is added in the form of single copper, and the purity of the single copper is greater than or equal to 99.99%;
[0011] The smelting process comprises: adding single copper into a graphite crucible and adding a graphite powder covering agent, using a medium frequency induction smelting furnace, in an atmospheric environment, heating up to 1250°C-1260°C at a rate of 50°C / min-100°C / min with the furnace and keeping the temperature, and after the copper is completely melted, continuing to heat up to 1350°C-1360°C, adding a Cu-Cr master alloy, and keeping the temperature until it is completely melted; cooling down to 1250°C-1260°C at a rate of 10°C / min-30°C / min and keeping the temperature, adding a Cu-Zr master alloy, and after it is completely melted, adding a Cu-rare earth element master alloy for smelting to obtain a mixed melt.
[0012] In some embodiments of the present invention, the Cr element is added in the form of a Cu-Cr master alloy, and the mass fraction of the Cr element is 10% to 15%;
[0013] The Zr element is added in the form of a Cu-Zr master alloy, and the mass fraction of the Zr element is 20% to 40%;
[0014] The rare earth element is added in the form of a Cu-rare earth element master alloy, and the mass fraction of the rare earth element is 10% to 20%.
[0015] In some embodiments of the present invention, the alloy ingot is produced by non-vacuum melting and near-liquidus casting; wherein the near-liquidus casting method uses a graphite mold with a temperature of 300°C to 320°C and a casting temperature of 1100°C to 1120°C.
[0016] In some embodiments of the present invention, the solution treatment process includes: loading the alloy ingot into a heat treatment furnace, heating the furnace to 940°C~960°C, keeping the temperature for 115min~125min, and then quenching in water, the water temperature is 22°C~26°C.
[0017] In some embodiments of the present invention, the multiple rolling and multi-step aging alternating and continuous processing includes at least three rolling and three-step aging treatments, and the temperature of the multiple rolling is 22°C~26°C, and the heating rate of the three-step aging treatment is 5°C / min~10°C / min.
[0018] In some embodiments of the present invention, the three-step rolling and three-step aging treatment process includes:
[0019] The solution treated billet is subjected to a first rolling, and the first aging treatment is performed on the billet after the first rolling; and
[0020] Performing a second rolling on the billet after the first aging treatment, and performing a second aging treatment on the billet after the second rolling; and
[0021] The billet after the second step aging treatment is subjected to a third rolling, and the billet after the third rolling is subjected to a third step aging treatment.
[0022] In some embodiments of the present invention, the deformation of the first rolling is 75% to 85%, the temperature of the first aging treatment is 440° C. to 460° C., and the time is 55 min to 65 min;
[0023] The deformation of the second rolling is 65% to 75%, and the temperature of the second aging treatment is 390°C to 410°C for 25min to 35min.
[0024] The deformation amount of the third rolling is 45% to 55%, the temperature of the third aging treatment is 390° C. to 410° C., and the time is 25 min to 35 min.
[0025] Compared with the prior art, the present invention achieves the following technical effects:
[0026] The invention can effectively refine the grains by adding rare earth elements Ce and La to the Cu-Cr-Zr alloy. Meanwhile, the rare earth elements Ce and La can react with impurities to purify the matrix, form intermetallic compounds with alloy elements, refine the precipitated phase, and effectively improve the comprehensive performance of the alloy.
[0027] The preparation environment of the present invention is in an atmospheric environment and at room temperature, and the adopted equipment and process flow are simple, without other special requirements, and can meet the conditions for large-scale production.
[0028] The rare earth copper alloy Cu-Cr-Zr-rare earth element (RE) alloy plate prepared by the present invention has a tensile strength exceeding 620MPa and a relative conductivity higher than 85%IACS, and has excellent performance, which can meet the performance requirements of high-end fields for high-strength and high-conductivity copper alloys.
[0029] The Cu-Cr-Zr-RE alloy plate prepared by the present invention has a tensile strength of 620MPa-639MPa, a yield strength of 615MPa-633MPa, a relative conductivity of 85.2%IACS-88.5%IACS, and an elongation after fracture of 5.7%-9%.
[0030] The Cu-Cr-Zr-RE alloy sheet prepared by the present invention has high strength and high conductivity. Under the three-step rolling + three-step aging alternating and continuous processing technology, fine substructures such as stacking faults, nano-level twins and nano-level precipitation can be obtained. Under the effect of the above structure, high strength and high conductivity are achieved to meet the requirements of high-performance cutting-edge technology.
[0031] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only used for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. In the accompanying drawings:
[0033] Figure 1 is a process flow chart of a preparation method according to some embodiments of the present invention;
[0034] Figure 2 The stacking fault of the Cu-0.6Cr-0.15Zr-0.1Ce alloy plate prepared in Example 1 of the present invention after three-step aging;
[0035] Figure 3 The nano-scale twins of the Cu-0.6Cr-0.15Zr-0.1Ce alloy plate prepared in Example 1 of the present invention after three-step aging;
[0036] Figure 4 It is the nanoscale precipitation phase of the Cu-0.6Cr-0.15Zr-0.1Ce alloy plate prepared in Example 1 of the present invention after three-step aging;
[0037] Figure 5The engineering stress-strain curve of the Cu-0.6Cr-0.15Zr-0.1Ce alloy plate prepared in Example 1 of the present invention after three-step aging;
[0038] Figure 6 The engineering stress-strain curve of the Cu-0.6Cr-0.15Zr-0.05Ce-0.05La alloy plate prepared in Example 2 of the present invention after three-step aging;
[0039] Figure 7 This is the engineering stress-strain curve of the Cu-0.6Cr-0.15Zr alloy plate prepared in Comparative Example 1 of the present invention after three-step aging. DETAILED DESCRIPTION
[0040] The exemplary embodiments of the present invention will be described in more detail below with reference to specific embodiments. It should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0041] Rare earth elements (RE) have typical metallic properties and are extremely active in chemical properties. They can interact with almost all elements except inert gases and have the ability to absorb a large amount of gas. Due to their unique properties, rare earth elements can produce deoxidation, degassing and impurity removal in copper alloys, and can also refine grains, enhance thermal stability, and have good high-temperature and room-temperature plasticity, which can significantly improve the comprehensive properties of the alloy.
[0042] The method for preparing the Cu-Cr-Zr-RE alloy plate by alternating rolling and aging and continuously processing is simple and easy. The alloy plate prepared by the method has excellent mechanical properties and electrical properties, solves the contradictory relationship between the mechanical and electrical properties of the existing high-strength and high-conductivity copper alloy, obtains a material with integrated structure and function, and meets the high comprehensive performance requirements in high-performance cutting-edge fields.
[0043] The present invention provides a method for preparing a high-strength and high-conductivity rare earth copper alloy Cu-Cr-Zr plate. The preparation method is carried out according to the following steps.
[0044] The alloy ratio is determined according to the alloy composition of the target plate.
[0045] In some embodiments of the present invention, the Cu-Cr-Zr-RE alloy components are formulated according to mass percentage, and the alloy components include Cr element, Zr element, rare earth element, and the balance is Cu element.
[0046] In some embodiments of the present invention, the rare earth element is Ce, or Ce and La. Ce and La have a large output, and can reduce the preparation cost while achieving high conductivity and high strength performance, meet the application of high-end fields, and can be widely promoted and applied.
[0047] In some embodiments of the present invention, the alloy composition of the target plate includes the following elements in mass percentage:
[0048] 0.58%~0.62% Cr element, 0.13%~0.17% Zr element, 0.09%~0.11% rare earth element, and the balance is Cu element.
[0049] For example, the mass percentage of the Cr element may be one of 0.58%, 0.59%, 0.60%, 0.61%, 0.62%, or any value satisfying the above range. The mass percentage of the Zr element may be one of 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, or any value satisfying the above range. The mass percentage of the rare earth element may be one of 0.09%, 0.10%, 0.11%, or any value satisfying the above range.
[0050] The metal elements and alloys of each element are mixed and smelted, and then cast to obtain alloy ingots.
[0051] In some embodiments of the present invention, the alloy ingot is produced by non-vacuum melting and near-liquidus casting.
[0052] Among them, a medium frequency induction melting furnace is adopted, a graphite crucible is used, and melting is carried out in an atmospheric environment.
[0053] A graphite mold is used in the near-liquidus casting method, and the graphite mold is preheated so that the temperature of the graphite mold is 300°C~320°C, for example, 310°C, 305°C, 315°C; the casting temperature is 1100°C~1120°C, that is, the mixed melt temperature during casting is 1100°C~1120°C.
[0054] In some embodiments of the present invention, during smelting, the Cr element is added in the form of a Cu-Cr master alloy, and the mass fraction of the Cr element is 10% to 15%.
[0055] Exemplarily, the mass fraction of the Cr element may be one of 10%, 11%, 12%, 13%, 14%, 15%, or any value satisfying the above range.
[0056] In some embodiments of the present invention, during smelting, the Zr element is added in the form of a Cu-Zr master alloy, and the mass fraction of the Zr element is 20% to 40%.
[0057] Exemplarily, the mass fraction of the Zr element can be one of 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, or any value satisfying the above range.
[0058] In some embodiments of the present invention, during smelting, rare earth elements are added in the form of Cu-rare earth element master alloy, and the mass fraction of the rare earth elements is 10% to 20%.
[0059] Illustratively, the mass fraction of the rare earth element can be one of 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, or any value satisfying the above range.
[0060] In some embodiments of the present invention, during smelting, the Cu element is added in the form of single copper, and the purity of the single copper is greater than or equal to 99.99%.
[0061] In some embodiments of the present invention, the smelting process includes adding elemental copper to a graphite crucible and adding a graphite powder covering agent, using a medium frequency induction melting furnace, and in an atmospheric environment, heating to 1250°C~1260°C at a rate of 50°C / min~100°C / min with the furnace and keeping warm, and after the copper is completely melted, continuing to heat to 1350°C~1360°C, adding a Cu-Cr master alloy, and keeping warm until it is completely melted; cooling to 1250°C~1260°C at a rate of 10°C / min~30°C / min and keeping warm, adding a Cu-Zr master alloy, and after it is completely melted, adding a Cu-rare earth element master alloy and keeping warm to obtain a mixed melt.
[0062] The alloy ingot is subjected to solution treatment to obtain an intermediate billet.
[0063] In some embodiments of the present invention, the solution treatment process includes charging the alloy ingot into a heat treatment furnace, heating the furnace to 940°C~960°C, keeping the temperature for 115min~125min to allow the alloy elements to fully dissolve, and then quenching in water at a water temperature of 22°C~26°C.
[0064] The intermediate billet is subjected to multiple rolling and multi-step aging treatments to obtain a high-strength and high-conductivity rare earth copper alloy Cu-Cr-Zr sheet.
[0065] In some embodiments of the present invention, the multiple rolling and multi-step aging continuous treatments include at least three rollings and three-step aging treatments, and the temperature of the multiple rollings is 22°C~26°C, and the heating rates of the three-step aging treatments are 5°C / min~10°C / min.
[0066] In some embodiments of the present invention, the three-step rolling and three-step aging treatment process includes:
[0067] The intermediate billet after the solution treatment is subjected to the first rolling with a deformation amount of 75% to 85%, and the billet after the first rolling is subjected to the first aging treatment; the temperature of the first aging treatment is 440°C to 460°C, and the time is 55min to 65min; and
[0068] The billet after the first aging treatment is subjected to a second rolling with a deformation amount of 65% to 75%, and the billet after the second rolling is subjected to a second aging treatment; the temperature of the second aging treatment is 390° C. to 410° C., and the time is 25 min to 35 min; and
[0069] The billet after the second step aging treatment is rolled for the third time with a deformation of 45%~55%, and the billet after the third rolling is subjected to the third step aging treatment. The temperature of the third step aging treatment is 390℃~410℃, and the time is 25min~35min.
[0070] The present invention also provides a high-strength and high-conductivity rare earth copper alloy Cu-Cr-Zr plate prepared by the above preparation method. The tensile strength of the alloy plate can reach 620MPa~639MPa, the yield strength can reach 615MPa~633MPa, the relative conductivity can reach 85.2%IACS~88.5%IACS, and the elongation after fracture can reach 5.7%~9%.
[0071] The chemical reagents used in the specification and examples of the present invention include any conventional models or types in the art, and the present invention does not impose any special limiting requirements.
[0072] Example 1
[0073] Example 1 discloses a high-strength and high-conductivity rare earth copper alloy Cu-0.6Cr-0.15Zr-0.1Ce plate, in which the composition ratios are as follows by mass percentage: 0.6% Cr, 0.15% Zr, 0.1% Ce, and the balance is Cu element.
[0074] The preparation method of the high-strength and high-conductivity rare earth copper alloy Cu-0.6Cr-0.15Zr-0.1Ce plate comprises the following steps:
[0075] (1) The alloy elements are proportioned according to the composition requirements of the Cu-Cr-Zr-Ce alloy. The composition of the Cu-Cr-Zr-Ce alloy is recorded as follows in mass percentage: 0.6% Cr, 0.15% Zr, 0.1% Ce, and the balance is Cu element.
[0076] Among them, the Cu element is added in the form of single copper with a purity of 99.99%; the Cr element is added in the form of Cu-Cr master alloy, and the mass fraction of the Cr element is 10%; the Zr element is added in the form of Cu-Zr master alloy, and the mass fraction of the Zr element is 40%; the Ce element is added in the form of Cu-Ce master alloy, and the mass fraction of the Ce element is 20%.
[0077] (2) The alloys prepared in step (1) are mixed and smelted, and a Cu-Cr-Zr-Ce alloy ingot is produced by a non-vacuum melting + near-liquidus casting method.
[0078] Specifically, the smelting process uses a graphite crucible, adds 99.99% pure copper to the graphite crucible and adds a graphite powder covering agent. Use a medium frequency induction melting furnace, in an atmospheric environment, quickly heat up with the furnace, the heating rate is 80℃ / min, and the temperature is kept at 1255℃ until the copper is completely melted; after complete melting, continue to heat up to 1355℃, add Cu-Cr intermediate alloy, and keep it warm until it is completely melted; when the temperature slowly drops to 1255℃, keep it warm, add Cu-Zr intermediate alloy, the cooling rate is 20℃ / min, and after complete melting, add Cu-Ce intermediate alloy, keep it warm for 10 minutes to obtain a mixed melt.
[0079] The non-vacuum melting + near-liquidus casting method uses a graphite mold with a temperature of about 310°C and casts at 1110°C to obtain a Cu-Cr-Zr-Ce alloy ingot.
[0080] (3) The Cu-Cr-Zr-Ce alloy ingot obtained in step (2) is subjected to a solid solution treatment to obtain an intermediate billet.
[0081] The solution treatment process is as follows: the Cu-Cr-Zr-Ce alloy ingot is loaded into a heat treatment furnace, the temperature is slowly raised to 950°C, and after being kept warm for 60 minutes, water quenching is performed, and the water temperature is room temperature 25°C to obtain an intermediate billet.
[0082] (4) The intermediate billet obtained in step (3) is subjected to three rolling + three-step aging alternating and continuous processing to obtain a Cu-Cr-Zr-Ce alloy plate product. The three rolling temperatures are all room temperature 25°C, and the three-step aging treatment is all slowly heated with the furnace, and the heating rate is 8°C / min.
[0083] Specifically, the first rolling + first aging process is as follows: the billet obtained in step (3) is subjected to the first rolling with a deformation amount of 80%, and the billet after the first rolling is subjected to the first aging treatment at a temperature of 450° C. and a time of 60 min.
[0084] The second rolling + second aging process is as follows: the billet after the first aging treatment is subjected to a second rolling with a deformation of 70%, and the billet after the second rolling is subjected to a second aging treatment at a temperature of 400°C and a time of 30 minutes.
[0085] The third rolling + third step aging process is as follows: the billet after the second step aging is rolled for the third time with a deformation of 50%, and the billet after the third rolling is subjected to the third step aging treatment at a temperature of 400°C and a time of 30 minutes to obtain a Cu-0.6Cr-0.15Zr-0.1Ce alloy plate.
[0086] The present invention performs performance tests on the Cu-0.6Cr-0.15Zr-0.1Ce alloy plate prepared in Example 1. The test results are shown in Table 1. The Cu-0.6Cr-0.15Zr-0.1Ce alloy plate has good comprehensive performance: the tensile strength reaches 620 MPa; the relative conductivity is as high as 88.51% IACS, which exceeds the ideal performance indicators of high-strength and high-conductivity copper alloys (tensile strength not less than 600 MPa; relative conductivity not less than 80% IACS).
[0087] Figure 2 The stacking fault of the Cu-0.6Cr-0.15Zr-0.1Ce alloy prepared by the present invention after three-step aging, Figure 3 The nano-scale twins of the Cu-0.6Cr-0.15Zr-0.1Ce alloy prepared by the present invention after three-step aging are shown in FIG. Figure 4 This is the nanoscale precipitation phase of the Cu-0.6Cr-0.15Zr-0.1Ce alloy prepared by the present invention after three-step aging. Figure 2-4 It can be found that after three rolling and three-step aging, stacking faults, nano-scale twins and nano-scale precipitation phases are formed inside the alloy. Through analysis, it can be seen that the addition of Ce element not only reduces the stacking fault energy of Cu-Cr-Zr alloy and promotes the formation of stacking faults during deformation, but also forms new precipitation phases with alloy elements to further refine the precipitation phases. Fine substructures such as nano-scale precipitation phases, nano-scale twins, and stacking faults can significantly improve the mechanical properties of the alloy while having little negative impact on the electrical properties, so the balance point between the tensile strength and relative conductivity of the alloy is raised to a very high position.
[0088] Example 2
[0089] Example 2 discloses a high-strength and high-conductivity rare earth copper alloy Cu-0.6Cr-0.15Zr-0.05Ce-0.05La plate, whose component ratios are as follows, by mass percentage: 0.6% Cr, 0.15% Zr, 0.05% Ce, 0.05% La, and the remainder is Cu element.
[0090] The preparation method of the high-strength and high-conductivity rare earth copper alloy Cu-0.6Cr-0.15Zr-0.05Ce-0.05La plate comprises the following steps:
[0091] (1) The alloy elements are proportioned according to the composition requirements of the Cu-Cr-Zr-Ce-La alloy. The composition of the Cu-Cr-Zr-Ce-La alloy is recorded as follows in mass percentage: 0.6% Cr, 0.15% Zr, 0.05% Ce, 0.05% La, and the balance is Cu element.
[0092] Among them, the Cu element is added in the form of single copper with a purity of 99.99%; the Cr element is added in the form of Cu-Cr master alloy, and the mass fraction of the Cr element is 10%; the Zr element is added in the form of Cu-Zr master alloy, and the mass fraction of the Zr element is 40%; the Ce element is added in the form of Cu-Ce master alloy, and the mass fraction of the Ce element is 20%; the La element is added in the form of Cu-La master alloy, and the mass fraction of the La element is 20%.
[0093] (2) The alloys prepared in step (1) are mixed and smelted, and a Cu-Cr-Zr-Ce-La alloy ingot is produced by a non-vacuum melting + near-liquidus casting method.
[0094] Specifically, a graphite crucible is used in the smelting process, and 99.99% pure copper is added to the graphite crucible and a graphite powder covering agent is added. A medium-frequency induction melting furnace is used, and the temperature is rapidly increased with the furnace under atmospheric conditions, with a heating rate of 80°C / min. After the temperature is increased to 1255°C, it is kept warm until the copper is completely melted; after it is completely melted, the temperature is continued to be increased to 1355°C, and the Cu-Cr intermediate alloy is added and kept warm until it is completely melted; when the temperature slowly drops to 1255°C, it is kept warm, and the Cu-Zr intermediate alloy is added, and the cooling rate is 20°C / min. After it is completely melted, Cu-Ce and Cu-La intermediate alloys are added, and the temperature is kept warm for 10 minutes to obtain a mixed melt.
[0095] The non-vacuum melting + near-liquidus casting method uses a graphite mold with a temperature of 310°C and casts at 1110°C to obtain a Cu-Cr-Zr-Ce-La alloy ingot.
[0096] (3) The Cu-Cr-Zr-Ce-La alloy ingot obtained in step (2) is subjected to a solid solution treatment to obtain an intermediate billet.
[0097] Among them, the solution treatment process is: the Cu-Cr-Zr-Ce-La alloy ingot is loaded into a heat treatment furnace, and the temperature is slowly raised to 950°C with the furnace. After keeping warm for 120 minutes, it is water quenched, and the water temperature is room temperature 25°C to obtain an intermediate billet.
[0098] (4) The intermediate billet obtained in step (3) is subjected to three rolling + three-step aging alternating and continuous processing to obtain a Cu-Cr-Zr-Ce-La alloy plate product. The three rolling temperatures are all room temperature 25°C, and the three-step aging treatment is all slowly heated with the furnace, and the heating rate is 8°C / min.
[0099] Specifically, the first rolling + first aging process is as follows: the billet obtained in step (3) is subjected to the first rolling with a deformation amount of 80%, and the billet after the first rolling is subjected to the first aging treatment at a temperature of 450° C. and a time of 60 min.
[0100] The second rolling + second aging process is as follows: the billet after the first aging treatment is subjected to a second rolling with a deformation of 70%, and the billet after the second rolling is subjected to a second aging treatment at a temperature of 400°C and a time of 30 minutes.
[0101] The third rolling + third step aging process flow is: the billet after the second step aging treatment is rolled for the third time with a deformation of 50%, and the billet after the third rolling is subjected to the third step aging treatment at a temperature of 400°C and a time of 30 minutes to obtain the Cu-0.6Cr-0.15Zr-0.05Ce-0.05La alloy plate.
[0102] The present invention performs performance tests on the Cu-0.6Cr-0.15Zr-0.05Ce-0.05La alloy plate prepared in Example 2. The test results are shown in Table 1. The Cu-0.6Cr-0.15Zr-0.05Ce-0.05La alloy plate has good comprehensive performance, and is better than the performance of the plate in Example 1.
[0103] Comparative Example 1
[0104] Comparative Example 1 discloses a copper alloy Cu-0.6Cr-0.15Zr alloy plate, in which the composition ratios are as follows, by mass percentage: 0.6% Cr, 0.15% Zr, and the balance is Cu element.
[0105] The preparation method of the copper alloy Cu-Cr-Zr plate comprises the following steps:
[0106] (1) The alloy elements are proportioned according to the requirements of the Cu-Cr-Zr alloy composition. The composition of the Cu-Cr-Zr alloy is recorded as follows in mass percentage: 0.6% Cr, 0.15% Zr, and the balance is Cu element.
[0107] Among them, the Cu element is added in the form of single copper with a purity of 99.99%; the Cr element is added in the form of Cu-Cr master alloy, and the mass fraction of the Cr element is 10%; the Zr element is added in the form of Cu-Zr master alloy, and the mass fraction of the Zr element is 40%.
[0108] (2) The alloys prepared in step (1) are mixed and smelted, and a Cu-Cr-Zr alloy ingot is produced by a non-vacuum melting + near-liquidus casting method.
[0109] Specifically, the smelting process uses a graphite crucible, adds 99.99% pure copper to the graphite crucible and adds a graphite powder covering agent. A medium-frequency induction melting furnace is used, and the temperature is rapidly increased with the furnace under atmospheric conditions, with a heating rate of 80°C / min. After the temperature is increased to 1255°C, it is kept warm until the copper is completely melted; after melting, the temperature is continued to be increased to 1355°C, and the Cu-Cr intermediate alloy is added and kept warm until it is completely melted; when the temperature slowly drops to 1255°C, it is kept warm, and the Cu-Zr intermediate alloy is added, and the cooling rate is 20°C / min. After it is completely melted, it is kept warm for 10 minutes to obtain a mixed melt.
[0110] The non-vacuum melting + near-liquidus casting method uses a graphite mold with a temperature of 310°C and casts at 1110°C to obtain a Cu-Cr-Zr alloy ingot.
[0111] (3) The Cu-Cr-Zr alloy ingot obtained in step (2) is subjected to a solid solution treatment to obtain an intermediate billet.
[0112] The solution treatment process is as follows: the Cu-Cr-Zr alloy ingot is placed into a heat treatment furnace, the temperature is slowly raised to 950°C, and after being kept warm for 120 minutes, water quenching is performed at a water temperature of 25°C, which is room temperature, to obtain an intermediate billet.
[0113] (4) The intermediate billet obtained in step (3) is subjected to three rolling + three-step aging alternating and continuous processing to obtain a Cu-Cr-Zr alloy plate product. The three rolling temperatures are all room temperature 25°C, and the three-step aging treatment is all slowly heated with the furnace, and the heating rate is 8°C / min.
[0114] Specifically, the first rolling + first aging process is as follows: the billet obtained in step (3) is subjected to the first rolling with a deformation amount of 80%, and the billet after the first rolling is subjected to the first aging treatment at a temperature of 450° C. and a time of 60 min.
[0115] The second rolling + second aging process is as follows: the billet after the first aging treatment is subjected to a second rolling with a deformation of 70%, and the billet after the second rolling is subjected to a second aging treatment at a temperature of 400°C and a time of 30 minutes.
[0116] The third rolling + third step aging process is as follows: the billet after the second step aging treatment is rolled for the third time with a deformation of 50%, and the billet after the third rolling is subjected to the third step aging treatment at a temperature of 400°C and a time of 30 minutes to obtain a Cu-0.6Cr-0.15Zr alloy plate.
[0117] The performance of the Cu-0.6Cr-0.15Zr alloy plate prepared in Comparative Example 1 of the present invention was tested, and the test results are shown in Table 1. Its performance index is significantly lower than that of Example 1 and Example 2 in which trace Ce and La elements are added. It shows that after rare earth microalloying of Cu-Cr-Zr alloy, two performance indexes with contradictory relationship can be improved simultaneously and to a large extent: tensile strength and relative conductivity. Therefore, the present invention provides an economical and convenient way to optimize the performance and structure of high-strength and high-conductivity Cu-Cr-Zr alloy.
[0118] Performance Testing
[0119] The tensile strength test was carried out on alloy plates with different compositions and different processing technologies. The samples were cut into I-type flat plate samples using an electric spark wire cutting machine. The dimensions were as follows: the gauge section length was 25mm, the thickness was the original thickness of the sample, the width was 4mm, the clamping section width was 10mm, the length was 12mm, and the total length of the sample was 55mm. After the sample was made, the tensile specimen was ground to a smooth surface to remove burrs and other macro defects. Using a universal tensile testing machine, the clamping sections at both ends of the sample were clamped with the universal testing machine fixture and the measurement began. The strain rate during the tensile test was 1mm / s. Three tensile test sample results were selected for each state, and the average value was taken as the final tensile strength, yield strength, and elongation value of the sample.
[0120] Conductivity tests were conducted on alloys with different compositions and different processing technologies. The samples were cut into long flat specimens using an EDM wire cutting machine. The size was 2*40mm and the thickness was the original thickness of the specimen. The specimens were polished to be smooth, without oxide scale and macro defects. The FM100GH four-probe resistivity tester was used to test and record the resistance data of the samples. Three sample results were selected for each state and the average value was calculated as the resistance value of the sample. Finally, the international annealed copper standard conductivity percentage (%IACS) was converted into relative conductivity using formula (1-1) in GB / T351-2019 Metal Material Resistivity Measurement Method.
[0121] %IACS= ×100 (1-1)
[0122] ρ: Volume resistivity of the sample at 20°C, in ohm-meter (Ω∙m).
[0123] Table 1 Summary of properties of alloy plates obtained in Examples and Comparative Examples
[0124]
[0125] Combined with Table 1 and Appendix Figures 5 to 7 It can be seen that the alloy sheet prepared by the present invention has excellent mechanical properties and electrical properties, especially in terms of tensile strength and relative conductivity, which are superior to the Cu-Cr-Zr alloy in Comparative Example 1, and in terms of elongation, such as Figures 5 to 7 As shown in the alloy stress-strain curve, the Cu-Cr-Zr-RE alloy is slightly different from the Cu-Cr-Zr alloy, but both have certain plasticity, so the comprehensive performance of the alloy plate in the present invention is more superior.
[0126] The Cu-Cr-Zr-RE alloy plate prepared by the present invention has a tensile strength of 620MPa-639MPa, a yield strength of 615MPa-633MPa, a relative conductivity of 85.2%IACS-88.5%IACS, and an elongation after fracture of 5.7%-9%.
[0127] It should be understood that the terms used herein are only for the purpose of describing specific example embodiments and are not intended to be limiting. Unless the context clearly indicates otherwise, the singular forms "one", "an" and "said" as used herein may also be meant to include plural forms. The terms "include", "comprise", "contain", and "have" are inclusive, and therefore specify the existence of stated features, steps, operations, elements and / or parts, but do not exclude the existence or addition of one or more other features, steps, operations, elements, parts, and / or combinations thereof. The method steps, processes, and operations described herein are not interpreted as necessarily requiring them to be performed in the specific order described or illustrated, unless the execution order is clearly indicated. It should also be understood that additional or alternative steps may be used.
[0128] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A method for preparing a high-strength and high-conductivity rare earth copper alloy Cu-Cr-Zr plate, characterized in that: The following steps are involved: The alloy ratio is made according to the alloy composition of the plate, and the metal single substance of each element and the master alloy are mixed and smelted, and cast to obtain an alloy ingot; wherein the alloy composition of the plate contains the following elements in percentage by mass: 0.58% to 0.62% Cr element, 0.13% to 0.17% Zr element, 0.09% to 0.11% rare earth element, and the balance is Cu element; the rare earth element is Ce element, or Ce and La element; The alloy ingot is subjected to solution treatment, three rolling and three-step aging treatments alternately and continuously, wherein the temperature of the three rollings is 22°C to 26°C, and the heating rate of the three-step aging treatment is 5°C / min to 10°C / min, to obtain the high-strength and high-conductivity rare earth copper alloy Cu-Cr-Zr plate; During smelting, the Cr element is added in the form of a Cu-Cr master alloy, the Zr element is added in the form of a Cu-Zr master alloy, the rare earth element is added in the form of a Cu-rare earth element master alloy, and the Cu element is added in the form of single copper, and the purity of the single copper is greater than or equal to 99.99%; The smelting process comprises: adding single copper into a graphite crucible and adding a graphite powder covering agent, using a medium frequency induction melting furnace, in an atmospheric environment, heating up to 1250°C-1260°C at a rate of 50°C / min-100°C / min with the furnace and keeping the temperature, and after the copper is completely melted, continuing to heat up to 1350°C-1360°C, adding a Cu-Cr master alloy, and keeping the temperature until it is completely melted; cooling down to 1250°C-1260°C at a rate of 10°C / min-30°C / min and keeping the temperature, adding a Cu-Zr master alloy, and after it is completely melted, adding a Cu-rare earth element master alloy for smelting to obtain a mixed melt; The three-step rolling and three-step aging treatment process includes: The solution treated billet is subjected to a first rolling, and the billet is subjected to a first aging treatment; the deformation of the first rolling is 75% to 85%, the temperature of the first aging treatment is 440° C. to 460° C., and the time is 55 min to 65 min; and The billet after the first aging treatment is subjected to a second rolling, and the billet after the second rolling is subjected to a second aging treatment; the deformation amount of the second rolling is 65% to 75%, the temperature of the second aging treatment is 390° C. to 410° C., and the time is 25 min to 35 min; and The billet after the second aging treatment is rolled for the third time, and the billet after the third rolling is subjected to the third aging treatment, the deformation amount of the third rolling is 45%~55%, the temperature of the third aging treatment is 390℃~410℃, and the time is 25min~35min.
2. The method for preparing the high-strength and high-conductivity rare earth copper alloy Cu-Cr-Zr sheet according to claim 1, characterized in that: The Cr element is added in the form of a Cu-Cr master alloy, and the mass fraction of the Cr element is 10% to 15%; The Zr element is added in the form of a Cu-Zr master alloy, and the mass fraction of the Zr element is 20% to 40%; The rare earth element is added in the form of a Cu-rare earth element master alloy, and the mass fraction of the rare earth element is 10% to 20%.
3. The method for preparing the high-strength and high-conductivity rare earth copper alloy Cu-Cr-Zr sheet according to claim 1, characterized in that: The alloy ingot is obtained by non-vacuum melting and near-liquidus casting; wherein, in the near-liquidus casting method, a graphite mold with a temperature of 300°C to 320°C is used, and the casting temperature is 1100°C to 1120°C.
4. The method for preparing the high-strength and high-conductivity rare earth copper alloy Cu-Cr-Zr sheet according to claim 1, characterized in that: The solution treatment process includes: placing the alloy ingot into a heat treatment furnace, heating the furnace to 940°C-960°C, keeping the temperature for 115min-125min, and then quenching in water at a water temperature of 22°C-26°C.