Carbon cloth-supported CuS / SnS2 heterostructure photo-assisted electrode materials, preparation and applications
By loading CuS/SnS2 nanoparticles in situ on the carbon cloth to form a heterostructure, the problem of low photogenerated charge carrier recombination efficiency of tin disulfide-based materials is solved, and the photo-assisted charging capacity and electrode performance are improved. It is suitable for light Auxiliary supercapacitor.
Patent Information
- Application Number
- CN202411161747.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-23
AI Technical Summary
Tin disulfide-based materials have the problem of low photogenerated charge carrier recombination efficiency in supercapacitors, which limits their photo-assisted charging capabilities and affects capacitance performance.
The carbon cloth is equipped with CuS/SnS2 heterostructured photo-assisted electrode material, and the carbon cloth is pretreated and SnS2 and CuS nanoparticles are loaded in situ on its surface to form a heterostructure to improve the photogenerated carrier separation efficiency.
It significantly improves the optical assisted charging capacity, enhances the specific capacity and capacity retention rate of the electrode, and is suitable for optical assisted supercapacitors.
Smart Images

Figure CN118675905B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of light-assisted energy storage electrode materials, and in particular to a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material, and its preparation and application. Background Art
[0002] With the rapid consumption of non-renewable energy, people's demand for renewable energy is increasing. Therefore, it is very important to develop green and sustainable methods to improve energy storage efficiency. Among various sustainable energy sources, sunlight has been widely used due to its advantages such as abundance, easy access and cleanliness. Therefore, people have introduced it into energy storage devices to improve the performance of materials, and developed energy storage devices with photocharging or photo-assisted charging capabilities to promote its electrochemical charge storage using solar energy. Although tin disulfide has the disadvantages of low conductivity and poor cycle stability, it has the advantages of excellent theoretical specific capacity, environmental friendliness and low cost. As a photosensitive semiconductor, tin disulfide has been widely used in photocatalysis, solar cells and supercapacitors. However, the photoinduced capacitance enhancement behavior of supercapacitors based on tin disulfide-based materials has not been reported in the literature, which may be related to the easy recombination of tin disulfide-based materials with photogenerated charge carriers. However, since supercapacitors based on tin disulfide-based materials have great application potential, it is a very important issue to study the ability of photo-assisted charging of supercapacitors based on tin disulfide-based materials to enhance their capacitance. Summary of the invention
[0003] In order to solve the problem that tin disulfide-based materials are easily recombined with photogenerated charge carriers, the present invention provides a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material, preparation and application.
[0004] The present invention is achieved through the following technical scheme: A method for preparing a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material, comprising the following steps:
[0005] S1: Pretreatment of carbon cloth
[0006] S2: Preparation of SnS2@CC
[0007] A mixed aqueous solution is obtained by mixing tin chloride, citric acid and thiourea, and the pretreated carbon cloth (abbreviated as CC) is mixed with the mixed aqueous solution, and heated in a sealed container for reaction; after naturally cooling to room temperature, the carbon cloth with SnS2 attached is taken out, rinsed with deionized water, and dried to obtain SnS2@CC;
[0008] S3: Preparation of CuS / SnS2@CC
[0009] The ethylene glycol solution of thioacetamide is added to the aqueous solution of copper sulfate, and after mixing and reaction, a brown suspension is obtained; then SnS2@CC and the brown suspension are heated to react in a sealed container; naturally cooled to room temperature, the carbon cloth attached with SnS2 and CuS is taken out, rinsed with deionized water, and dried to obtain CuS / SnS2@CC, which is a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material.
[0010] As a further improvement of the technical solution of the present invention, in step S2, the pretreated carbon cloth is mixed with the mixed aqueous solution and heated in a sealed container at a reaction temperature of 160-200° C. for a heating reaction time of 8-14 hours.
[0011] As a further improvement of the technical solution of the present invention, in step S3, SnS2@CC and the brown suspension are heated in a reaction container at a reaction temperature of 170-190° C. and a heating reaction time of 4-6 h.
[0012] As a further improvement of the technical solution of the present invention, in step S2, the molar ratio of tin chloride, citric acid and thiourea is 0.00028-0.00075:0.00073-0.0020:0.00085-0.0023.
[0013] As a further improvement of the technical solution of the present invention, in step S3, the molar ratio of thioacetamide to copper sulfate is 0.0034-0.013:0.0025-0.01, and the molar ratio of tin chloride in step S2 to copper sulfate in step S3 is 0.00028-0.00075:0.0025-0.01.
[0014] As a further improvement of the technical solution of the present invention, in step S1, the pretreatment of the carbon cloth includes the following steps: ultrasonic cleaning to remove impurities on the surface of the carbon cloth, and after drying, soaking the carbon cloth in concentrated nitric acid. After soaking, repeatedly washing the carbon cloth to remove residual acid on the surface of the carbon cloth, and drying to complete the pretreatment of the carbon cloth.
[0015] As a further improvement of the technical solution of the present invention, the carbon cloth is immersed in concentrated nitric acid at room temperature and for 10-12 hours.
[0016] The present invention also provides the use of CuS / SnS2@CC obtained by the preparation method of the carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material as an electrode material in light-assisted energy storage.
[0017] As a further improvement of the application technical solution of the present invention, the light-assisted energy storage is a light-assisted supercapacitor.
[0018] The present invention also provides a CuS / SnS2@CC obtained by a method for preparing a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material.
[0019] The carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material, preparation and application of the present invention have the following advantages compared with the prior art:
[0020] The CuS / SnS2 heterostructure is loaded on the carbon cloth substrate by the in-situ loading method. The formation of the heterostructure greatly improves the separation efficiency of photogenerated carriers and greatly improves the light-assisted charging capability, thereby improving the specific capacity and capacity retention rate of the electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0023] Figure 1 This is the XRD comparison diagram of CC in Comparative Example 1, SnS2@CC in Comparative Example 2, and CuS / SnS2@CC in Example 1.
[0024] Figure 2 This is the XPS comparison chart of Sn 3d of SnS2@CC in Comparative Example 2 and CuS / SnS2@CC in Example 1.
[0025] Figure 3 The following is a comparison of the UV curves of pure SnS2 and CuS. (a) is the UV curve of pure SnS2, and (b) is the UV curve of pure CuS.
[0026] Figure 4 The energy band gap comparison diagram of pure SnS2 and CuS. In the figure, (a) is the energy band gap diagram of pure SnS2, and (b) is the energy band gap diagram of pure CuS.
[0027] Figure 5 The XPS valence band spectrum comparison of pure SnS2 and CuS. (a) is the XPS valence band spectrum of pure SnS2, and (b) is the XPS valence band spectrum of pure CuS.
[0028] Figure 6 Schematic diagram of the energy band arrangement of CuS / SnS2@CC in Example 1.
[0029] Figure 7 The current density is 0.5 mA cm -2 GCD comparison diagram of CuS / SnS2@CC in Example 1, CC in Comparative Example 1, SnS2@CC in Comparative Example 2, and CuS@CC in Comparative Example 3.
[0030] Figure 8 This is a comparison chart of the capacity retention rates of CuS / SnS2@CC in Example 1, SnS2@CC in Comparative Example 2, and CuS@CC in Comparative Example 3.
[0031] Fig. 9 This is a comparison diagram of the impedance of CuS / SnS2@CC in Example 1 under dark and light conditions.
[0032] Fig.10 The current density is 0.5 mA cm -2 GCD comparison diagram of CuS / SnS2@CC in Example 1 under dark and light conditions.
[0033] Fig.11 The current density is 0.5 mA cm -2 GCD comparison of SnS2@CC in comparative example 2 under dark and light conditions.
[0034] Fig.12 Specific capacity and photoinduced capacitance increase percentage of CuS / SnS2@CC in Example 1 at a series of charge and discharge current densities under dark and visible light illumination. DETAILED DESCRIPTION
[0035] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0036] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.
[0037] The present invention provides a method for preparing a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material, comprising the following steps:
[0038] S1: Pretreatment of carbon cloth
[0039] S2: Preparation of SnS2@CC
[0040] A mixed aqueous solution is obtained by mixing tin chloride, citric acid and thiourea, and the pretreated carbon cloth is mixed with the mixed aqueous solution, and heated in a sealed container for reaction; after naturally cooling to room temperature, the carbon cloth with SnS2 attached is taken out, rinsed with deionized water, and dried to obtain SnS2@CC;
[0041] S3: Preparation of SnS2 / CuS@CC
[0042] The ethylene glycol solution of thioacetamide is added to the aqueous solution of copper sulfate, and after mixing and reaction, a brown suspension is obtained; then SnS2@CC and the brown suspension are heated to react in a sealed container; naturally cooled to room temperature, the carbon cloth attached with SnS2 and CuS is taken out, rinsed with deionized water, and dried to obtain CuS / SnS2@CC, which is a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material.
[0043] In one embodiment provided by the present invention, in step S2, the pretreated carbon cloth is mixed with the mixed aqueous solution and heated in a sealed container at a reaction temperature of 160-200°C, and the heating reaction time is 8-14h. In different embodiments, in step S2, the reaction temperature can be 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 185°C, 190°C, 195°C, 200°C, or at a reaction temperature within any two defined ranges. In different embodiments, in step S2, the reaction time can be 8h, 8.5h, 9h, 9.5h, 10h, 10.5h, 11h, 11.5h, 12h, 12.5h, 13h, 13.5h, 14h, or at a reaction time within any two defined ranges. The sealed container in the present invention can be a stainless steel reactor lined with polytetrafluoroethylene, or it can be other closed containers with heating function.
[0044] In another embodiment provided by the present invention, in step S3, SnS2@CC and the brown suspension are heated in a sealed container at a reaction temperature of 170-190°C, and the heating reaction time is 4-6h. In different embodiments, in step S3, the reaction temperature can be 170°C, 175°C, 180°C, 185°C, 185°C, 190°C, or at a reaction temperature within any two defined ranges. In different embodiments, in step S3, the reaction time can be 4h, 4.5h, 5h, 5.5h, 6h, or at a reaction time within any two defined ranges. The sealed container in the present invention can be a stainless steel autoclave lined with polytetrafluoroethylene, or it can be other closed containers with heating function.
[0045] In one embodiment provided by the present invention, in step S2, the molar ratio of tin chloride, citric acid and thiourea is 0.00028-0.00075:0.00073-0.0020:0.00085-0.0023. In step S3, the molar ratio of thioacetamide to copper sulfate is 0.0034-0.013:0.0025-0.01, and the molar ratio of tin chloride in step S2 to copper sulfate in step S3 is 0.00028-0.00075:0.0025-0.01.
[0046] In another embodiment provided by the present invention, in step S1, the pretreatment of the carbon cloth includes the following steps: ultrasonic cleaning to remove impurities on the surface of the carbon cloth, and after drying, soaking the carbon cloth in concentrated nitric acid. After soaking, repeatedly washing the carbon cloth to remove the acid remaining on the surface of the carbon cloth, and drying to complete the pretreatment of the carbon cloth. Specifically, the soaking temperature of the carbon cloth in concentrated nitric acid is room temperature, and the soaking time is 10-12 hours.
[0047] The present invention also provides the use of CuS / SnS2@CC obtained by the method for preparing the carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material as an electrode material in light-assisted energy storage. The CuS / SnS2@CC prepared by the above method has good light-assisted performance, thereby improving the specific capacity and rate performance, and is suitable for the electrode material of light-assisted supercapacitors.
[0048] The present invention further provides CuS / SnS2@CC obtained by the preparation method of the carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material.
[0049] The specific embodiments of the present invention are described in detail below.
[0050] Example 1
[0051] 1.1 Pretreatment of carbon cloth
[0052] First, the carbon cloth (CC) was ultrasonically cleaned in an ultrasonic bath for 20 min with acetone, anhydrous ethanol and deionized water to remove surface impurities. The cleaned carbon cloth was dried in an oven at 80 °C for 12 h. After drying, the carbon cloth was soaked in 50 ml of 12M concentrated nitric acid at room temperature of 25 °C for 12 h, and then repeatedly rinsed with distilled water to remove residual acid, and then dried in an oven at 60 °C overnight.
[0053] 1.2 Preparation of SnS2@CC
[0054] 0.1315g SnCl4·5H2O, 0.1875g citric acid (C6H8O7) and 0.0857g thiourea (CH4N2S) were dissolved in 15ml deionized water, and magnetic stirring was performed until completely dissolved. The pretreated CC was mixed with the solution and sealed in a stainless steel reactor lined with polytetrafluoroethylene, and heated to 180°C for 12h. After cooling naturally to room temperature, the CC attached with SnS2 was taken out from the reactor, rinsed with deionized water three times, and dried in an oven at 80°C overnight to obtain SnS2@CC.
[0055] The molar ratio of SnCl4·5H2O, citric acid and thiourea is 0.00036:0.00098:0.0011.
[0056] 1.3 Preparation of CuS / SnS2@CC
[0057] Dissolve 1.2484gCuSO4·5H2O in 26mL deionized water and stir until completely dissolved. Then, take 0.506g thioacetamide (CH3CSNH2), fully dissolve it in 10ml ethylene glycol, and then slowly add it to the above solution. After 60min of reaction, it becomes a brown suspension with an odor. The prepared SnS2@CC and the obtained brown suspension are placed in a 20ml stainless steel autoclave lined with polytetrafluoroethylene and heated to 180℃ for 5h. Finally, cool to room temperature, rinse the CC attached with SnS2 and CuS with deionized water 3 times, and then dry it in an oven at 80℃ for 12h to obtain CuS / SnS2@CC.
[0058] Wherein, the molar ratio of thioacetamide to copper sulfate is 0.0067:0.005.
[0059] Furthermore, the CuS / SnS2@CC obtained in Example 1 was characterized and experimentally tested. For specific results, see Figure 1-2 , Figure 6-10 as well as Fig.12 .
[0060] Comparative Example 1
[0061] An untreated carbon cloth (CC) of 1.8 cm×1.8 cm was used.
[0062] The carbon cloth (CC) in comparative example 1 was tested experimentally. For specific results, see Figure 1 , Figure 7 .
[0063] Comparative Example 2
[0064] First, the CC was ultrasonically cleaned in an ultrasonic bath for 20 min with acetone, anhydrous ethanol and deionized water to remove surface impurities. The cleaned carbon cloth was dried in an oven at 80 °C for 12 h. After drying, the carbon cloth was soaked in 50 ml of 12 M concentrated nitric acid at room temperature 25 °C for 12 h, then repeatedly rinsed with distilled water to remove residual acid, and then dried in an oven at 60 °C overnight.
[0065] 0.1315g SnCl4·5H2O, 0.1875g citric acid (C6H8O7) and 0.0857g thiourea (CH4N2S) were dissolved in 15ml deionized water, and magnetic stirring was performed until completely dissolved. The pretreated CC was mixed with the solution and sealed in a stainless steel reactor lined with polytetrafluoroethylene, and heated to 180°C for 12h. After cooling naturally to room temperature, the CC attached with SnS2 was taken out from the reactor, rinsed with deionized water three times, and dried in an oven at 80°C overnight to obtain SnS2@CC.
[0066] The SnS2@CC in comparative example 2 was tested experimentally. For specific results, see Figure 1-2 , Figure 7-8 as well as Fig.11 .
[0067] Comparative Example 3
[0068] First, the CC was ultrasonically cleaned in an ultrasonic bath for 20 min with acetone, anhydrous ethanol and deionized water to remove surface impurities. The cleaned carbon cloth was dried in an oven at 80 °C for 12 h. After drying, the carbon cloth was soaked in 50 ml of 12 M concentrated nitric acid at room temperature 25 °C for 12 h, then repeatedly rinsed with distilled water to remove residual acid, and then dried in an oven at 60 °C overnight.
[0069] Dissolve 1.2484gCuSO4·5H2O in 26mL deionized water and stir until completely dissolved. Subsequently, take 0.506g thioacetamide (CH3CSNH2), fully dissolve it in 10ml ethylene glycol, and then slowly add it dropwise to the above solution. After 60min of reaction, it becomes a brown suspension with an odor. Mix the pretreated CC with this solution, seal it in a stainless steel reactor lined with polytetrafluoroethylene, heat it to 180℃, and heat it for 5h. After naturally cooling to room temperature, take out the CC with CuS attached from the reactor, rinse it with deionized water 3 times, and dry it in an oven at 80℃ overnight to obtain CuS@CC.
[0070] The CuS@CC in comparative example 3 was tested experimentally. For specific results, see Figure 7-8 .
[0071] Experimental testing
[0072] Figure 1 The X-ray diffraction patterns (XRD) of the CC sample of Comparative Example 1, the SnS2@CC sample of Comparative Example 2, and the CuS / SnS2@CC sample of Example 1 were compared. The three samples have a typical CC peak at 2θ=25°. The SnS2@CC sample of Comparative Example 2 has new diffraction peaks at 2θ=15.03°, 32.12°, 41.89°, 49.96°, and 52.45°, respectively, corresponding to the (001), (101), (102), (110), and (111) peaks of SnS2 (JCPDS: 23-0677), respectively. Therefore, XRD confirms the successful formation of SnS2 on the CC surface. The CuS / SnS2@CC sample of Example 1 showed several new diffraction peaks at 2θ=29.28°, 31.78°, 32.85°, 47.94°, 52.71°, and 59.35°, corresponding to the (102), (103), (006), (110), (108), and (116) peaks of the CuS (JCPDS: 06-0464) phase, respectively. Therefore, by loading CuS nanoparticles on the SnS2@CC sample, the second step of in situ growth was achieved, and the CuS / SnS2@CC sample was successfully prepared.
[0073] Figure 2 The upper part is the Sn 3d peak of the CuS / SnS2@CC sample of Example 1. There is a pair of peaks at 486.45eV and 494.91eV, which belong to Sn 3d 5 / 2 and Sn 3d 3 / 2 , Figure 2 The lower part shows the Sn 3d peak of the SnS2@CC sample of comparative example 2, with binding energies of 487.05 eV and 495.51 eV, respectively. Comparison of the Sn 3d bond energy spectra of SnS2@CC and CuS / SnS2@CC shows that the binding energy of the latter is reduced by 0.60 eV. Therefore, the introduction of CuS affects the electronic structure of SnS2, further confirming the construction of the CuS / SnS2@CC heterostructure material.
[0074] Figure 3 The UV images of SnS2 and CuS show that SnS2 exhibits light absorption from the ultraviolet range to the visible light region, and CuS has an absorption region from the ultraviolet range to the near infrared.
[0075] Figure 4 The band gap diagram of SnS2 and CuS is shown, with the band gaps being 1.84eV and 1.35eV respectively. Figure 5 XPS valence band spectra of SnS2 and CuS, E VB The values are 1.24eV and -0.08eV respectively.
[0076] Figure 6 The band alignment of CuS / SnS2@CC is shown. It is speculated that due to the energy level matching between SnS2 and CuS, the band edges of the two components are staggered in the heterostructure to form the band edge characteristics of a pn-type heterostructure. Figure 2 The combination shows that compared with SnS2@CC, the Sn 3d state of CuS / SnS2@CC sample shifts to the low energy region. This result shows that in the CuS / SnS2@CC sample, electrons migrate from CuS to SnS2, and photogenerated holes migrate from SnS2 to CuS. Moreover, SnS2 is an n-type semiconductor and CuS is a p-type semiconductor. This electron migration mechanism conforms to the pn-type mechanism.
[0077] Figure 7 The CC of Comparative Example 1, the SnS2@CC sample of Comparative Example 2, the CuS@CC sample of Comparative Example 3 and the CuS / SnS2@CC sample of Example 1 were compared as electrode materials at a current density of 0.5 mA cm -2 The constant current charge-discharge curves at 1000 s are shown. When conducting electrochemical tests, the traditional three-electrode system is used. CC, SnS2@CC, CuS@CC, and CuS / SnS2@CC are directly used as working electrodes, platinum wire electrodes and Ag / AgCl electrodes are used as counter electrodes and reference electrodes, respectively. The voltage window is -0.9-0.3V, and 3M KOH is used as the electrolyte. The voltage window and current parameters are set on the Jiangsu Donghua electrochemical workstation for electrochemical performance testing. It can be clearly seen that the discharge time of CC, SnS2@CC samples, and CuS@CC samples is shorter than that of CuS / SnS2@CC samples, proving that compared with a single material, the electrochemical performance of the CuS / SnS2@CC sample is better.
[0078] Figure 8 The capacity retention rates of the SnS2@CC sample of Comparative Example 2, the CuS@CC sample of Comparative Example 3, and the CuS / SnS2@CC sample of Example 1 as electrode materials are shown. The conventional three-electrode system is used and the current density is set to 0.5 mA cm -2 , 1mA cm -2 , 1.5mA cm -2 , 2mA cm -2 , 2.5mA cm -2 , 3mA cm -2 , tested on an electrochemical workstation, the voltage window, electrolyte, counter electrode and reference electrode are the same as above. As can be seen from the figure, when the current density is from 0.5mA cm -2 Increase to 3 mA cm -2When the specific capacity of CuS / SnS2@CC sample is calculated, it reaches 785.25mF cm -2 , the capacity retention rate is 75.30%.
[0079] Fig. 9 The Nyquist comparison diagram of the CuS / SnS2@CC sample of Example 1 as an electrode material under dark and light conditions is shown. The measurement frequency range is 10 -2 ~10 5 Hz, data under lighting conditions tested with a 300W xenon lamp. It can be clearly seen from the figure that it includes two different parts, including a semicircle in the medium and high frequency area and an inclined straight line in the low frequency area. The slope of the straight line in the low frequency area is limited, which can represent the diffusion behavior of the electrolyte in the electrode pores and the ions in the active material. Under visible light irradiation, the slope of the straight line of the CuS / SnS2@CC material in the low frequency region is greater than the slope of the straight line under dark conditions, indicating that visible light irradiation can enhance its conductivity through photogenerated carriers. In addition, the smaller semicircle diameter is displayed at medium and high frequencies under illumination conditions, indicating that light-assisted conditions help to improve the electron flow of the heterostructure, thereby effectively improving the interface resistance.
[0080] Fig.10 The charge and discharge current density of 0.5 mA cm-2 is shown in the dark and under visible light illumination. -2 , GCD curve comparison of CuS / SnS2@CC electrode in Example 1, tested on an electrochemical workstation, voltage window, electrolyte, counter electrode and reference electrode are the same as above, light source is 300W xenon lamp. It can be clearly seen that the discharge time is longer under light conditions.
[0081] Fig.11 The charge and discharge current density of 0.5 mA cm-2 is shown in the dark and under visible light illumination. -2 , Comparison of GCD curves of SnS2@CC electrode in Example 2, tested on an electrochemical workstation, voltage window, electrolyte, counter electrode and reference electrode are the same as above, and the light source is a 300W xenon lamp. Fig.10 By comparison, it can be seen that the charge and discharge time of the CuS / SnS2@CC electrode of Example 1 under light and dark conditions, as well as the time difference between the two conditions, are higher than those of the SnS2@CC electrode of Comparative Example 2. This further proves the specific advantages of the CuS / SnS2@CC electrode.
[0082] Fig.12 The specific capacity comparison diagram of the CuS / SnS2@CC sample in Example 1 as the electrode material at different current densities is shown in Figure 1. The conventional three-electrode system is used and the current density is set to 0.5 mA cm -2 , 1mA cm -2, 1.5mA cm -2 , 2mAcm -2 , 2.5mA cm -2 , 3mA cm -2 , tested on an electrochemical workstation, the voltage window, electrolyte, counter electrode and reference electrode are the same as above, and the light source is a 300W xenon lamp. The figure shows that at a current density of 0.5mA cm -2 When the specific capacity is calculated from 1043mF cm in dark conditions, -2 Increased to 1155mF cm in visible light conditions -2 , increased by 10.7% when the current density increased to 3 mA cm -2 When the photoelectric capacitance is increased by 17.4%,
[0083] The results show that the CuS / SnS2@CC prepared by the above method is expected to have good light-assisted performance as an electrode material, thereby improving the specific capacity and rate performance, and is suitable for the electrode material of light-assisted supercapacitors. The present invention provides a heterostructure material with improved light-assisted performance, and improves the specific capacity and capacity retention rate through the design of the heterostructure. The implementation process of the present invention is simple and has broad application prospects.
[0084] The above is only a specific implementation of the present invention, which enables those skilled in the art to understand or implement the present invention. Although detailed descriptions are given with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments, and they should all be covered by the protection scope of the claims.
Claims
1. A method for preparing a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material, characterized in that: The steps include: S1: Pretreatment of carbon cloth S2: Preparation of SnS2@CC A mixed aqueous solution is obtained by mixing tin chloride, citric acid and thiourea, and the pretreated carbon cloth is mixed with the mixed aqueous solution, and heated in a sealed container for reaction; after naturally cooling to room temperature, the carbon cloth with SnS2 attached is taken out, rinsed with deionized water, and dried to obtain SnS2@CC; S3: Preparation of CuS / SnS2@CC The ethylene glycol solution of thioacetamide is added to the aqueous solution of copper sulfate, and after mixing and reaction, a brown suspension is obtained; then SnS2@CC and the brown suspension are heated to react in a sealed container; naturally cooled to room temperature, the carbon cloth attached with SnS2 and CuS is taken out, rinsed with deionized water, and dried to obtain CuS / SnS2@CC, which is a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material.
2. The method for preparing a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material according to claim 1, characterized in that: In step S2, the pretreated carbon cloth and the mixed aqueous solution are mixed in a sealed container and heated to a reaction temperature of 160-200° C. for a heating reaction time of 8-14 hours.
3. The method for preparing a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material according to claim 1, characterized in that: In step S3, SnS2@CC and the brown suspension are heated in a reaction container at a reaction temperature of 170-190° C. for a heating reaction time of 4-6 h.
4. The method for preparing a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material according to claim 1, characterized in that: In step S2, the molar ratio of tin chloride, citric acid and thiourea is 0.00028-0.00075:0.00073-0.0020:0.00085-0.0023.
5. The method for preparing a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material according to claim 1, characterized in that: In step S3, the molar ratio of thioacetamide to copper sulfate is 0.0034-0.013:0.0025-0.01, and the molar ratio of tin chloride in step S2 to copper sulfate in step S3 is 0.00028-0.00075:0.0025-0.
01.
6. The method for preparing a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material according to claim 1, characterized in that: In step S1, the pretreatment of the carbon cloth includes the following steps: ultrasonic cleaning to remove impurities on the surface of the carbon cloth, and after drying, soaking the carbon cloth in concentrated nitric acid. After soaking, repeatedly washing the carbon cloth to remove residual acid on the surface of the carbon cloth, and drying to complete the pretreatment of the carbon cloth.
7. The method for preparing a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material according to claim 6, characterized in that: The carbon cloth is immersed in concentrated nitric acid at room temperature for 10-12 hours.
8. Application of CuS / SnS2@CC obtained by the method for preparing a carbon cloth-supported CuS / SnS2 heterostructure light-assisted electrode material as claimed in any one of claims 1 to 7 as an electrode material in light-assisted energy storage.
9. The use according to claim 8, characterized in that The light-assisted energy storage is a light-assisted supercapacitor.