Blade mold device and mold manufacturing method
By adopting the combined structure of the casting system mold shell, blade mold shell and splicing block in turbine blade casting, independent inspection and cleaning of mold shells is achieved, solving the problem of cracking of mold shells, core breakage and foreign matter cleaning, and improving castings Pass rate and production efficiency.
Patent Information
- Application Number
- CN202411162046.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-23
AI Technical Summary
During the precision casting of turbine blades, the prior art has problems such as cracking of mold shells, broken cores, and inability to clean foreign matters in mold shells, resulting in scrapping of castings, increasing costs and prolonging production cycles.
A blade mold shell device and mold shell manufacturing method are provided, and a combination structure of mold shell, blade mold shell and splicing block is adopted to realize independent inspection and cleaning of mold shells through connection channels, reducing cost waste.
Through independent inspection and cleaning, the efficiency of internal quality inspection of mold shells is improved, the unqualified mold shells enter the casting process is reduced, cost waste is reduced, and casting pass rate is improved.
Smart Images

Figure CN118682075B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of precision casting, and in particular to a blade mold shell device and a mold shell manufacturing method. Background Art
[0002] Turbine blades are the core hot end components of aircraft engines and industrial gas turbines, and have the characteristics of high quality requirements, high technical difficulty, high manufacturing cost, high technical development cost and long production process. Turbine blades are made of high-temperature alloys, which are expensive and account for more than 70% of the raw material cost of turbine blades. In order to improve production efficiency and alloy utilization, at present, multiple turbine blades are usually welded into a wax tree during the wax mold manufacturing stage, and then made into a mold shell (casting), that is, pouring a casting can produce multiple turbine blades at the same time.
[0003] For example, the propeller blade production process based on precision casting provided by Chinese patent CN202011453855.1 includes the following process steps: installing the wax cylinder and the wax model mold on the wax mold injection machine, aligning the wax nozzle of the injection machine with the wax injection port of the mold, and then starting to press the wax mold; installing the die head mold on the wax mold injection machine, aligning the wax nozzle of the injection machine with the wax injection port of the mold, and then starting to press the die head; taking out the pressed die head for inspection and removing unqualified products, heating the die head with a soldering iron and welding it to the weld of the wax mold; cleaning, dewaxing, and roasting the welded module; pouring molten metal from the die head into the shell, and completing the casting of the propeller blade after cooling.
[0004] However, in the process of precision casting of turbine blades, shell making, dewaxing, roasting and other processes often encounter problems such as mold cracking, core breaking, foreign matter in the mold and being unable to be cleaned. The mold, die head and wax mold used in the propeller blade production process provided by the patent are an integral structure, which has the following defects: First, it is inconvenient or impossible to conduct a good inspection of the inside of the mold. For example, cracking and core breaking on the inner surface can only be found after pouring the casting by non-destructive testing and other technical inspections. The consequences are scrapping of castings, increased costs and extended production cycles; second, when some foreign matter in the mold is cleaned by water cleaning and other methods, the foreign matter generally only flows out through the channel of the pouring cup (die head). For castings or pouring systems with complex structures, more foreign matter may remain and the cleaning effect is poor; third, when defects such as mold cracking and core breaking are found, the entire mold usually needs to be scrapped, delaying the construction period; and for hollow turbine blades, the price of a single ceramic core ranges from 200 to 1,000 yuan, and scrapping the mold will cause a waste of thousands of yuan in costs. Summary of the invention
[0005] The object of the present invention is to provide a blade mold device and a mold manufacturing method to solve the problems existing in the above-mentioned prior art, which is conducive to improving the qualified rate of castings and reducing or avoiding cost waste.
[0006] To achieve the above object, the present invention provides the following solutions:
[0007] The present invention provides a blade mold device, including a casting system mold, a blade mold and a splicing block, wherein the blade mold and the splicing block are at least one, each of the splicing blocks has a connecting channel running through the splicing block, the two ends of each of the splicing blocks are respectively fixedly connected to the casting system mold and one of the blade molds, and each of the connecting channels is connected to the casting system mold and the corresponding blade mold.
[0008] Preferably, each of the splicing blocks includes a first splicing block and a second splicing block that are interconnected, one end of the first splicing block is fixedly connected to one end of the second splicing block, the end face of the second splicing block connected to the first splicing block is a first end face, and the projection of the first splicing block on the plane where the first end face is located is located within the outer edge of the first end face; at least one connecting groove is provided on the end of the casting system mold away from the pouring port or on the side wall of the casting system mold, and a connecting hole is provided on the inner bottom wall of each connecting groove, and each connecting hole is connected to the pouring port; each of the first splicing blocks is at least partially arranged in one of the connecting holes, and each of the second splicing blocks is at least partially arranged in a corresponding one of the connecting grooves, and the first end face of each of the second splicing blocks can contact the inner bottom wall of the corresponding connecting groove.
[0009] Preferably, an adhesive layer is provided at least one between the outer wall of each first splicing block and the corresponding inner wall of the connecting hole, between each first end face and the corresponding inner bottom wall of the connecting groove, and between the outer wall of each second splicing block and the corresponding inner wall of the connecting groove.
[0010] Preferably, the blade mold shell and the splicing block are both multiple, the casting system mold shell is a casting wax mold, and the blade mold shell is a blade wax mold.
[0011] Preferably, the casting system mold shell includes a pouring cup, a filter screen mounting ring mold shell and a cross runner which are fixedly connected and communicated in sequence, and the side of the cross runner away from the pouring cup is connected to the splicing block.
[0012] The present invention provides a method for manufacturing a mold shell, comprising the following steps:
[0013] Obtain a casting system mold, at least one blade mold and at least one splicing block with a connecting channel, and respectively fix each splicing block to the casting system mold and one of the blade molds, and make the connecting channel communicate with both the casting system mold and the corresponding blade mold;
[0014] Or, obtain the casting system mold and at least one assembly, and the method for obtaining the assembly is: obtain at least one of the splicing blocks having the connecting channel, and when making the blade mold, mold the blade mold at one end of one of the splicing blocks to obtain the assembly; fix the other end of the splicing block to the casting system mold, and make the connecting channel communicate with the casting system mold and the corresponding blade mold.
[0015] Preferably, the method for forming the blade mold shell on the splicing block comprises: obtaining at least one blade mold, so that each of the blade molds can be detachably fixedly connected to one of the splicing blocks;
[0016] Connecting one of the splicing blocks to each of the blade molds, using each of the blade molds to make the blade mold shell, so that each of the splicing blocks is inlaid with one of the blade mold shells to form a combination;
[0017] The blade mold is removed from the splicing block.
[0018] Preferably, before each blade formwork is manufactured, the splicing blocks on each assembly are wrapped.
[0019] Preferably, a wax injection machine is used to manufacture the casting system mold and the blade mold.
[0020] Preferably, after the casting system mold and the blade mold are manufactured, the casting system mold and the blade mold are dewaxed; and the casting system mold and the blade mold are fired.
[0021] Compared with the prior art, the present invention has achieved the following technical effects:
[0022] The present invention provides a blade mold device and a mold manufacturing method, including a casting system mold, a blade mold and a splicing block, there are at least one blade mold and one splicing block, each splicing block has a connecting channel running through the splicing block, both ends of each splicing block are respectively fixedly connected to the casting system mold and a blade mold, and each connecting channel is connected to the casting system mold and the corresponding blade mold. The casting system mold and the blade mold of the above-mentioned blade mold device can be manufactured separately, and compared with the integral molding of the casting system mold and the blade mold, it has the following beneficial effects: first, after the casting system mold and the blade mold are processed, they can be inspected for defects separately, which is convenient for visual inspection or inspection with the help of an endoscope, and the internal quality of the mold can be better inspected, reducing or avoiding unqualified molds from entering the casting process, reducing or avoiding cost waste. Second, after the processing of the casting system mold and the blade mold is completed, they can be cleaned separately. The channel for the outflow of foreign matter is shorter, the channel diameter is larger, and the blade mold can be cleaned through the outlet of its own internal channel, which can significantly improve the reliability of foreign matter cleaning, greatly reduce the risk of foreign matter inclusion, and help improve the qualified rate of castings. Third, when the casting system mold and the blade mold are inspected and found to have defects such as broken cores and cracked shells, the casting system mold and the blade mold can be replaced separately to reduce cost consumption. At the same time, if the casting system mold and the blade mold are directly connected, the precision requirements for both are high, and the matching accuracy is difficult to ensure. The connection between the casting system mold and the blade mold is achieved through the splicing block. The splicing block only needs to achieve the matching and connection with the casting system mold and the blade mold. It does not need to have a complex shape and is easy to process and control the accuracy. Therefore, the casting system mold and the blade mold are connected through the splicing block, which is convenient for processing and ensures that the casting system mold and the blade mold can be well connected. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 It is a structural schematic diagram of the casting system mold shell in Example 1;
[0025] Figure 2 A schematic diagram of the structure of the splicing block provided in Example 1;
[0026] Figure 3 A cross-sectional view of the splicing block provided in Example 1;
[0027] Figure 4A schematic structural diagram of a blade shell device provided in Example 1;
[0028] Figure 5 A flow chart of the mold shell manufacturing method provided in Example 2;
[0029] Figure 6 It is a structural schematic diagram of the shell making tooling in Example 2;
[0030] In the figure: 100, blade mold device; 1, casting system mold; 101, connecting groove; 102, connecting hole; 103, pouring cup; 104, filter screen mounting ring mold; 105, cross runner; 2, blade mold; 3, splicing block; 301, first splicing block; 302, second splicing block; 303, first end face; 304, groove; 4, adhesive layer; 5, cutting line; 6, blade mold; 6, shell making tooling; 601, main body; 602, mold support; 603, handle. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] The object of the present invention is to provide a blade mold device and a mold manufacturing method to solve the problems existing in the above-mentioned prior art, which is conducive to improving the qualified rate of castings and reducing or avoiding cost waste.
[0033] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0034] Example 1
[0035] like Figure 1-4As shown, the present embodiment provides a blade mold device 100, including a casting system mold 1, a blade mold 2 and a splicing block 3, wherein there are at least one blade mold 2 and at least one splicing block 3, each splicing block 3 has a connecting channel penetrating the splicing block 3, and both ends of each splicing block 3 are respectively fixedly connected to the casting system mold 1 and a blade mold 2, and each connecting channel is connected to the casting system mold 1 and the corresponding blade mold 2. The casting system mold 1 and the blade mold 2 of the blade mold device 100 can be manufactured separately, and compared with the integral molding of the casting system mold 1 and the blade mold 2, it has the following beneficial effects: first, after the casting system mold 1 and the blade mold 2 are processed, they can be inspected for defects separately, which is convenient for visual inspection or inspection with the help of an endoscope, and the internal quality of the mold can be better inspected, which reduces or avoids unqualified molds from entering the casting process, and reduces or avoids cost waste. Second, after the gating system mold 1 and the blade mold 2 are processed, they can be cleaned separately. The channel for the outflow of foreign matter is shorter, the channel diameter is larger, and the blade mold 2 can be cleaned through the outlet of the inner cavity of the blade mold 2, which can significantly improve the reliability of foreign matter cleaning, greatly reduce the risk of foreign matter inclusion, and help improve the qualified rate of castings. Third, when the gating system mold 1 and the blade mold 2 are inspected and found to have defects such as broken cores and cracked shells, the gating system mold 1 and the blade mold 2 can be replaced separately to reduce cost consumption. At the same time, if the casting system mold 1 and the blade mold 2 are directly connected, the precision requirements for the two are high, and the matching accuracy is difficult to ensure. The connection between the casting system mold 1 and the blade mold 2 is achieved through the splicing block 3. The splicing block 3 only needs to achieve the matching and connection with the casting system mold 1 and the blade mold 2. It does not need to have a complex shape and is easy to process and control the accuracy. Therefore, the casting system mold 1 and the blade mold 2 are connected through the splicing block 3, which is convenient for processing and ensures that the casting system mold 1 and the blade mold 2 can be well connected.
[0036] As a preferred embodiment, the splicing block 3 is made of metal.
[0037] In this embodiment, each splicing block 3 includes a first splicing block 301 and a second splicing block 302 which are interconnected, one end of the first splicing block 301 is fixedly connected to one end of the second splicing block 302, the end face of the second splicing block 302 connected to the first splicing block 301 is the first end face 303, and the projection of the first splicing block 301 on the plane where the first end face 303 is located is located within the outer edge of the first end face 303; at least one connecting groove 101 is provided on the end of the casting system mold shell 1 away from the pouring port or on the side wall of the casting system mold shell 1, and a connecting hole 102 is provided on the inner bottom wall of each connecting groove 101, and each connecting hole 102 is connected to the pouring port; each first splicing block 301 is at least partially arranged in a connecting hole 102, and each second splicing block 302 is at least partially arranged in a corresponding connecting groove 101, and the first end face 303 of each second splicing block 302 can contact the inner bottom wall of the corresponding connecting groove 101. The inner bottom wall of the connection groove 101 can limit and position the connection block, so as to facilitate the connection between the splicing block 3 and the casting system mold shell 1.
[0038] In this embodiment, an adhesive layer 4 is provided at least one place between the outer wall of each first splicing block 301 and the inner wall of the corresponding connecting hole 102, between each first end face 303 and the inner bottom wall of the corresponding connecting groove 101, and between the outer wall of each second splicing block 302 and the inner wall of the corresponding connecting groove 101. Since the inner bottom wall of the connecting groove 101 can limit and position the connecting block, the convenience of the bonding operation and the firmness of the bonding can be improved, while reducing or avoiding the risk of slag falling.
[0039] As a preferred embodiment, an adhesive layer 4 is provided between each first end surface 303 and the inner bottom wall of the corresponding connection groove 101 , and between the outer wall of each second assembly block 302 and the inner wall of the corresponding connection groove 101 .
[0040] In this embodiment, there are multiple blade mold shells 2 and splicing blocks 3, which is conducive to improving processing efficiency. The casting system mold shell 1 is a casting wax mold, and the blade mold shell 2 is a blade wax mold.
[0041] In this embodiment, the casting system mold shell 1 includes a pouring cup 103, a filter screen mounting ring mold shell 104 and a runner 105 which are fixedly connected and connected in sequence, and the side of the runner 105 away from the pouring cup 103 is connected to the splicing block 3. The filter screen mounting ring mold shell 104 is used to manufacture a filter screen mounting ring, and the filter screen mounting ring is used to install a filter screen to filter the casting liquid.
[0042] Example 2
[0043] like Figure 5 As shown, this embodiment provides a mold shell manufacturing method, comprising the following steps:
[0044] Obtain a casting system mold 1, at least one blade mold 2 and at least one splicing block 3 with a connecting channel, and respectively fix the two ends of each splicing block 3 to the casting system mold 1 and a blade mold 2, and make the connecting channel communicate with the casting system mold 1 and the corresponding blade mold 2;
[0045] Or, obtain a casting system mold 1 and at least one assembly, and the method for obtaining the assembly is: obtain at least one splicing block 3 with a connecting channel, and when making a blade mold 2, mold the blade mold 2 at one end of a splicing block 3 to obtain the assembly; fix the other end of the splicing block 3 to the casting system mold 1, and make the connecting channel connected to the casting system mold 1 and the corresponding blade mold 2.
[0046] This embodiment provides great convenience for the inspection of cracks inside the mold shell, broken core inspection, replacement of the casting system mold shell 1 and / or the blade mold shell 2, and inspection and cleaning of foreign matter inside the mold shell. It can reduce or avoid the flow of unqualified mold shells to the casting process, reduce alloy waste, greatly shorten the production cycle, and can replace the casting system mold shell 1 and the blade mold shell 2 separately, which can enhance the flexibility of turbine blade precision casting production.
[0047] In this embodiment, the method for forming the blade mold shell 2 on the splicing block 3 includes: obtaining at least one blade mold so that each blade mold can be detachably fixedly connected to a splicing block 3; connecting a splicing block 3 to each blade mold, using each blade mold to make a wax mold of the blade mold shell 2, and forming each blade mold shell 2 on the corresponding splicing block 3, so that each blade mold shell 2 is inlaid with a splicing block 3 to form a combination; removing the blade mold from the splicing block 3.
[0048] As a preferred embodiment, a protrusion or groove 304 is provided at one end of the splicing block 3 for connecting with the blade mold, and a groove or protrusion is provided at one end of the blade mold for connecting with the splicing block 3, and the splicing block 3 and the blade mold are detachably fixedly connected by the engagement of the groove 304 and the protrusion. As a more preferred embodiment, grooves 304 are provided on two oppositely disposed outer side walls of the second splicing block 302 of the splicing block 3, and the grooves 304 are used to be inlaid with the blade mold or the wax mold.
[0049] In this embodiment, before each blade formwork 2 is manufactured, the splicing blocks 3 on each assembly are wrapped.
[0050] In this embodiment, a wax injection machine is used to manufacture the casting system mold 1 and the blade mold 2.
[0051] In this embodiment, after the casting system mold shell 1 and the blade mold shell 2 are manufactured, the casting system mold shell 1 and the blade mold shell 2 are dewaxed; and the casting system mold shell 1 and the blade mold shell 2 are baked.
[0052] The detailed operation steps of this embodiment are as follows:
[0053] 1. Use a general wax injection machine and wax injection parameters to make a casting mold. The structural diagram of the casting mold is as follows: Figure 1 It should be noted that Figure 1 The purpose is to illustrate the typical structure of spliced casting, but the specific structure of the casting mold is not limited to Figure 1 In the structure shown, the casting mold can adjust the size and / or shape of the casting mold and the splicing block 3 according to the process design or the blade size.
[0054] A general wax injection machine and wax injection parameters are used to make a blade mold. The blade mold is embedded with a prefabricated alumina splicing block 3. The splicing block 3 is shaped as follows: Figure 2 and 3 shown.
[0055] 2. Perform shell making operations on the blade mold and the casting mold respectively to obtain the blade mold shell 2 and the casting system mold shell 1 respectively. Before the blade mold shell is made, the splicing block 3 is wrapped with tape to ensure that the splicing block 3 is not stained with shell making materials.
[0056] As a preferred embodiment, in order to improve the shell production efficiency of the blade mold, a special shell making tool 6 is designed to realize the shell making operation of multiple blade molds at the same time. Figure 6 The shell making tool 6 shown includes a main body 601 and a plurality of mold support members 602 fixedly connected to the main body 601. The end of the splicing block 3 away from the blade mold shell 2 can be plugged into a mold support member 602, that is, the mold support member 602 can be inserted into the end of the connecting channel away from the blade mold shell 2, and the outer side wall of the end of the mold support member 602 away from the main body 601 is completely in contact with the inner side wall of the end of the connecting channel away from the blade mold shell 2, so as to support the blade mold shell 2. The shell making tool 6 can also include a handle 603, which is fixedly connected to the side of the main body 601 away from the mold support member 602. The shell making tool 6 is made of metal.
[0057] Use a cutting machine or an angle grinder to manually cut off the mold shell of the pouring system mold shell 1 at the splicing position along the cutting line 5, so that the lower end of the pouring system mold shell 1 forms an opening for communicating with the splicing block 3. The cutting line 5 is Figure 1 The dotted line position is shown.
[0058] 3. Dewaxing the blade mold shell 2 and the casting system mold shell 1.
[0059] 4. The blade mold shell 2 and the casting system mold shell 1 are baked.
[0060] 5. Check the blade mold 2 and the casting system mold 1 to ensure that the molds have no defects such as cracks.
[0061] 6. Prepare the adhesive slurry: Use a clean plastic container to weigh 500 ml of the surface slurry, add the surface powder into the surface slurry, and stir until the slurry becomes viscous.
[0062] 7. Use the adhesive paste prepared in step 6 to bond the splicing block 3 to the splicing position of the casting system mold shell 1. It should be noted that the gap between the splicing position of the splicing block 3 and the casting system mold shell 1 also needs to be filled with adhesive paste, as shown in the schematic diagram. Figure 4 shown.
[0063] 8. Allow the assembled mold shell to dry naturally for more than 24 hours before using it for pouring.
[0064] The present invention uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core ideas of the present invention. At the same time, for those skilled in the art, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A blade shell device, characterized in that: It comprises a casting system mold, a blade mold and a splicing block, wherein the blade mold and the splicing block are at least one, each of the splicing blocks has a connecting channel running through the splicing block, and both ends of each of the splicing blocks are respectively fixedly connected to the casting system mold and one of the blade molds, and each of the connecting channels is connected to the casting system mold and the corresponding blade mold; Each of the splicing blocks includes a first splicing block and a second splicing block that are interconnected, one end of the first splicing block is fixedly connected to one end of the second splicing block, the end face of the second splicing block connected to the first splicing block is the first end face, and the projection of the first splicing block on the plane where the first end face is located is located within the outer edge of the first end face; at least one connecting groove is provided on the end of the casting system mold away from the pouring port or on the side wall of the casting system mold, and a connecting hole is provided on the inner bottom wall of each connecting groove, and each connecting hole is connected to the pouring port; each of the first splicing blocks is at least partially arranged in one of the connecting holes, and each of the second splicing blocks is at least partially arranged in a corresponding one of the connecting grooves, and the first end face of each of the second splicing blocks can contact the inner bottom wall of the corresponding connecting groove.
2. The blade formwork device according to claim 1, characterized in that: An adhesive layer is provided at least one between the outer wall of each first assembling block and the inner wall of the corresponding connecting hole, between each first end surface and the inner bottom wall of the corresponding connecting groove, and between the outer wall of each second assembling block and the inner wall of the corresponding connecting groove.
3. The blade formwork device according to claim 1, characterized in that: There are multiple blade mold shells and multiple splicing blocks. The casting system mold shell is a casting wax mold, and the blade mold shell is a blade wax mold.
4. The blade formwork device according to claim 1, characterized in that: The casting system mold shell comprises a pouring cup, a filter screen mounting ring mold shell and a cross runner which are fixedly connected and communicated in sequence, and the side of the cross runner away from the pouring cup is connected to the splicing block.
5. A method for manufacturing a mold shell of a blade mold shell device according to any one of claims 1 to 4, characterized in that: The steps include: Obtain a casting system mold, at least one blade mold and at least one splicing block with a connecting channel, and respectively fix each splicing block to the casting system mold and one of the blade molds, and make the connecting channel communicate with both the casting system mold and the corresponding blade mold; Or, obtaining the casting system mold and at least one assembly, wherein the assembly is obtained by: obtaining at least one of the splicing blocks having the connecting channel, and when making the blade mold, molding the blade mold at one end of one of the splicing blocks to obtain the assembly; The other end of the splicing block is fixedly connected to the casting system mold shell, and the connecting channel is communicated with the casting system mold shell and the corresponding blade mold shell.
6. The method for manufacturing a mold shell according to claim 5, characterized in that: The method for forming the blade mold shell on the splicing block comprises: obtaining at least one blade mold, so that each of the blade molds can be detachably fixedly connected to one of the splicing blocks; Connecting one of the splicing blocks to each of the blade molds, using each of the blade molds to make the blade mold shell, so that each of the splicing blocks is inlaid with one of the blade mold shells to form a combination; The blade mold is removed from the splicing block.
7. The method for manufacturing a mold shell according to claim 6, characterized in that: Before each blade formwork is manufactured, the splicing blocks on each assembly are wrapped.
8. The method for manufacturing a mold shell according to claim 5, characterized in that: A wax injection machine is used to manufacture the casting system mold and the blade mold.
9. The method for manufacturing a mold shell according to claim 8, characterized in that: After the casting system mold shell and the blade mold shell are manufactured, the casting system mold shell and the blade mold shell are dewaxed; and the casting system mold shell and the blade mold shell are baked.
Citation Information
Patent Citations
Propeller blade production process based on precision casting
CN112642991A
A the gating system and single crystal blade be wax tree structure for shaping for single crystal blade