A method for synthesizing a highly oxygen-permeable ionomer using benzoyl peroxide as an initiator, and its product, film and application

By using benzoyl peroxide as an initiator and a composite solvent of chloroform with perfluorohexane or trifluorotrichloroethane, the production problem of perfluorosulfonic acid resin poly (PDD-co-PSVE) in the prior art has been solved. It achieves efficient and low-cost synthesis, improves the oxygen permeability and stability of the product, and is suitable for the catalyst layer of hydrogen fuel cells.

CN118684808BActive Publication Date: 2024-11-08FUJIAN KERUN CENTURY HYDROGEN ENERGY MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411160806.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The prior art is difficult to produce high-oxygen perfluorosulfonic acid resin poly (PDD-co-PSVE) in a large scale at low cost, efficient and stable, and the existing initiators are not easy to produce and are expensive, and they are unable to effectively replace the high-cost full. Fluorine structure initiator to obtain stable highly oxygen permeable ionomers.

Method used

Using benzoyl peroxide as an initiator, a composite solvent composed of chloroform, perfluorohexane or trifluorotrichloroethane is used to improve the efficiency of free radical initiation. By adjusting the reaction conditions and solvent ratio, poly(PDD-co is successfully improved. -PSVE) molecular weight, proton conductivity and oxygen permeability achieve efficient and low-cost synthesis.

Benefits of technology

The high-efficiency synthesis of poly (PDD-co-PSVE) is achieved, the comprehensive performance and production stability of the product are improved, the yield reaches 90%, and the excellent catalytic effect is shown in hydrogen fuel cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0005068086120000011
    Figure FDA0005068086120000011
  • Figure 977VDQRRDXKO3DKICCVTMOFUBN29HOYS7W2BNLWZ
    Figure 977VDQRRDXKO3DKICCVTMOFUBN29HOYS7W2BNLWZ
  • Figure N7ZDUPANLYAK7R7DU4UEO3EMA2ROQ5YXDGRTA5VQ
    Figure N7ZDUPANLYAK7R7DU4UEO3EMA2ROQ5YXDGRTA5VQ
Patent Text Reader

Abstract

The invention discloses a method for synthesizing a high oxygen permeability ionomer using benzoyl peroxide as an initiator, and its product, film and application. The synthesis method comprises the following steps: (1) purging a reactor with nitrogen, and introducing liquid nitrogen into the shell interlayer of the reactor to cool down; (2) dissolving a perfluorodimethyldioxole monomer and an oxyperfluoroolefin having a sulfonyl fluoride group in a composite solvent respectively to obtain a perfluorodimethyldioxole solution and an oxyperfluoroolefin having a sulfonyl fluoride group; dissolving an initiator in the composite solvent to obtain an initiator solution; (3) sequentially adding the perfluorodimethyldioxole solution and the oxyperfluoroolefin having a sulfonyl fluoride group into the reactor, and adding the initiator solution; (4) starting stirring, sealing the reactor, maintaining pressure and gradually increasing temperature; (5) cooling to room temperature, releasing pressure, filtering and taking out solidified material in the reactor, devolatilizing, washing and drying; and (6) hydrolyzing and hydrogenating to obtain a hydrogen-type ionomer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrogen fuel cells, and in particular to a method for synthesizing a high oxygen permeability ionomer using benzoyl peroxide as an initiator, and a product, a film and application thereof. Background Art

[0002] The most important part of a hydrogen fuel cell is the catalyst. The catalytic efficiency of the catalyst directly determines the power of the entire fuel cell; at the same time, the amount of platinum (Pt) in the catalyst also plays an important role in the cost of the entire fuel cell. In fact, the distribution of Pt in the fuel cell is uneven (8 / 9 of the Pt / C catalyst is distributed at the positive electrode of the fuel cell). This is because in a hydrogen fuel cell, the negative electrode undergoes the HOR reaction H2→2e-+2H (two electron transfer, fast kinetic process), and the positive electrode undergoes the ORR reaction O2+4e-+4H+→2H2O (four electron transfer, slow kinetic process). According to theoretical calculations comparing the two reaction kinetic processes, the positive electrode ORR reaction rate is 6 orders of magnitude lower than the negative electrode HOR reaction, so the reaction rate of the total reaction depends on the positive electrode. The chemical reaction rate is proportional to the amount of Pt catalyst used, so the amount of catalyst used at the positive electrode is about 8 times that of the negative electrode.

[0003] The catalyst Pt / C is adhered between the proton exchange membrane (PEM) and the gas diffusion layer (GDL) by a polymer binder. The polymer binder is called an ionomer. The surface of the catalyst Pt is wrapped by the ionomer, and oxygen must first permeate through the ionomer before it can contact the catalyst Pt, thereby initiating the ORR reaction. Therefore, the oxygen permeability of the ionomer has a significant effect on the catalytic effect of Pt. The higher the oxygen permeability of the ionomer, the better the catalytic effect of Pt. The currently commercially available ionomer is a Nafion-type perfluorosulfonic acid resin, and its oxygen permeability constant is 0.1-0.3cm 3 / m.24h.0.1MPa.

[0004] At present, perfluorosulfonic acid resin poly(PDD-co-PSVE) is a new type of ionomer used in hydrogen fuel cell cathode in recent years. It is a copolymer of perfluoro-2,2-dimethyl-1,3-dioxopentene (PDD) and perfluorosulfonylethoxypropyl vinyl ether (PSVE). The synthesis process of poly(PDD-co-PSVE) reported publicly at home and abroad is a free radical polymerization reaction system, and the initiator is perfluorodibenzoyl peroxide (PBPO). Its structure is:

[0005]

[0006] It can be seen that PBPO has 10 F atoms, while the monomers PDD and PSVE are both perfluorinated structures (also containing more F atoms). PBPO has good compatibility with the monomers, which is conducive to initiating monomer polymerization to generate poly(PDD-co-PSVE). However, PBPO is not easy to produce, expensive, and has no stable commercial supply source. In addition, the units reported publicly have not been able to publicly provide commercial samples of poly(PDD-co-PSVE). How to produce poly(PDD-co-PSVE) at low cost, high efficiency, stability and in large quantities is an urgent problem to be solved. In addition, the preparation method of perfluorosulfonic acid resin disclosed in Patent 1 (CN116284538A) uses perfluoro-2,2-dimethyl-1,3-dioxolane and sulfonyl fluoride vinyl ether as monomers, fluorocarbon solvents such as perfluorocyclohexane and 1,2-trifluoro-1,2,2 trichloroethane and chlorofluoroalkanes as solvents, and peroxides as initiators. Patent 2 (CN118085155A) discloses that 4,5-difluoro-2,2-bis(trifluoromethyl)-1,3-dioxole and at least one perfluorosulfonyl fluoride monomer are copolymerized by free radicals in the presence of an initiator to obtain a perfluorosulfonyl fluoride resin, wherein benzoyl peroxide is used as an initiator. However, Patents 1 and 2, which are representative of the prior art, do not consider the influence of solvent characteristics on the ionomer polymerization system of a certain initiator, and how to achieve low-cost initiators to replace high-cost perfluoro structure initiators and obtain stable high oxygen permeability ionomers is the focus of research and development in this industry. Summary of the invention

[0007] In view of the problems existing in the background technology, the purpose of the present invention is to provide a method for synthesizing a highly oxygen permeable ionomer (poly(PDD-co-PSVE)). Compared with the existing synthesis method, the present invention adopts a common free radical initiator on the market-benzoyl peroxide, and unexpectedly finds that a composite solvent composed of chloroform and other fluorinated solvents such as perfluorohexane or trifluorotrichloroethane can greatly improve the free radical initiation efficiency of benzoyl peroxide in the synthesis process of poly(PDD-co-PSVE), successfully achieving high-efficiency synthesis of poly(PDD-co-PSVE), and the comprehensive properties of poly(PDD-co-PSVE) such as molecular weight, proton conductivity and oxygen permeability are improved, and the strength is also significantly improved, and no rupture occurs during use. The present invention solves the problem of commercial production of poly(PDD-co-PSVE) and has the advantages of high efficiency, low cost and stable production.

[0008] In order to achieve the above object, the present invention provides a method for synthesizing a high oxygen permeability ionomer using benzoyl peroxide as an initiator, wherein the polymerization monomer of the high oxygen permeability ionomer comprises a perfluorodimethyldioxole monomer and an oxoperfluoroolefin having a sulfonyl fluoride group; the initiator is benzoyl peroxide; the polymerization monomer and the initiator are respectively dissolved in a composite solvent, the composite solvent is a combination of chloroform and a fluorine-containing solvent, the mass ratio of the chloroform to the fluorine-containing solvent is 1:2-4, the fluorine-containing solvent is perfluorohexane or trifluorotrichloroethane; the structural formula of the perfluorodimethyldioxole monomer is:

[0009] ;

[0010] The oxyperfluoroolefin having a sulfonyl fluoride group is perfluorosulfonyl ethoxypropyl vinyl ether, and the structural formula is: CF2═CFOCF2CF(CF3)OCF2CF2SO2F.

[0011] Optionally, the mass ratio of the perfluorodimethyldioxole monomer, the oxoperfluoroolefin having a sulfonyl fluoride group and benzoyl peroxide is: 8-15:40-60:1.5-3.

[0012] Optionally, the ratio of perfluorodimethyldioxole monomer to the composite solvent is 100 g:1 mL; the ratio of oxyperfluoroolefin having sulfonyl fluoride group to the composite solvent is 100 g:1 mL; the ratio of benzoyl peroxide to the composite solvent is 50-60 g:1 mL.

[0013] Optionally, the method for synthesizing a highly oxygen permeable ionomer using benzoyl peroxide as an initiator comprises the following steps: (1) purging a reactor with nitrogen for 3-5 times, introducing liquid nitrogen into the shell interlayer of the reactor to cool the reactor, and maintaining the temperature of the reactor below -20°C; (2) dissolving a perfluorodimethyldioxole monomer and an oxyperfluoroolefin having a sulfonyl fluoride group in a composite solvent to obtain a perfluorodimethyldioxole solution and an oxyperfluoroolefin having a sulfonyl fluoride group; dissolving an initiator in the composite solvent to obtain an initiator solution; (3) sequentially adding perfluorodimethyldioxole to the reactor; Prepare a solution of 1,2-dioxolane and a solution of 1,2-dioxolane having a sulfonyl fluoride group, add the initiator solution while the stirring paddle is kept stirring, stop stirring, evacuate and pass nitrogen, and repeat the operation 2-3 times; (4) start stirring, seal the reactor, maintain the pressure and gradually increase the temperature at a rate of 2-4°C / min to 40-50°C, and maintain the reaction for 12-24h; continue to maintain the pressure and heat to 90-100°C and maintain for 5-8h; (5) cool to room temperature, release the pressure, filter out the solidified material in the reactor, devolatilize, wash and dry; (6) hydrolyze and hydrogenate to obtain a hydrogen-type high oxygen permeability ionomer.

[0014] The present invention also provides a high oxygen permeability ionomer prepared by the synthesis method as described above, wherein the number average molecular weight Mn of the ionomer is greater than 180,000; and wherein the ionomer has a proton conductivity greater than 106 mS / cm at 80°C and 95% relative humidity, and has a proton conductivity greater than 50×10 -9 SCCcm / cm 2 Oxygen permeability in scmHg.

[0015] The present invention also provides a film made from the above-mentioned high oxygen permeability ionomer, wherein the tensile strength of the film is greater than 50 MPa.

[0016] The present invention also provides a use of the high oxygen permeability ionomer as described above, which is applied to a Pt / C catalyst layer of a hydrogen fuel cell.

[0017] The beneficial effects of the present invention are as follows:

[0018] 1. For the first time, benzoyl peroxide was successfully used to replace perfluorobenzoyl peroxide as an initiator for the synthesis of poly(PDD-co-PSVE), with a yield of about 90% and stable productivity.

[0019] 2. The composite solvent composed of chloroform and perfluorohexane or trifluorotrichloroethane can significantly improve the initiation efficiency of benzoyl peroxide in the synthesis process, indicating that chloroform has a significant solubilizing effect on benzoyl peroxide in solvents such as perfluorohexane or trifluorotrichloroethane; although chloroform and perfluorohexane or trifluorotrichloroethane have similar structures, the use of similar monofluorodichloroethane to replace chloroform cannot increase the yield of poly(PDD-co-PSVE), indicating that the polarization property of chloroform significantly improves the compatibility and dispersibility of the free radical monomer after the decomposition of benzoyl peroxide in the synthesis system, and gives full play to its initiation polymerization effect on perfluorodimethyldioxole monomer (PDD) and oxygen-containing perfluoroolefin (PSVE) with sulfonyl fluoride. In the same research process, acetone with good general solubility was used as a solvent, but poly(PDD-co-PSVE) could not be obtained. Analysis shows that the active hydrogen of acetone affects the polymerization reaction, indicating that the solvent should not only consider solubility in the polymerization reaction, but also pay attention to its chemical and polarization properties. The composite solvent composed of chloroform and perfluorohexane or trifluorotrichloroethane of the present invention has better dissolving and synthesis promoting effects.

[0020] 3. The synthesis method of the present invention has cheap raw material sources, a stable production process, a high product performance qualification rate, and can be mass-produced. DETAILED DESCRIPTION

[0021] In order to make the above-mentioned objects, features and advantages of the invention more obvious and easy to understand, the specific embodiments of the invention are described in detail below.

[0022] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0023] In the method for synthesizing a highly oxygen permeable ionomer using benzoyl peroxide as an initiator according to the present invention, the polymerized monomers of the highly oxygen permeable ionomer include a perfluorodimethyldioxole monomer and an oxoperfluoroolefin having a sulfonyl fluoride group; the initiator is benzoyl peroxide; the polymerized monomer and the initiator are respectively dissolved in a composite solvent, the composite solvent is a combination of chloroform and a fluorine-containing solvent, the mass ratio of the chloroform to the fluorine-containing solvent is 1:2-4, the fluorine-containing solvent is perfluorohexane or trifluorotrichloroethane; the structural formula of the perfluorodimethyldioxole monomer is:

[0024] ;

[0025] The oxyperfluoroolefin having a sulfonyl fluoride group is perfluorosulfonyl ethoxypropyl vinyl ether, and the structural formula is: CF2═CFOCF2CF(CF3)OCF2CF2SO2F.

[0026] In the method for synthesizing a highly oxygen permeable ionomer using benzoyl peroxide as an initiator according to the present invention, the mass ratio of the perfluorodimethyldioxole monomer, the oxyperfluoroolefin having a sulfonyl fluoride group and benzoyl peroxide can be: 8-15:40-60:1.5-3.

[0027] In the method for synthesizing a highly oxygen permeable ionomer using benzoyl peroxide as an initiator according to the present invention, the ratio of the perfluorodimethyldioxole monomer to the composite solvent may be 100 g:1 mL; the ratio of the oxyperfluoroolefin having a sulfonyl fluoride group to the composite solvent may be 100 g:1 mL; and the ratio of benzoyl peroxide to the composite solvent may be 50-60 g:1 mL.

[0028] In the method for synthesizing a highly oxygen permeable ionomer using benzoyl peroxide as an initiator according to the present invention, the method for synthesizing a highly oxygen permeable ionomer using benzoyl peroxide as an initiator may include the following steps: (1) purging a reactor with nitrogen for 3-5 times, introducing liquid nitrogen into the shell interlayer of the reactor to cool the reactor, and maintaining the temperature of the reactor below -20°C; (2) dissolving a perfluorodimethyldioxole monomer and an oxyperfluoroolefin having a sulfonyl fluoride group in a composite solvent, respectively, to obtain a perfluorodimethyldioxole solution and an oxyperfluoroolefin having a sulfonyl fluoride group; and dissolving an initiator in the composite solvent to obtain an initiator solution; (3) Add perfluorodimethyldioxole solution and sulfonyl fluoride-containing perfluoroolefin solution to the reaction kettle in sequence, add the initiator solution while the stirring paddle is kept stirring, stop stirring, evacuate and pass nitrogen, and repeat the operation 2-3 times; (4) start stirring, seal the reaction kettle, maintain pressure and gradually increase the temperature at a rate of 2-4°C / min to 40-50°C, and maintain the reaction for 12-24h; continue to maintain pressure and heat to 90-100°C and maintain for 5-8h; (5) cool to room temperature, release pressure, filter out the solidified material in the reaction kettle, devolatilize, wash and dry; (6) hydrolyze and hydrogenate to obtain a hydrogen-type high oxygen permeability ionomer.

[0029] In the high oxygen permeability ionomer prepared according to the synthesis method of the present invention, the number average molecular weight Mn of the ionomer is greater than 180,000; and wherein the ionomer has a proton conductivity greater than 106 mS / cm at 80°C and 95% relative humidity, and has a proton conductivity greater than 50×10 -9 SCCcm / cm 2 Oxygen permeability in scmHg.

[0030] The tensile strength of the film prepared from the high oxygen permeability ionomer according to the present invention is greater than 50 MPa.

[0031] The high oxygen permeability ionomer according to the present invention can be applied to the Pt / C catalyst layer of a hydrogen fuel cell.

[0032] The following examples specifically illustrate the synthesis method of the high oxygen permeability ionomer using benzoyl peroxide as an initiator, its products, films and applications. Main raw materials and equipment used: Unless otherwise specified, the raw materials and equipment of each embodiment and comparative example are the same; materials without specific models or types are from the same common models purchased on the market, and are not specifically limited.

[0033] Example 1

[0034] (1) The reactor was purged with nitrogen three times, and liquid nitrogen was introduced into the outer shell of the reactor to cool it down and maintain the temperature of the reactor below -20°C.

[0035] (2) Preparation of composite solvent: The mass ratio of chloroform to trichlorotrifluoroethane is 1:2.

[0036] (3) Perfluorodimethyldioxole monomer (PDD) and perfluorosulfonylethoxypropyl vinyl ether (PSVE) are dissolved in a composite solvent to obtain a PDD solution and a PSVE solution, respectively; the initiator benzoyl peroxide is dissolved in the composite solvent to obtain an initiator solution; the ratio of PDD to the composite solvent in the PDD solution is 100 g:1 mL; the ratio of PSVE to the composite solvent in the PSVE solution is 100 g:1 mL; the ratio of benzoyl peroxide to the composite solvent in the initiator solution is 50 g:1 mL; the mass ratio of PDD, PSVE and benzoyl peroxide is 8:40:1.5.

[0037] (4) Add PDD solution and PSVE solution to the reactor in sequence. While the stirring paddle is still stirring, add the initiator solution. Stop stirring and repeat the vacuum and nitrogen flow operation twice.

[0038] (5) Start stirring, seal the reactor, maintain pressure and gradually increase the temperature at a rate of 2°C / min to 40°C, and maintain the reaction for 12 h; continue to maintain pressure and heat to 90°C and maintain for 5 h.

[0039] (6) Cool down to room temperature, release the pressure, filter out the solidified material in the reactor, devolatilize, wash and dry.

[0040] (7) Hydrolysis with 20 wt% KOH aqueous solution and hydrogenation with 20 wt% hydrochloric acid solution to obtain a hydrogen-type high oxygen permeability ionomer.

[0041] Example 2

[0042] (1) The reactor was purged with nitrogen for 5 times, and liquid nitrogen was introduced into the outer shell interlayer of the reactor to cool it down and maintain the temperature of the reactor below -20°C.

[0043] (2) Preparation of composite solvent: The mass ratio of chloroform to perfluorohexane is 1:4.

[0044] (3) Perfluorodimethyldioxole monomer (PDD) and perfluorosulfonylethoxypropyl vinyl ether (PSVE) are dissolved in a composite solvent to obtain a PDD solution and a PSVE solution, respectively; an initiator benzoyl peroxide is dissolved in the composite solvent to obtain an initiator solution; the ratio of PDD to the composite solvent in the PDD solution is 100 g:1 mL; the ratio of PSVE to the composite solvent in the PSVE solution is 100 g:1 mL; the ratio of benzoyl peroxide to the composite solvent in the initiator solution is 60 g:1 mL; and the mass ratio of PDD, PSVE and benzoyl peroxide is 15:60:3.

[0045] (4) Add PDD solution and PSVE solution to the reactor in sequence. While the stirring paddle is still stirring, add the initiator solution. Stop stirring and repeat the vacuum and nitrogen gas flow operation three times.

[0046] (5) Start stirring, seal the reactor, maintain pressure and gradually increase the temperature at a rate of 4°C / min to 50°C, and maintain the reaction for 24 hours; continue to maintain pressure and heat to 100°C and maintain for 8 hours.

[0047] (6) Cool down to room temperature, release the pressure, filter out the solidified material in the reactor, devolatilize, wash and dry.

[0048] (7) Hydrolysis with 20 wt% KOH aqueous solution and hydrogenation with 20 wt% hydrochloric acid solution to obtain a hydrogen-type high oxygen permeability ionomer.

[0049] Example 3

[0050] (1) The reactor was purged with nitrogen 4 times, and liquid nitrogen was introduced into the outer shell interlayer of the reactor to cool it down and maintain the temperature of the reactor below -20°C.

[0051] (2) Preparation of composite solvent: The mass ratio of chloroform to perfluorohexane is 1:3.

[0052] (3) Perfluorodimethyldioxole monomer (PDD) and perfluorosulfonylethoxypropyl vinyl ether (PSVE) were dissolved in a composite solvent to obtain a PDD solution and a PSVE solution, respectively; the initiator benzoyl peroxide was dissolved in the composite solvent to obtain an initiator solution; the ratio of PDD to the composite solvent in the PDD solution was 100 g:1 mL; the ratio of PSVE to the composite solvent in the PSVE solution was 100 g:1 mL; the ratio of benzoyl peroxide to the composite solvent in the initiator solution was 55 g:1 mL; the mass ratio of PDD, PSVE and benzoyl peroxide was 12:50:2.5.

[0053] (4) Add PDD solution and PSVE solution to the reactor in sequence. While the stirring paddle is still stirring, add the initiator solution. Stop stirring and repeat the vacuum and nitrogen gas flow operation three times.

[0054] (5) Start stirring, seal the reactor, maintain pressure and gradually increase the temperature at a rate of 3°C / min to 45°C, and maintain the reaction for 12-24 hours; continue to maintain pressure and heat to 95°C for 7 hours.

[0055] (6) Cool down to room temperature, release the pressure, filter out the solidified material in the reactor, devolatilize, wash and dry.

[0056] (7) Hydrolysis with 20 wt% KOH aqueous solution and hydrogenation with 20 wt% hydrochloric acid solution to obtain a hydrogen-type high oxygen permeability ionomer.

[0057] Comparative Example 1

[0058] Except that monofluorodichloroethane was used instead of chloroform, the other steps were the same as those in Example 3.

[0059] Comparative Example 2

[0060] Except that acetone was used instead of chloroform, the other conditions were the same as in Example 3, but no ionomer could be obtained.

[0061] Performance Testing

[0062] 1. The yield (ratio of product to raw material), exchange equivalent EW value (GB / T20042.3-2022) and number average molecular weight of the hydrogen-type ionomers of the examples and comparative examples were tested respectively.

[0063] 2. At 23°C and 0% relative humidity, the oxygen permeability of the catalyst layer after peeling off from the surface of the base membrane PET was tested using an instrument (MoconOX-Tran®, Minneapolis, MN, USA); at 80°C and 95% relative humidity, the catalyst layer was loaded into the electrolyte membrane of the electrochemical cell, the test electrodes were connected to both sides of the electrolyte membrane, an external voltage was applied, and the proton conductivity was calculated.

[0064] 3. After the hydrogen-type ionomer is dissolved in the solvent, it is cast into a film with a thickness of 0.5 mm; the mechanical strength of the hydrogen-type ionomer film is tested using a universal material testing machine (GB / T20042.3-2022).

[0065] See Table 1 for specific data.

[0066] Table 1

[0067]

[0068] It can be seen from the data of the embodiments and comparative examples that the present invention utilizes chloroform and a composite solvent with perfluorohexane or trifluorotrichloroethane to improve the free radical initiation efficiency of benzoyl peroxide in the synthesis process of poly(PDD-co-PSVE), with high yield, and can obtain a hydrogen-type ionomer film with excellent performance.

[0069] The above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.

Claims

1. A method for synthesizing a highly oxygen permeable ionomer using benzoyl peroxide as an initiator, It is characterized in that The polymerized monomers of the high oxygen permeability ionomer include perfluorodimethyldioxole monomers and oxoperfluoroolefins having sulfonyl fluoride groups; the initiator is benzoyl peroxide; the polymerized monomers and the initiator are dissolved in a composite solvent, the composite solvent is a combination of chloroform and a fluorine-containing solvent, the mass ratio of chloroform to the fluorine-containing solvent is 1:2-4, and the fluorine-containing solvent is perfluorohexane or trifluorotrichloroethane; The structural formula of the perfluorodimethyldioxole monomer is: The oxoperfluoroolefin having a sulfonyl fluoride group is perfluorosulfonylethoxypropyl vinyl ether, and the structural formula is: CF 2 ═CFOCF 2 CF(CF 3 )OCF 2 CF 2 SO 2 F.

2. The method for synthesizing a highly oxygen permeable ionomer using benzoyl peroxide as an initiator as claimed in claim 1, It is characterized in that The mass ratio of the perfluorodimethyldioxole monomer, the oxoperfluoroolefin having a sulfonyl fluoride group and benzoyl peroxide is: 8-15:40-60:1.5-3.

3. The method for synthesizing a high oxygen permeability ionomer using benzoyl peroxide as an initiator as claimed in claim 1, It is characterized in that The ratio of perfluorodimethyldioxole monomer to the composite solvent is 100 g:1 mL; the ratio of oxyperfluoroolefin having sulfonyl fluoride group to the composite solvent is 100 g:1 mL; the ratio of benzoyl peroxide to the composite solvent is 50-60 g:1 mL.

4. The method for synthesizing a highly oxygen permeable ionomer using benzoyl peroxide as an initiator according to any one of claims 1 to 3, It is characterized in that The following steps are involved: (1) purging a reactor with nitrogen for 3-5 times, introducing liquid nitrogen into the outer shell interlayer of the reactor to cool down, and maintaining the temperature of the reactor below -20°C; (2) dissolving a perfluorodimethyldioxole monomer and an oxyperfluoroolefin having a sulfonyl fluoride group in a composite solvent to obtain a perfluorodimethyldioxole solution and an oxyperfluoroolefin having a sulfonyl fluoride group; dissolving an initiator in the composite solvent to obtain an initiator solution; (3) sequentially adding the perfluorodimethyldioxole solution and the oxyperfluoroolefin having a sulfonyl fluoride group into the reactor; The perfluoroolefin solution is added with an initiator solution while the stirring blade is kept stirring. The stirring is stopped and the vacuum and nitrogen are introduced, and the operation is repeated 2-3 times; (4) stirring is started, the reaction kettle is sealed, the pressure is maintained and the temperature is gradually increased at a rate of 2-4°C / min to 40-50°C, and the reaction is maintained for 12-24 hours; the pressure is continued to be maintained and heated to 90-100°C for 5-8 hours; (5) the temperature is lowered to room temperature, the pressure is released, the solidified material in the reaction kettle is filtered out, the volatilization is carried out, and the solidified material is washed and dried; (6) hydrolyzed and hydrogenated to obtain a hydrogen-type high oxygen permeability ionomer.