Highly hygroscopic chemical fiber and preparation method thereof

Through modified copolymer slices and surface modification treatment, combined with adsorption and irradiation treatment of tea polyphenols and crosslinking agents, highly absorbent chemical fibers were prepared, which solved the shortcomings of polyester fibers in terms of hygroscopicity and versatility. It achieves efficient antibacterial and odor removal and ultraviolet protection effects.

CN118685984BActive Publication Date: 2024-11-15WEIFANG WEINI NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411172761.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-15
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Existing polyester fibers have shortcomings in hygroscopicity and versatility, and it is difficult to have both high hygroscopicity, antibacteriality, anti-odor, anti-odor and anti-ultraviolet properties.

Method used

Through the preparation of modified copolymer slices, highly absorbent chemical fibers were prepared by special-shaped spinneret hole spinning, alkali reduction treatment and surface modification treatment, combined with adsorption and irradiation treatment of tea polyphenols and crosslinking agents, and enhanced the Hygroscopicity and functionality of fibers.

Benefits of technology

It has achieved multifunctional properties such as high hygroscopicity, antibacterial and odor removal, and ultraviolet ray protection, and improved the softness and structural stability of the fiber. It has E. coli inhibition rate >90%, Candida albican inhibition rate >88%, and ammonia The reduction rate is >87%, the moisture retraction rate is >10%, and the ultraviolet transmittance is <5%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 89RLHHEZGS0FLPLFZOMUNETDD32NA6QBCEZ6BXZO
    Figure 89RLHHEZGS0FLPLFZOMUNETDD32NA6QBCEZ6BXZO
Patent Text Reader

Abstract

The present invention belongs to the technical field of chemical fibers, and specifically relates to highly hygroscopic chemical fibers and a preparation method thereof. The preparation method of the highly hygroscopic chemical fibers uses terephthalic acid and ethylene glycol as main raw materials, polyamide salt and polyethylene glycol as modifiers, prepares modified copolymer slices and spins them to obtain modified copolymer short fibers; then performs alkali reduction treatment in an aqueous solution of sodium hydroxide and ethylene glycol, and then performs adsorption treatment in a highly hygroscopic substance solution and an aqueous solution containing tea polyphenols and a cross-linking agent in turn, and performs irradiation treatment in an aqueous solution of zinc acetate or silver acetate to obtain highly hygroscopic chemical fibers. The highly hygroscopic chemical fibers prepared by the present invention have both high hygroscopicity and multifunctional properties of antibacterial, deodorizing, and UV protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical fibers, and in particular relates to highly hygroscopic chemical fibers and a preparation method thereof. Background Art

[0002] Polyester fiber is a chemical fiber made from synthetic polymer compounds. It has the advantages of high strength, light weight, easy to wash and dry, good elasticity, and no fear of mold and mildew. However, it also has the disadvantages of poor hygroscopicity and water absorption compared to natural fibers, and poor wearing comfort. In order to improve the hygroscopicity of polyester fiber, the prior art either adopts blending modification, copolymerization modification, or blending and spinning with functional substances to give chemical fibers high hygroscopicity and additional functionality.

[0003] For example, patent CN103710782A discloses a highly hygroscopic and easy-to-dye cotton-like polyester staple fiber and its preparation method, wherein the fiber comprises the following raw materials in mass percentage: 38-69% purified terephthalic acid, 21-36% ethylene glycol, 3-10% 2,2-dihydroxymethyl propionic acid, 4-7% polyethylene glycol, 2.7-7% sodium diethylene glycol 5-sulfonate isophthalate, and 0.3-2.5% titanium dioxide; the above raw materials are subjected to esterification polycondensation reaction to obtain highly hygroscopic and easy-to-dye polyester slices, and the surface and cross-sectional morphology, crystallization, and orientation structure of the fiber are regulated through spinning and post-treatment processes to obtain highly hygroscopic and easy-to-dye cotton-like polyester fibers. The invention simultaneously modifies the hydrophilicity and easy-to-dye properties of polyester fibers, so that the reactive groups have great randomness in the reaction process, and titanium dioxide is also added. Titanium dioxide is added to the fiber material by physical mixing, and is easy to migrate during the later use of the fiber, and is also easy to cause photodegradation of the fiber.

[0004] Patent CN112410923A discloses a method for preparing antibacterial moisture-absorbing and heat-insulating polyester fiber, wherein polyester powder and micro-nano calcium carbonate are vacuum pre-crystallized and dried; then, they are mixed by twin screws, cooled and pelletized to obtain a moisture-absorbing polyester fiber masterbatch; after the moisture-absorbing polyester fiber masterbatch, antibacterial polyester fiber masterbatch and polyester slices are evenly mixed, they are spun through a C-type hollow spinneret to obtain primary fibers; the primary fibers are then drafted, heat-set, washed, dried and wound to obtain polyester long fibers; finally, the polyester long fibers and low-melting-point polyester staple fibers are thermally bonded; the antibacterial moisture-absorbing and heat-insulating polyester fiber of the invention uses micro-nano calcium carbonate to modify the polyester fiber and uses a C-type hollow spinneret to spin, and the moisture absorption effect is significantly improved. The invention improves the hygroscopicity of polyester fibers by adding micro-nano calcium carbonate to polyester powder, but the degree of improvement in the hygroscopicity of polyester fibers is limited.

[0005] Qi Xiaojie et al. prepared ultra-soft and highly hygroscopic modified polyethylene terephthalate fibers. This technology used pentamethylenediamine adipate (PA56 salt) and its derivative adipic acid glutaramide (APA56 salt) as modified monomers, copolymerized with ethylene terephthalate (PET) and melt-spun. Compared with PET fibers, the moisture regains of PA56 salt and APA56 salt modified PET fibers were increased by 39~200% and 53~213%, respectively (Qi Xiaojie et al., Preparation and Properties of Ultra-Soft and Highly Hygroscopic Modified Polyethylene Terephthalate Fibers, Journal of Textile Research, 2023, Vol. 44, No. 9). However, this study only improved the hygroscopicity of PET fibers to a limited extent through the introduction of pentamethylenediamine adipate and adipic acid glutaramide, and the modified polyester fibers were not multifunctional.

[0006] Zhao Mancai prepared fibers by adding acid-soluble nano inorganic particles to PET slices, and then used acid to dissolve the inorganic particles in the prepared fibers to obtain microcavity high hygroscopic PET fibers. The fiber can significantly improve its hygroscopicity after acid treatment, and the hygroscopicity rate increased from 0.4% to 1.382% (Zhao Mancai, Preparation and Hygroscopicity Study of Microcavity High Hygroscopic PET Fiber, Synthesis Technology and Application, March 2011, Vol. 26, No. 1). This study used acid to react the acid-soluble nano inorganic particles in the fiber. Since the fiber is a solid structure, it is difficult for the nano inorganic particles inside the fiber to react completely, thus affecting the effect of improving hygroscopicity. Summary of the invention

[0007] In view of the problems existing in the prior art, the purpose of the present invention is to provide a highly hygroscopic chemical fiber, which modifies polyester fiber so that it has both high hygroscopicity and multifunctional properties such as antibacterial, deodorizing and UV protection; the present invention also provides a preparation method thereof, which is feasible and convenient for mass production.

[0008] The method for preparing the highly hygroscopic chemical fiber of the present invention comprises the following steps:

[0009] (1) Preparation of modified copolymer chips:

[0010] Using terephthalic acid and ethylene glycol as main raw materials, polyamide salt and polyethylene glycol as modifiers, and carrying out polycondensation reaction under the action of a catalyst, a modified copolymer slice is obtained;

[0011] (2) Preparation of modified copolymer staple fibers:

[0012] The modified copolymer slices are spun through a spinneret provided with special-shaped spinneret holes, and cut to obtain modified copolymer short fibers;

[0013] (3) Alkali reduction treatment:

[0014] The modified copolymer staple fibers are immersed in an aqueous solution of sodium hydroxide and ethylene glycol for alkali reduction treatment, and after the treatment is completed, they are neutralized, washed with water, and dried in sequence to obtain alkali-etched modified copolymer staple fibers;

[0015] (4) Surface modification:

[0016] The modified copolymer staple fibers etched with alkali are immersed in a highly water-absorbent solution for a first adsorption treatment, then immersed in an aqueous solution containing tea polyphenols and a cross-linking agent for a second adsorption treatment, then immersed in an aqueous solution of zinc acetate or silver acetate for irradiation treatment, and finally softened, oiled, and dried to obtain highly hygroscopic chemical fibers;

[0017] The highly absorbent material solution is a solution obtained by dissolving protein and / or cellulose in NMMO solution or ionic liquid; and the cross-linking agent is at least one of acrylic acid, acrylonitrile, ethyl acrylate and acrylamide.

[0018] In step (1), the mass ratio of terephthalic acid (PTA) to ethylene glycol (EG) is 1:1.2-1.4.

[0019] In step (1), the polyamide salt is at least one of pentamethylenediamine adipate (PA56 salt), caprolactam salt (PA6), and hexamethylenediamine adipate (PA66); and the amount of the polyamide salt added is 8-12% of the mass of terephthalic acid.

[0020] In step (1), the polyethylene glycol is at least one of PEG-200, PEG-300, PEG-400, and PEG-600; and the amount of polyethylene glycol added is 6-8% of the mass of terephthalic acid.

[0021] When preparing the modified copolymer slice, the present invention simultaneously introduces polyamide salt and polyethylene glycol as modifiers, and the hygroscopicity of the copolymer can be better improved by introducing different hydrophilic groups, and the introduction of polyethylene glycol can enhance the softness of the fiber.

[0022] In step (1), the catalyst is at least one of ethylene glycol antimony, antimony trioxide, and antimony trioxide; and the amount of the catalyst added is 0.021-0.032% of the mass of terephthalic acid.

[0023] In step (1), the polycondensation reaction process is:

[0024] After mixing terephthalic acid and ethylene glycol, add a catalyst, heat up to 215-220°C, start stirring, continue to heat up to 235-250°C, add polyamide salt and polyethylene glycol, evacuate to 0.0098-0.05Pa, carry out a pre-polycondensation reaction at 235-250°C for 50-70min, continue to heat up to 260-270°C for a polycondensation reaction for 150-180min, and after the polycondensation reaction is completed, granulate and dry to obtain a modified copolymer slice with a characteristic viscosity of 0.65-0.71dL / g.

[0025] Preferably, during drying, vacuum drying is first performed at 85-105° C. for 50-70 min to allow the slices to be pre-crystallized, and then vacuum drying is continued at 120-135° C. until the moisture content is less than 100 ppm.

[0026] In step (2), a twin-screw extruder is used for spinning. The temperature of the twin-screw extruder is divided into three zones. The temperature of zone one is 260-270°C, the temperature of zone two is 270-275°C, the temperature of zone three is 275-280°C, the temperature of the metering pump is 280-285°C, and the temperature of the pipeline and the box is 280-290°C.

[0027] In step (2), the spinning speed is 1000-1200 m / min, and the drafting multiple is 1.8-3.2 times.

[0028] In step (2), the special-shaped spinneret hole is preferably one of a flat spinneret hole, a cross-shaped spinneret hole, and a Y-shaped spinneret hole, but is not limited to the above shapes. The special-shaped spinneret hole can increase the surface area of ​​the fiber.

[0029] In step (3), in the aqueous solution of sodium hydroxide and ethylene glycol, the concentration of sodium hydroxide is 2.2-3.5wt.%, and the concentration of ethylene glycol is 20-30wt.%. The present invention adopts the aqueous solution of sodium hydroxide and ethylene glycol for alkali reduction treatment, wherein ethylene glycol is one of the main raw materials of the modified copolymer, which can make sodium hydroxide penetrate better, thereby improving the alkali reduction rate.

[0030] In step (3), the alkali reduction treatment conditions are: temperature 60-80°C, treatment bath ratio 1:20-30, and time 30-45 min.

[0031] In step (3), during neutralization, acetic acid having a concentration of 0.5 to 1.2 wt.% is preferably used for neutralization.

[0032] In step (3), the alkali reduction rate of the modified copolymer staple fibers etched by alkali is 12.21-16.18%. Through the alkali reduction treatment, the surface of the modified copolymer staple fibers is alkali-etched, and pits are formed on the surface, which facilitates the subsequent surface modification.

[0033] In step (4), the concentration of the highly hygroscopic substance in the highly hygroscopic substance solution is 5.5-8.0 wt.%. The highly hygroscopic substance is added to the NMMO solution or the ionic liquid and dissolved by a thin film evaporator to obtain a highly hygroscopic substance solution.

[0034] Preferably, the ionic liquid is an alkyl imidazole type ionic liquid, wherein the cation is one of allyl, ethyl and butyl; and the anion is one of Cl-, SCN- and CH3COO-.

[0035] In step (4), the first adsorption treatment temperature is 80-85°C, and the treatment time is 45-60 minutes.

[0036] In step (4), the aqueous solution containing tea polyphenols and a cross-linking agent has a tea polyphenol concentration of 15-20 wt.%, a cross-linking agent concentration of 16-20 wt.%, and a pH value of 5.5-6.8 adjusted with acetic acid or lactic acid.

[0037] In step (4), the second adsorption treatment temperature is 50-60°C, and the treatment time is 40-60 minutes.

[0038] The second adsorption treatment is carried out in an aqueous solution containing tea polyphenols and a cross-linking agent, which can make the adsorbed highly absorbent material form and precipitate on the surface of the modified copolymer staple fiber. At the same time, the highly absorbent material can further adsorb tea polyphenols and the cross-linking agent during the precipitation process, which is convenient for subsequent complexation and cross-linking.

[0039] Tea polyphenols are a mixture of polyphenols, which have excellent antioxidant, antibacterial, and UV protection properties, and have good absorption in the ultraviolet region of 290 to 320 nm, and can directly absorb ultraviolet rays to prevent ultraviolet rays from damaging the skin. The present invention allows tea polyphenols to exist stably by absorbing, complexing, and cross-linking tea polyphenols, thereby giving the fiber good UV protection.

[0040] In step (4), the concentration of zinc acetate or silver acetate in the aqueous solution of zinc acetate or silver acetate is 10-15 wt.%.

[0041] In step (4), the irradiation treatment conditions are: room temperature, air atmosphere, and an absorbed dose of 80-100 kGy. During the irradiation treatment, on the one hand, tea polyphenols and zinc acetate or silver acetate are complexed, which can give the chemical fiber stable antibacterial, deodorizing and UV protection functions; on the other hand, the irradiation treatment can cause cross-linking between the cross-linking agents and between the cross-linking agents and highly absorbent substances, thereby enhancing the stability of the fiber structure.

[0042] The highly hygroscopic chemical fiber prepared by the present invention has an Escherichia coli inhibition rate of more than 90% (GB / T20944.3-2008), a Candida albicans inhibition rate of more than 88% (GB / T20944.3-2008), an ammonia reduction rate of more than 87% (GB / T33610.2-2017), a moisture regain rate of more than 10% (GB / T6503-2008), and an ultraviolet transmittance of less than 5% (GB / T 18830-2009).

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] (1) The present invention uses hydrophilic monomers to modify the copolymer system during the copolymerization process to improve the water absorption of the copolymer fiber body; at the same time, flat, cross-shaped and other special-shaped spinnerets are used during the spinning process to increase the surface area of ​​the fiber, further improving the hygroscopicity of the fiber;

[0045] (2) The present invention firstly performs an alkali reduction treatment on the modified copolymer staple fibers to increase the fiber surface area, and then uses a highly water-absorbent substance solution to treat the alkali-etched modified copolymer staple fibers, thereby forming and precipitating the highly water-absorbent substance. Since the hydrophilic substance contains a large number of hydrophilic groups such as hydroxyl groups and amino groups, its water absorption is much higher than that of copolymers of the same mass, thereby improving the hygroscopicity of the fiber;

[0046] (3) The cross-linking agent used in the surface modification treatment of the present invention contains a large number of hydrophilic groups, which can not only improve the hydrophilicity of the fiber, but also serve as a group for later cross-linking. By irradiation, cross-linking occurs between the cross-linking agents and between the cross-linking agent and the water-absorbing substance, thereby enhancing the stability of the fiber structure.

[0047] (4) The present invention adopts an adsorption process, with tea polyphenols, zinc acetate or silver acetate as functional components, and is supplemented with modification treatments such as crosslinking agent treatment and irradiation. Through the complexation between tea polyphenols and zinc acetate or silver acetate, the fiber is endowed with good antibacterial and deodorizing functionality;

[0048] (5) The chemical fiber prepared by the present invention not only has high hygroscopicity, but also has multifunctional properties such as antibacterial, deodorizing, and UV protection. Its Escherichia coli inhibition rate is greater than 90%, Candida albicans inhibition rate is greater than 88%, ammonia reduction rate is greater than 87%, regain rate is greater than 10%, and UV transmittance is less than 5%. In addition, the fabric prepared by the chemical fiber has good softness. DETAILED DESCRIPTION

[0049] The present invention is further described below in conjunction with the examples. The raw materials used in the examples, unless otherwise specified, are all commercially available conventional raw materials; the process methods used in the examples, unless otherwise specified, are all conventional methods in the art. The examples of the present invention do not limit the level of the amount of each raw material, and any weight level can be used for preparation, as long as the specific raw material ratio is followed.

[0050] Example 1

[0051] The highly hygroscopic chemical fiber is prepared as follows:

[0052] (1) Preparation of modified copolymer chips:

[0053] After mixing terephthalic acid and ethylene glycol in a mass ratio of 1:1.2, add ethylene glycol antimony accounting for 0.032% of the mass of terephthalic acid, heat to 215°C, start stirring, continue to heat to 235°C, add pentamethylenediamine adipate accounting for 8% of the mass of terephthalic acid and PEG-200 accounting for 6% of the mass of terephthalic acid, evacuate to 0.0098Pa, carry out pre-polycondensation reaction at 235°C for 50min, continue to heat to 260°C for polycondensation reaction for 180min, after the polycondensation reaction is completed, granulate to obtain slices, first vacuum dry at 85°C for 50min to pre-crystallize the slices, and then continue to vacuum dry at 120°C until the water content is less than 100ppm, to obtain modified copolymer slices with an intrinsic viscosity of 0.65dL / g;

[0054] (2) Preparation of modified copolymer staple fibers:

[0055] The modified copolymer slices were spun by a twin-screw extruder. The temperature of the twin-screw extruder was divided into three zones: the temperature of zone 1 was 260°C, the temperature of zone 2 was 270°C, the temperature of zone 3 was 275°C, the temperature of the metering pump was 285°C, the temperature of the pipeline and the box was 280°C, the spinning speed was 1000m / min, the drafting multiple was 1.8 times, the spinneret used a flat spinneret hole, and the modified copolymer short fibers were cut after spinning to obtain;

[0056] (3) Alkali reduction treatment:

[0057] The modified copolymer staple fibers were immersed in an aqueous solution containing 2.2wt.% sodium hydroxide and 20wt.% ethylene glycol for alkali reduction treatment at a temperature of 60°C, a bath ratio of 1:30, and a treatment time of 30 minutes. After the treatment, the fibers were neutralized with 0.5wt.% acetic acid, then washed with water and dried to obtain alkali-etched modified copolymer staple fibers, with an alkali reduction rate of 12.21%.

[0058] (4) Surface modification:

[0059] The protein was added to the NMMO solution and dissolved using a thin film evaporator to obtain a highly water-absorbent solution having a protein concentration of 5.5 wt.%;

[0060] The modified copolymer staple fibers etched by alkali are immersed in a solution of a highly water-absorbent substance for a first adsorption treatment at a temperature of 80°C for 45 minutes; then immersed in an aqueous solution containing 15wt.% tea polyphenols and 16wt.% acrylic acid (the pH value of which is adjusted to 5.5 with acetic acid) for a second adsorption treatment at a temperature of 50°C for 40 minutes; then immersed in a 10wt.% zinc acetate aqueous solution for irradiation treatment under the following conditions: room temperature, air atmosphere, and an absorbed dose of 80 kGy; finally, softened, oiled, and dried to obtain a highly hygroscopic chemical fiber.

[0061] Example 2

[0062] The highly hygroscopic chemical fiber is prepared as follows:

[0063] (1) Preparation of modified copolymer chips:

[0064] After mixing terephthalic acid and ethylene glycol in a mass ratio of 1:1.3, antimony trioxide accounting for 0.026% of the mass of terephthalic acid was added, the temperature was raised to 218°C, stirring was started, the temperature was continued to be raised to 243°C, caprolactam salt accounting for 10.5% of the mass of terephthalic acid and PEG-300 accounting for 7.2% of the mass of terephthalic acid were added, the temperature was evacuated to 0.025 Pa, a pre-polycondensation reaction was carried out at 250°C for 65 minutes, the temperature was continued to be raised to 265°C for polycondensation reaction for 170 minutes, after the polycondensation reaction was completed, granulation was performed to obtain slices, vacuum dried at 95°C for 61.5 minutes to pre-crystallize the slices, and then vacuum dried at 130°C until the water content was less than 100 ppm to obtain modified copolymer slices with an intrinsic viscosity of 0.71 dL / g;

[0065] (2) Preparation of modified copolymer staple fibers:

[0066] The modified copolymer slices were spun by a twin-screw extruder. The temperature of the twin-screw extruder was divided into three zones: the temperature of zone 1 was 265°C, the temperature of zone 2 was 272°C, the temperature of zone 3 was 278°C, the temperature of the metering pump was 283°C, the temperature of the pipeline and the box was 285°C, the spinning speed was 1100m / min, the drafting multiple was 2.5 times, the spinneret used a cross-shaped spinneret hole, and the modified copolymer short fibers were cut after spinning to obtain;

[0067] (3) Alkali reduction treatment:

[0068] The modified copolymer staple fibers were immersed in an aqueous solution containing 2.8wt.% sodium hydroxide and 25wt.% ethylene glycol for alkali reduction treatment at a temperature of 72°C, a bath ratio of 1:25, and a treatment time of 38min. After the treatment, 0.9wt.% acetic acid was used for neutralization, followed by washing and drying to obtain alkali-etched modified copolymer staple fibers, with an alkali reduction rate of 14.39%;

[0069] (4) Surface modification:

[0070] Cellulose was added to an ionic liquid (cation was allyl, anion was Cl - ), dissolving by thin film evaporator to obtain a highly water-absorbent solution having a cellulose concentration of 6.9 wt.%;

[0071] The modified copolymer staple fibers etched with alkali were immersed in a solution of a highly absorbent substance for a first adsorption treatment at a temperature of 82.5°C for a treatment time of 53 min; then immersed in an aqueous solution containing 17.6wt.% tea polyphenols and 18.1wt.% ethyl acrylate (the pH value of which was adjusted to 6.1 with acetic acid) for a second adsorption treatment at a temperature of 56°C for a treatment time of 52 min; then immersed in a 13.1wt.% silver acetate aqueous solution for irradiation treatment at room temperature, air atmosphere, and an absorption dose of 90 kGy; finally, softened, oiled, and dried to obtain highly hygroscopic chemical fibers.

[0072] Example 3

[0073] The highly hygroscopic chemical fiber is prepared as follows:

[0074] (1) Preparation of modified copolymer chips:

[0075] After mixing terephthalic acid and ethylene glycol in a mass ratio of 1:1.4, add antimony triacid accounting for 0.021% of the mass of terephthalic acid, heat to 220°C, start stirring, continue to heat to 250°C, add hexamethylenediamine adipate accounting for 12% of the mass of terephthalic acid and PEG-600 accounting for 8% of the mass of terephthalic acid, evacuate to 0.05Pa, carry out pre-polycondensation reaction at 250°C for 70min, continue to heat to 270°C for polycondensation reaction for 150min, after the polycondensation reaction is completed, granulate to obtain slices, first vacuum dry at 105°C for 70min to pre-crystallize the slices, and then continue to vacuum dry at 135°C until the water content is less than 100ppm, to obtain modified copolymer slices with an intrinsic viscosity of 0.71dL / g;

[0076] (2) Preparation of modified copolymer staple fibers:

[0077] The modified copolymer chips are spun by a twin-screw extruder. The temperature of the twin-screw extruder is divided into three zones: the temperature of zone 1 is 270°C, the temperature of zone 2 is 275°C, the temperature of zone 3 is 280°C, the temperature of the metering pump is 285°C, the temperature of the pipeline and the box is 290°C, the spinning speed is 1200m / min, the drafting multiple is 3.2 times, the spinneret adopts a Y-type spinneret hole, and the modified copolymer short fibers are cut after spinning to obtain;

[0078] (3) Alkali reduction treatment:

[0079] The modified copolymer staple fibers were immersed in an aqueous solution containing 3.5wt.% sodium hydroxide and 30wt.% ethylene glycol for alkali reduction treatment at a temperature of 80°C, a bath ratio of 1:20, and a treatment time of 45 minutes. After the treatment, the fibers were neutralized with 1.2wt.% acetic acid, then washed with water and dried to obtain alkali-etched modified copolymer staple fibers with an alkali reduction rate of 16.18%.

[0080] (4) Surface modification:

[0081] Protein and cellulose in a mass ratio of 1:1 were added to an ionic liquid (cation: ethyl; anion: CH3COO - ), dissolving by thin film evaporator to obtain a highly water-absorbing substance solution with a total concentration of protein and cellulose of 8.0 wt.%;

[0082] The modified copolymer staple fibers etched by alkali are immersed in a solution of a highly water-absorbent substance for a first adsorption treatment at a temperature of 85°C for a treatment time of 60 minutes; then immersed in an aqueous solution containing 20wt.% tea polyphenols and 20wt.% acrylamide (the pH value of which is adjusted to 6.8 with lactic acid) for a second adsorption treatment at a temperature of 60°C for a treatment time of 60 minutes; then immersed in a 15wt.% zinc acetate aqueous solution for irradiation treatment under the following irradiation treatment conditions: room temperature, air atmosphere, and an absorption dose of 100kGy; finally, softened, oiled, and dried to obtain a highly hygroscopic chemical fiber.

[0083] Comparative Example 1

[0084] The difference between this comparative example and Example 1 is that when preparing the modified copolymer slices in step (1), pentamethylenediamine adipate is replaced by an equal mass of PEG-200.

[0085] Comparative Example 2

[0086] The difference between this comparative example and Example 1 is that during the alkali weight reduction treatment in step (3), the modified copolymer staple fibers are immersed in an aqueous solution containing 2.2 wt.% sodium hydroxide for alkali weight reduction treatment, and no ethylene glycol is added.

[0087] Comparative Example 3

[0088] The difference between this comparative example and Example 1 is that the alkali weight reduction treatment in step (3) is omitted, and the modified copolymer staple fibers are directly subjected to surface modification treatment.

[0089] Comparative Example 4

[0090] The difference between this comparative example and Example 1 is that, during the surface modification treatment in step (4), the first adsorption treatment of the highly absorbent solution is not performed.

[0091] Comparative Example 5

[0092] The difference between this comparative example and Example 1 is that no crosslinking agent is used in the surface modification treatment in step (4), which is as follows:

[0093] The protein was added into the NMMO solution and dissolved by a thin film evaporator to obtain a highly water-absorbent solution with a protein concentration of 5.5 wt.%. The modified copolymer staple fibers etched by alkali were immersed in the highly water-absorbent solution for a first adsorption treatment at a temperature of 80°C for 45 min. The fibers were then immersed in an aqueous solution containing 15 wt.% of tea polyphenols (the pH value of which was adjusted to 5.5 with acetic acid) for a second adsorption treatment at a temperature of 50°C for 40 min. The fibers were then immersed in a 10 wt.% aqueous zinc acetate solution for complexation. Finally, the fibers were softened, oiled and dried to obtain highly hygroscopic chemical fibers.

[0094] The chemical fibers prepared in each embodiment and comparative example were subjected to performance tests, wherein the inhibition rate of Escherichia coli and the inhibition rate of Candida albicans were tested in accordance with the standard GB / T20944.3-2008; the ammonia reduction rate was tested in accordance with the standard GB / T33610.2-2017; the moisture regain was tested in accordance with the standard GB / T6503-2008; the ultraviolet transmittance was tested in accordance with the standard GB / T 18830-2009; and the softness was tested in accordance with the standard GBT8942-2016. During the test, the chemical fibers were made into nonwoven fabrics of the same specifications. The test results are shown in Table 1.

[0095]

[0096] As can be seen from Table 1, the chemical fibers prepared in Examples 1-3 of the present invention not only have high hygroscopicity, but also have multifunctional properties such as antibacterial, deodorizing, and UV protection. Compared with Example 1, Comparative Example 1 does not add pentamethylenediamine adipate when preparing the modified copolymer slices, which mainly affects the moisture regain and softness of the chemical fiber. Although the softness of the prepared chemical fiber is increased, the moisture regain is reduced; Comparative Example 2 does not add ethylene glycol during the alkali reduction treatment, so that the degree of alkali reduction is reduced. During the surface modification treatment, the adsorption amount of functional components is reduced, thereby reducing the antibacterial, deodorizing, moisture regain and UV protection of the chemical fiber; Comparative Example 3 does not perform alkali reduction treatment. During the surface modification treatment, the adsorption amount of functional components is significantly reduced, resulting in the final chemical fiber. The antibacterial property, deodorizing property, moisture regain and UV resistance are greatly reduced; in comparative example 4, the first adsorption treatment of the highly water-absorbent solution is not performed, which can increase the adsorption amount of tea polyphenols and cross-linking agent during the second adsorption treatment, thereby improving the antibacterial property, deodorizing property and UV resistance of the chemical fiber, but the moisture regain of the chemical fiber is significantly reduced; in comparative example 5, no cross-linking agent is used during the surface modification treatment, so that the degree of cross-linking on the surface of the chemical fiber is reduced, which can increase the softness of the chemical fiber, but also leads to a large loss of adsorbed functional substances, thereby reducing the antibacterial property, deodorizing property, UV resistance and hygroscopicity of the chemical fiber.

Claims

1. A method for preparing highly hygroscopic chemical fibers, Features: The following steps are involved: (1) Preparation of modified copolymer chips: Using terephthalic acid and ethylene glycol as main raw materials, polyamide salt and polyethylene glycol as modifiers, and carrying out polycondensation reaction under the action of a catalyst, a modified copolymer slice is obtained; Wherein, the catalyst is at least one of ethylene glycol antimony, antimony trioxide, and antimony trioxide; (2) Preparation of modified copolymer staple fibers: The modified copolymer slices are spun through a spinneret provided with special-shaped spinneret holes, and cut to obtain modified copolymer short fibers; (3) Alkali reduction treatment: The modified copolymer staple fibers are immersed in an aqueous solution of sodium hydroxide and ethylene glycol for alkali reduction treatment, and after the treatment is completed, they are neutralized, washed with water, and dried in sequence to obtain alkali-etched modified copolymer staple fibers; (4) Surface modification: The modified copolymer staple fibers etched with alkali are immersed in a highly water-absorbent solution for a first adsorption treatment, then immersed in an aqueous solution containing tea polyphenols and a cross-linking agent for a second adsorption treatment, then immersed in an aqueous solution of zinc acetate or silver acetate for irradiation treatment, and finally softened, oiled, and dried to obtain highly hygroscopic chemical fibers; The highly absorbent material solution is a solution obtained by dissolving protein and / or cellulose in NMMO solution or ionic liquid; and the cross-linking agent is at least one of acrylic acid, acrylonitrile, ethyl acrylate and acrylamide.

2. The method for preparing the highly hygroscopic chemical fiber according to claim 1, Features: In step (1), the mass ratio of terephthalic acid to ethylene glycol is 1:1.2-1.

4.

3. The method for preparing the highly hygroscopic chemical fiber according to claim 1, Features: In step (1), the polyamide salt is at least one of pentamethylenediamine adipate, caprolactam salt, and hexamethylenediamine adipate; the amount of the polyamide salt added is 8-12% of the mass of terephthalic acid; The polyethylene glycol is at least one of PEG-200, PEG-300, PEG-400 and PEG-600; the amount of polyethylene glycol added is 6-8% of the mass of terephthalic acid.

4. The method for preparing the highly hygroscopic chemical fiber according to claim 1, Features: In step (2), the special-shaped spinneret hole is one of a flat spinneret hole, a cross-shaped spinneret hole, and a Y-shaped spinneret hole.

5. The method for preparing the highly hygroscopic chemical fiber according to claim 1, Features: In step (3), in the aqueous solution of sodium hydroxide and ethylene glycol, the concentration of sodium hydroxide is 2.2-3.5 wt.%, and the concentration of ethylene glycol is 20-30 wt.%.

6. The method for preparing the highly hygroscopic chemical fiber according to claim 1, Features: In step (3), the alkali weight reduction treatment conditions are: temperature 60-80° C., treatment bath ratio 1:20-30, and time 30-45 min; the alkali weight reduction rate of the alkali-etched modified copolymer staple fibers is 12.21-16.18%.

7. The method for preparing the highly hygroscopic chemical fiber according to claim 1, Features: In step (4), the concentration of the highly water-absorbent substance in the highly water-absorbent substance solution is 5.5-8.0 wt.%; The first adsorption treatment temperature is 80~85°C and the treatment time is 45~60min.

8. The method for preparing the highly hygroscopic chemical fiber according to claim 1, Features: In step (4), the aqueous solution containing tea polyphenols and a cross-linking agent has a tea polyphenol concentration of 15-20 wt.%, a cross-linking agent concentration of 16-20 wt.%, and the pH value thereof is adjusted to 5.5-6.8 using acetic acid or lactic acid; The second adsorption treatment temperature is 50~60℃, and the treatment time is 40~60min.

9. The method for preparing highly hygroscopic chemical fiber according to claim 1, Features: In step (4), the concentration of zinc acetate or silver acetate in the aqueous solution is 10-15 wt.%; Irradiation treatment conditions are: room temperature, air atmosphere, absorbed dose 80~100kGy.

10. A highly hygroscopic chemical fiber prepared by the preparation method according to any one of claims 1 to 9, Features: The inhibition rate of Escherichia coli is >90%, the inhibition rate of Candida albicans is >88%, the reduction rate of ammonia is >87%, the moisture regain is >10%, and the UV transmittance is <5%.