Taslon fabric and its processing technology
Through the improved processing technology of Tasilon fabric, the water-insoluble complex is formed by using graphene oxide modified nylon 6 ATY and acid dye combined with calcium and aluminum metal ions to form a water-insoluble complex, which solves the problem of the existing Jinpoly Tasilon fabric 85℃ soap washing and scrubbing of soap in 85℃ The problem of low degree has achieved good anti-ultraviolet and antibacterial properties.
Patent Information
- Application Number
- CN202411172885.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The existing Jindita Silong fabric has low fastness at 85℃, especially when dyed dark, and lacks UV and antibacterial properties.
The jewellery is made of a polyester tower wire cloth by a water jet loom. The warp yarn is polyester FDY and the weft yarn is graphene oxide modified nylon 6 ATY. It is cooled, flat desorbed, pre-determined, single dyed, spread cloth, steam-stealing Color and water washing molding process, combining acid dyes with calcium and aluminum metal ions to form a water-insoluble complex, improve the wet fastness of the fiber, and add sodium dihydrogen phosphate, sodium polyacrylate and calcium chloride to the compound solution to modify Pyramid stone powder and aluminum hydroxide enhance the fabric's UV and antibacterial properties.
The fabric has significantly improved the fastness of soap washing at 85℃ to reach level 4, and it also gives good UV resistance and antibacterial properties, especially the antibacterial rate of E. coli reaches more than 95%, and the UPF value reaches 50+.
Smart Images

Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textile fabrics, and in particular to a taslon fabric and a processing technology thereof. Background Art
[0002] Taslon fabrics are comfortable to wear, warm and breathable, and are one of the best-selling synthetic fiber imitation silk products all year round. Traditional Taslon is generally made of nylon (or polyester) filaments and nylon (or polyester) air-textured yarns. Now, nylon-polyester Taslon has also appeared, which uses the different dyeing properties of nylon and polyester to achieve a special coloring effect of single-dyeing nylon without dyeing polyester, while giving full play to the respective advantages of polyester and nylon.
[0003] The existing dyeing and finishing process of nylon-polyester taslon fabric generally includes pre-treatment, pre-setting, dyeing, color fixation and post-finishing setting. When dyeing, acid dyes are used to dye nylon, while polyester is not dyed with acid dyes. The molecular formula of nylon 6 is generally (C6H 11 NO)n, the groups in the molecular chain that can produce adsorption with acid dyes are terminal amino groups and amide groups. The anion of the acid dye forms an ion bond with the terminal amino group and a hydrogen bond with the amide group. The dyeing rate and levelness are good, but the soap fastness at 85℃ is generally not high, especially when dyeing dark colors. Summary of the invention
[0004] The invention aims to provide a taslon fabric and a processing technology thereof, which can improve the 85°C soap washing fastness of the fabric and at the same time give the fabric good anti-ultraviolet performance and antibacterial performance.
[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:
[0006] The processing technology of Taslon fabric includes the following steps:
[0007] S1. Weaving: a nylon-polyester taslon grey fabric with ground weave and side weave is obtained by weaving with a water jet loom, wherein the ground weave is a double plain weave weave, the side weave is a square weave, the warp yarn of the ground weave is 100D polyester full-dull FDY, the warp yarn of the side weave is 100D polyester semi-dull FDY, and the weft yarns of the ground weave and the side weave are both 160D graphene oxide modified nylon 6 ATY and 250D graphene oxide modified nylon 6 ATY, and the weft is cast in a ratio of 3:1;
[0008] S2, cold stacking: liquid rolling rate 50%-60%, vehicle speed 40m / min-50m / min, cold stacking time 10 hours-12 hours;
[0009] S3, open width desizing: the desizing solution contains 20g / L-25g / L of liquid alkali, 3g / L-4g / L of oil remover, 8g / L-12g / L of chelating dispersant, and 15g / L-20g / L of desizing agent; the liquid squeeze rate is 60%-70%, the desizing temperature is 95℃-98℃, and the desizing time is 100s-120s; hot washing, cold washing and acid washing are performed after desizing;
[0010] S4, pre-setting: temperature 150℃-155℃, time 20s-30s;
[0011] S5, single dyeing of graphene oxide modified nylon 6 ATY: bath ratio 1: 10-12, immersing in acidic dye solution and adjusting the pH value to 6-6.5, running for 10min-15min, slowly heating to 70℃-75℃ and keeping warm for 10min-15min, then heating to 105℃-110℃ at 1.5℃ / min-1.8℃ / min, keeping warm for 30min-40min, finally cooling to 70℃-75℃, draining, washing and discharging the cloth; the acidic dye solution includes acid black 2%-4%, leveling agent 1g / L-2g / L, bath softener CN 0.5g / L-1g / L, organic acid release agent VS 0.5g / L-1g / L;
[0012] S6, spreading the cloth, preheating to 60°C-70°C and then scraping the compound liquid on the surface of the cloth, the compound liquid is composed of the following components by weight: 1.5-3 parts of sodium dihydrogen phosphate, 4-6 parts of sodium polyacrylate, 8-12 parts of calcium chloride modified stamen powder, 15-20 parts of aluminum hydroxide, 100 parts of water, and the viscosity is 150 mPa•s-200 mPa•s;
[0013] S7, steaming fixation: steaming temperature is 110℃-120℃, steaming humidity is 80%-90%, steaming time is 20min-40min;
[0014] S8, washing and setting at a setting temperature of 160°C-165°C and a speed of 50m / min-55m / min to obtain taslon fabric.
[0015] Preferably, the warp and weft density of the Taslon fabric is 370 threads / 10cm×200 threads / 10cm, and the finished product width is 145cm.
[0016] Preferably, the cold stack in step S2 is processed by padding in five water tanks, the first and second water tanks are controlled at 90°C-95°C, the third and fourth water tanks are controlled at 80°C-85°C, and the fifth water tank is controlled at 60°C-65°C.
[0017] Preferably, the cold stack liquid in step S2 contains: 20g / L-25g / L of liquid caustic soda, 10g / L-15g / L of refining deoiling agent, and 2g / L-4g / L of penetrant.
[0018] Preferably, the acid black structural formula in step S5 is:
[0019] .
[0020] Preferably, the compound liquid preparation method in step S6 is: disperse the prefabricated calcium chloride modified stamen powder on a GFJ-0.4 disperser at 4000r / min-5000r / min for 10min-15min, then add sodium polyacrylate, aluminum hydroxide, disodium hydrogen phosphate and water, and continue to disperse at the same speed for 15min-20min.
[0021] Preferably, the prefabrication process of the calcium chloride modified quartz powder is: crushing the quartz to a particle size of 40 microns to 80 microns; calcining the quartz at 700° C. to 800° C.; adding a calcium chloride aqueous solution, mixing and reacting for 6-8 hours; washing with deionized water for multiple times, and drying.
[0022] Preferably, the washing in step S8 is carried out in sequence: cold water washing, soap washing, hot water washing and cold water washing.
[0023] The present invention further provides a taslon fabric produced by the above processing technology.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The warp yarn of the taslon fabric of the present invention is made of polyester FDY and the weft yarn is made of graphene oxide modified nylon 6 ATY. The warp and weft interweaving of the ground structure is a double weft plain weave structure, and the appearance presents a honeycomb taslon style.
[0026] The surface of the graphene oxide modified nylon 6 ATY of the present invention is rich in hydrophilic groups such as hydroxyl groups and carboxyl groups, as well as amide groups and amino groups. In the dyeing step, the acid dye is mainly combined with the amino groups and amide groups on the fiber surface through sulfonic acid groups through ionic bonds and hydrogen bonds, while most of the hydrophilic groups such as hydroxyl groups and carboxyl groups are exposed but at the same time there is a Coulomb repulsion between the acid dyes, so that the wet fastness of the acid dye on the fiber surface, especially the 85°C soap fastness, is poor. Therefore, in the step of scraping the compound liquid and steaming the color fixation, calcium and aluminum metal ions are coordinated with the hydroxyl groups, carboxyl groups exposed on the fiber surface and the two hydroxyl groups on the ortho position of the azo group of the acid dye to form a chelate ring structure, so that a water-insoluble complex is formed between the fiber, the acid dye and the calcium and aluminum metal ions, and the water-insoluble complex is adsorbed by the interaction between the fiber and the fiber through π-π bonds, thereby improving the 85°C soap fastness while ensuring the best level dyeing effect, and at the same time, the fabric is given good antibacterial and anti-ultraviolet properties based on graphene. DETAILED DESCRIPTION
[0027] Example 1
[0028] This embodiment provides a taslon fabric, and its processing technology specifically includes the following steps:
[0029] S1. Weaving: A nylon-polyester taslon grey fabric with ground and side weaves was obtained by weaving with a water jet loom, the warp and weft density was 370 / 10cm×200 / 10cm, and the finished width was 145cm. The ground weave was a double plain weave weave, the side weave was a square weave, the warp yarn of the ground weave was 100D polyester full-dull FDY (fully stretched yarn), the warp yarn of the side weave was 100D polyester semi-dull FDY, and the weft yarns of the ground weave and side weave were both 160D graphene oxide modified nylon 6 ATY (air-deformed yarn) and 250D graphene oxide modified nylon 6 ATY with a weft ratio of 3:1.
[0030] S2, cold stacking: immersion and rolling treatment in five water tanks, rolling rate 60%, vehicle speed 45m / min, cold stacking time 12 hours, the first and second water tanks are controlled at 90℃, the third and fourth water tanks are controlled at 85℃, and the fifth water tank is 65℃; the cold stacking liquid in each water tank contains 20g / L liquid caustic soda with a mass fraction of 32%, 12g / L refined degreasing agent HT, and 3g / L penetrant PT-70N.
[0031] S3, open width desizing: liquid alkali 20g / L, degreasing spirit TF-101CN 4g / L, chelating dispersant LT 10g / L, desizing agent TJ-1 18g / L, liquid rolling rate 65%, desizing temperature 95℃, desizing time 120 seconds; after desizing, hot wash, cold wash and acid wash at 80℃.
[0032] S4, pre-setting: temperature 155℃, time 30 seconds.
[0033] S5. Single dyeing of graphene oxide modified nylon 6 ATY: bath ratio 1:10, immersed in acidic dye solution and adjusted to pH 6.5, running for 10 minutes, slowly heated to 75°C and kept warm for 15 minutes, then heated to 105°C at 1.5°C / min, kept warm for 30 minutes, finally cooled to 75°C, drained, washed and discharged; the acidic dye solution included acid black 3% (owf), leveling agent peregrine O 1g / L, bath softener CN 1g / L, and organic acid release agent VS 0.5g / L.
[0034] The acid black structural formula is: .
[0035] S6, spread the cloth, preheat to 70°C and then scrape the compound liquid on the surface of the cloth, the compound liquid is composed of the following components by weight: 2 parts of sodium dihydrogen phosphate, 5 parts of sodium polyacrylate, 10 parts of calcium chloride modified stamen powder, 20 parts of aluminum hydroxide, 100 parts of water, and the viscosity is 175 mPa•s.
[0036] The preparation method of the compound liquid is as follows: the prefabricated calcium chloride modified stahl powder is dispersed on a GFJ-0.4 disperser at 4000r / min for 15min, and then sodium polyacrylate, aluminum hydroxide, disodium hydrogen phosphate and water are added, and the dispersion is continued at the same speed for 15min. The prefabrication process of the calcium chloride modified stahl powder is as follows: crushing the stahl to a particle size of 40 microns to 80 microns; calcining the stahl at 800°C; adding a calcium chloride aqueous solution, mixing and reacting for 8 hours; washing with deionized water for multiple times, and drying.
[0037] S7. Steaming fixation: the steaming temperature is 115°C, the steaming humidity is 85%, and the steaming time is 30 minutes.
[0038] S8, washing and shaping: flat car wash cold water washing → flat car wash soap washing: 2g / L neutral soap flakes, soap washing temperature 85℃, soap washing time 10 minutes → flat car wash hot water washing: water washing temperature 60℃ → flat car wash cold water washing. The shaping temperature is 165℃, speed 50m / min.
[0039] The 85°C soap washing fastness of the Taslon fabric of this embodiment reaches level 4 (ISO 105-C06-E2S (85°C test)), the Escherichia coli antibacterial rate reaches more than 95% (GB / T 20944.3-2008), and the UPF value reaches 50+ (GB / T18830-2009).
[0040] Example 2
[0041] This embodiment provides a taslon fabric, and its processing technology specifically includes the following steps:
[0042] S1. Weaving: A nylon-polyester taslon grey fabric with ground and side weaves was obtained by weaving with a water jet loom, the warp and weft density was 370 / 10cm×200 / 10cm, and the finished width was 145cm. The ground weave was a double plain weave weave, the side weave was a square weave, the warp yarn of the ground weave was 100D polyester full-dull FDY (fully stretched yarn), the warp yarn of the side weave was 100D polyester semi-dull FDY, and the weft yarns of the ground weave and side weave were both 160D graphene oxide modified nylon 6 ATY (air-deformed yarn) and 250D graphene oxide modified nylon 6 ATY with a weft ratio of 3:1.
[0043] S2, cold stacking: immersion and rolling treatment in five water tanks, rolling rate 55%, vehicle speed 50m / min, cold stacking time 12 hours, the first and second water tanks are controlled at 90℃, the third and fourth water tanks are controlled at 85℃, and the fifth water tank is 65℃; the cold stacking liquid in each water tank contains 22g / L liquid caustic soda with a mass fraction of 32%, 15g / L refining degreasing agent HT, and 3.5g / L penetrant PT-70N.
[0044] S3, open width desizing: liquid alkali 25g / L, degreasing spirit TF-101CN 3g / L / L, chelating dispersant LT 10g / L, desizing agent TJ-1 20g / L, liquid rolling rate 65%, desizing temperature 95℃, desizing time 120 seconds; after desizing, hot wash, cold wash and acid wash at 80℃.
[0045] S4, pre-setting: temperature 155℃, time 30 seconds.
[0046] S5. Single dyeing of graphene oxide modified nylon 6 ATY: bath ratio 1:10, immersed in acidic dye solution and adjusted to pH 6.5, running for 10 minutes, slowly heated to 75°C and kept warm for 15 minutes, then heated to 105°C at 1.5°C / min, kept warm for 30 minutes, finally cooled to 75°C, drained, washed and discharged; the acidic dye solution included acid black 3% (owf), leveling agent peregrine O 1g / L, bath softener CN 1g / L, and organic acid release agent VS 0.5g / L.
[0047] The acid black structural formula is: .
[0048] S6, spread the cloth, preheat to 70°C and then scrape the compound liquid on the surface of the cloth, the compound liquid is composed of the following components by weight: 2 parts of sodium dihydrogen phosphate, 6 parts of sodium polyacrylate, 12 parts of calcium chloride modified stamen powder, 18 parts of aluminum hydroxide, 100 parts of water, and the viscosity is 185 mPa•s.
[0049] The preparation method of the compound liquid is as follows: the prefabricated calcium chloride modified stahl powder is dispersed on a GFJ-0.4 disperser at 4000r / min for 15min, and then sodium polyacrylate, aluminum hydroxide, disodium hydrogen phosphate and water are added, and the dispersion is continued at the same speed for 15min. The prefabrication process of the calcium chloride modified stahl powder is as follows: crushing the stahl to a particle size of 40 microns to 80 microns; calcining the stahl at 800°C; adding a calcium chloride aqueous solution, mixing and reacting for 8 hours; washing with deionized water for multiple times, and drying.
[0050] S7. Steaming fixation: the steaming temperature is 120°C, the steaming humidity is 80%, and the steaming time is 30 minutes.
[0051] S8, washing and shaping: flat car wash cold water washing → flat car wash soap washing: 2g / L neutral soap flakes, soap washing temperature 85℃, soap washing time 10 minutes → flat car wash hot water washing: water washing temperature 60℃ → flat car wash cold water washing. The shaping temperature is 165℃, speed 50m / min.
[0052] The 85°C soap washing fastness of the Taslon fabric of this embodiment reaches level 4 (ISO 105-C06-E2S (85°C test)), the Escherichia coli antibacterial rate reaches more than 95% (GB / T 20944.3-2008), and the UPF value reaches 50+ (GB / T18830-2009).
[0053] Comparative Example 1
[0054] The difference between this comparative example and the above-mentioned embodiment 1 is that the weft yarns of the ground weave and the side weave are changed to 160D nylon 6ATY and 250D nylon 6 ATY at a ratio of 3:1.
[0055] The soap washing fastness of the taslon fabric in this comparative example at 85°C reaches Grade 3 (ISO 105-C06-E2S (85°C test)), and the antibacterial rate of E. coli and the UPF value are far inferior to those in Example 1.
[0056] Comparative Example 2
[0057] The only difference between this comparative example and the above-mentioned embodiment 1 is that the acid black in step S5 is weak acid black BR.
[0058] The 85°C soap washing fastness of the comparative taslon fabric reaches level 2 (ISO 105-C06-E2S (85 degrees test)), the Escherichia coli antibacterial rate reaches more than 95% (GB / T 20944.3-2008), and the UPF value reaches 50+ (GB / T18830-2009).
[0059] Comparative Example 3
[0060] The difference between this comparative example and the above-mentioned Example 1 is that steps S6-S7 are replaced by the following steps: acidic color fixing agent NBS is used for long-wheel color fixing, the temperature is 95° C., the vehicle speed is 30 m / min, the color fixing time is 25 min, and the amount of acidic color fixing agent NBS is 1.5% (owf).
[0061] The 85°C soap washing fastness of the comparative taslon fabric reaches level 2 (ISO 105-C06-E2S (85 degrees test)), the Escherichia coli antibacterial rate reaches more than 95% (GB / T 20944.3-2008), and the UPF value reaches 50+ (GB / T18830-2009).
[0062] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which shall fall within the scope of the present invention to be protected. The scope of protection of the present invention shall be defined by the attached claims and their equivalents.
Claims
1. Taslon fabric processing technology, characterized in that: The specific steps include: S1. Weaving: a nylon-polyester taslon grey fabric with ground weave and side weave is obtained by weaving with a water jet loom, wherein the ground weave is a double plain weave weave, the side weave is a square weave, the warp yarn of the ground weave is 100D polyester full-dull FDY, the warp yarn of the side weave is 100D polyester semi-dull FDY, and the weft yarns of the ground weave and the side weave are both 160D graphene oxide modified nylon 6ATY and 250D graphene oxide modified nylon 6 ATY, with the ratio of 3:1; S2, cold stacking: liquid rolling rate 50%-60%, vehicle speed 40m / min-50m / min, cold stacking time 10 hours-12 hours; S3, open width desizing: the desizing solution contains 20g / L-25g / L of liquid alkali, 3g / L-4g / L of oil remover, 8g / L-12g / L of chelating dispersant, and 15g / L-20g / L of desizing agent; the liquid squeeze rate is 60%-70%, the desizing temperature is 95℃-98℃, and the desizing time is 100s-120s; hot washing, cold washing and acid washing are performed after desizing; S4, pre-setting: temperature 150℃-155℃, time 20s-30s; S5, single dyeing of graphene oxide modified nylon 6 ATY: bath ratio 1: 10-12, immersing in acidic dye solution and adjusting the pH value to 6-6.5, running for 10min-15min, slowly heating to 70℃-75℃ and keeping warm for 10min-15min, then heating to 105℃-110℃ at 1.5℃ / min-1.8℃ / min, keeping warm for 30min-40min, finally cooling to 70℃-75℃, draining, washing and discharging the cloth; the acidic dye solution includes acid black 2%-4%, leveling agent 1g / L-2g / L, bath softener CN 0.5g / L-1g / L, organic acid release agent VS 0.5g / L-1g / L; The acid black structural formula in step S5 is: ; S6, spreading the cloth, preheating to 60°C-70°C and then scraping the composite liquid on the surface of the cloth, the composite liquid is composed of the following components by weight: 1.5-3 parts of sodium dihydrogen phosphate, 4-6 parts of sodium polyacrylate, 8-12 parts of calcium chloride modified stamen powder, 15-20 parts of aluminum hydroxide, 100 parts of water, and the viscosity is ; S7, steaming fixation: steaming temperature is 110℃-120℃, steaming humidity is 80%-90%, steaming time is 20min-40min; S8, washing and setting at a setting temperature of 160°C-165°C and a speed of 50m / min-55m / min to obtain taslon fabric.
2. The taslon fabric processing technology according to claim 1, characterized in that: The warp and weft density of the Taslon fabric is 370 threads / 10cm×200 threads / 10cm, and the finished product width is 145cm.
3. The taslon fabric processing technology according to claim 1, characterized in that: The cold stack in step S2 is subjected to padding treatment in five water tanks, the first and second water tanks are controlled at 90°C to 95°C, the third and fourth water tanks are controlled at 80°C to 85°C, and the fifth water tank is controlled at 60°C to 65°C.
4. The taslon fabric processing process according to claim 1, characterized in that: The cold stack liquid in step S2 contains: 20g / L-25g / L of liquid caustic soda, 10g / L-15g / L of refining degreasing agent, and 2g / L-4g / L of penetrant.
5. The taslon fabric processing technology according to claim 1, characterized in that: The preparation method of the compound liquid in step S6 is: disperse the prefabricated calcium chloride modified stamen powder on a GFJ-0.4 disperser at 4000r / min-5000r / min for 10min-15min, then add sodium polyacrylate, aluminum hydroxide, disodium hydrogen phosphate and water, and continue to disperse at the same speed for 15min-20min.
6. The taslon fabric processing technology according to claim 5, characterized in that: The prefabrication process of the calcium chloride modified quartz powder is as follows: crushing the quartz to a particle size of 40 microns to 80 microns; calcining the quartz at 700° C. to 800° C.; adding a calcium chloride aqueous solution, mixing and reacting for 6 to 8 hours; washing with deionized water for multiple times, and drying.
7. The taslon fabric processing technology according to claim 1, characterized in that: The washing in step S8 is carried out in sequence: cold water washing, soap washing, hot water washing and cold water washing.
8. A taslon fabric produced by the processing technology as claimed in any one of claims 1 to 7.