By using non-metal atoms in the platinum-based alloy catalyst to cooperate with platinum, M1 and M2, the problem of insufficient activity and stability of the platinum-based alloy catalyst is solved, achieving a substantial improvement in high activity and stability in fuel cells, and reducing the environmental pollution.
Patent Information
- Application Number
- CN202410755464.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-09-24
AI Technical Summary
Existing platinum-based alloy catalysts have problems of insufficient activity and low stability in fuel cells, especially catalyst deactivation and environmental pollution due to dissolution of precious metals.
Using a ternary platinum-based alloy catalyst, through the synergistic cooperation of non-metal atoms (N and/or P) and platinum, M1 and M2 elements, it inhibits metal dissolution, anchors nanoparticles, adjusts particle size, and improves the activity and stability of the catalyst. .
It significantly improves the activity and stability of the catalyst in the fuel cell cathode, reduces the migration and agglomeration of nanoparticles, reduces the amount of platinum used, and the preparation process is environmentally friendly and suitable for large-scale production.
Smart Images

Figure CN118693300A
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts and relates to a ternary platinum-based alloy catalyst and a preparation method and application thereof. Background Art
[0002] Platinum catalysts have become the preferred catalyst for proton exchange membrane fuel cells (PEMFC) due to their great potential in oxygen reduction reaction performance. However, in practical applications, they have problems such as excessive dosage and high price. In order to solve the above problems, the most effective way in the past 10 years is to prepare alloys of transition metals such as Fe, Co, Ni, etc. with Pt. The resulting PtM alloy can greatly improve the catalytic activity of the oxygen reduction reaction at the cathode of the fuel cell. Based on this, the development of low-platinum alloy electrocatalysts is imminent.
[0003] For example, CN116251602A discloses a method for preparing a platinum-copper alloy catalyst, a platinum-copper alloy catalyst and its application, which at least comprises the following steps: (1) mixing a raw material containing a platinum source, a copper source, a carrier and a surfactant with a solvent to obtain a mixed solution; (2) mixing the mixed solution obtained in (1) with sodium borohydride, reacting, and calcining to obtain the platinum-copper alloy catalyst.
[0004] Although the PtM alloy has a significant improvement in cathode oxygen reduction catalytic activity compared to Pt / C, with the development of the fuel cell field, the current activity is not enough to achieve commercialization. In addition, since the base metal of the PtM alloy is easily dissolved during the electrochemical process, it will poison the polymer in the fuel cell, thereby greatly reducing the stability of the fuel cell. In order to solve the above problems, there are studies on the formation of PtX catalysts or PtM binary alloy catalysts by doping non-metals, single transition metals or rare precious metals to improve the activity and stability of the cathode oxygen reduction reaction of fuel cells. However, the improvement of catalyst performance by single doping of non-metals is weak; the cost of doping of rare precious metals is high; doping of transition metals, due to their own instability, will gradually dissolve during the reaction, resulting in the deactivation or agglomeration of the alloy catalyst, affecting the activity and stability of the catalyst. At the same time, many preparation processes involve the use of a large amount of organic solvents and wastewater, which will cause pollution to the environment. In short, the effect of a single element on the stability of the alloy is weak.
[0005] Therefore, how to improve the stability of platinum-based alloy catalysts and enhance their catalytic performance is a technical problem that needs to be solved urgently. Summary of the invention
[0006] In view of the shortcomings of the prior art, the object of the present invention is to provide a ternary platinum-based alloy catalyst and a preparation method and use thereof. The ternary platinum-based alloy catalyst provided by the present invention effectively inhibits metal dissolution through the synergistic coordination of non-metallic atoms with platinum, M1 and M2 elements, strengthens the anchoring effect on nanoparticles, weakens the migration and agglomeration of nanoparticles, is conducive to adjusting the particle size of the platinum-based catalyst, and greatly improves the activity and stability of the catalyst in the cathode of the fuel cell.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a ternary platinum-based alloy catalyst, the ternary platinum-based alloy catalyst comprising a carrier and active particles supported in the carrier;
[0009] The ternary platinum-based alloy catalyst is doped with non-metallic atoms, and the non-metallic atoms include N atoms and / or P atoms; the active particles include a ternary platinum-based alloy material, and the constituent elements of the ternary platinum-based alloy material include Pt, M1 and M2, and M1 and M2 are different non-precious metal elements.
[0010] In the ternary platinum-based alloy catalyst provided by the present invention, non-metallic atoms (N and / or P) have a special synergistic effect on Pt, M1 and M2, and the incorporation of N / P does not reduce the amount of Pt used; on the one hand, the N and P elements can confine the Pt atoms to a certain extent, thereby inhibiting the migration and agglomeration of PtM1M2 nanoparticles (active particles) during the heat treatment process, and obtaining nanoparticles with small particle sizes; on the other hand, the 3d electron orbits of the N and P elements match the outermost electron orbit of Pt, which can produce specific electron interactions, change the electronic structure of Pt, and improve the oxygen reduction reaction (ORR reaction) activity. At the same time, due to the coordination effect of N and P on Pt, M1 and M2, the Pt, M1 and M2 atoms can be anchored, the migration of atoms in the ORR process is inhibited, the ORR reaction stability is improved, and the active particles are evenly dispersed on the carrier surface, thereby greatly improving the activity and stability of the catalyst in the cathode of the fuel cell.
[0011] In the present invention, non-metal atoms (N and / or P) and Pt, M1 and M2 cooperate with each other and are indispensable; if non-metal atoms are not contained, the particle size agglomeration and high ORR stability of the catalyst cannot be solved; and if it is a non-platinum-based precious metal alloy material, such as palladium-based, a higher ORR activity cannot be achieved; and if M1 or M2 is not contained, it is a non-ternary alloy material, and the catalyst cost cannot be reduced, and the ORR activity will also be partially affected.
[0012] Preferably, the non-metal atoms are doped on the surface of the carrier and / or in the active particles, preferably on the surface of the carrier.
[0013] In the present invention, non-metallic atoms are doped on the surface of the carbon carrier to better anchor the PtM1M2 nanoparticles, reduce agglomeration during the synthesis process, and improve the ORR stability.
[0014] Preferably, the mass proportion of the non-metallic atoms in the ternary platinum-based alloy catalyst is 0.1-5wt%, for example, 0.1wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% or 5wt%, etc., preferably 0.5-1wt%, but not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0015] In the present invention, if the mass proportion of non-metallic atoms in the ternary platinum-based alloy catalyst is too large, it will be detrimental to the stability of the carrier and will reduce the degree of graphitization of the carbon carrier; if the mass proportion is too small, the interaction between the non-metallic elements and the PtM1M2 nanoparticles will be weakened; further regulating to 0.5-1wt% can better enhance the above-mentioned interaction without affecting the degree of graphitization of the carbon carrier.
[0016] Preferably, the support comprises a carbon support.
[0017] Preferably, the mass proportion of Pt in the ternary platinum-based alloy catalyst is 10-50wt%, for example, 10wt%, 15wt%, 20wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 40wt%, 45wt% or 50wt%, preferably 25-35wt%, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0018] Preferably, the mass proportion of M1 in the ternary platinum-based alloy catalyst is 3 to 20 wt%, for example, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 6.5 wt%, 7 wt%, 7.5 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt% or 20 wt%, etc., preferably 6 to 8 wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, the M1 includes any one of Mn, Fe, Co, Ni, Cu or Zn, or a combination of at least two thereof.
[0020] Preferably, the mass proportion of M2 in the ternary platinum-based alloy catalyst is 3 to 20 wt%, for example, 3 wt%, 3.5 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt% or 20 wt%, etc., preferably 3 to 4 wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0021] In the present invention, the interaction of N\P elements on PtM1M2 is achieved by regulating the mass proportions of Pt, M1 and M2 in the active particles in the catalyst; and through further optimization of the mass proportions of the above elements, the element distribution in the alloy material is reasonable, the synergistic effect with non-metal atoms is more excellent, and the ORR activity and stability of the catalyst are better improved.
[0022] Preferably, the M2 includes any one of Mn, Fe, Co, Ni, Cu or Zn, or a combination of at least two of them.
[0023] Preferably, the average particle size of the active particles is 2 to 8 nm, for example 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm, 5 nm, 5.5 nm, 6 nm, 6.5 nm, 7 nm, 7.5 nm or 8 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] In the present invention, the average particle size of the active particles is within the numerical range of 2 to 8 nm, and has a relatively high specific surface area and electrochemical active area; while a particle size that is too large or too small will cause a loss in fuel cell performance.
[0025] In a second aspect, the present invention provides a method for preparing the ternary platinum-based alloy catalyst as described in the first aspect, the preparation method comprising the following steps:
[0026] Mixing a Pt precursor, an M1 precursor, an M2 precursor, a carrier and a first solvent to obtain a mixture, and thermally reducing the mixture to obtain the ternary platinum-based alloy catalyst;
[0027] Wherein, non-metallic atoms are doped during the mixing process or in the carrier, and the non-metallic atoms include N atoms and / or P atoms.
[0028] The preparation method provided by the invention has a simple preparation process, is easy to operate, is environmentally friendly, has low cost, and is suitable for large-scale production.
[0029] Preferably, the method of doping the carrier with non-metal atoms comprises:
[0030] A doping precursor and a carrier are mixed to obtain a carrier mixture, and a heat treatment is performed once to obtain a carrier doped with non-metallic atoms, wherein the doping precursor includes an N-containing doping precursor and / or a P-containing doping precursor.
[0031] Preferably, the doping precursor includes a gaseous doping precursor and / or a non-gaseous doping precursor.
[0032] Preferably, the doping precursor comprises a non-gaseous doping precursor, and the carrier mixture further comprises a second solvent.
[0033] In the present invention, when the doping precursor is a gas, the doping precursor gas and the protective gas are directly introduced into the carrier for mixing (the concentration of the doping precursor gas in the mixed gas is 5 to 10%), and then a heat treatment is performed to achieve doping modification; when it is a non-gas, it needs to be mixed in a second solvent.
[0034] Preferably, the support comprises a carbon support.
[0035] Preferably, the mass ratio of the doping precursor to the carrier is 1:1.5 to 1:4.5, for example, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4 or 1:4.5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] Preferably, the carrier mixture is subjected to a heat treatment after being dried by rotary evaporation;
[0037] Preferably, the N-doped precursor includes any one of aniline, polyaniline, melamine or ammonia, or a combination of at least two of them; the P-containing precursor includes any one of phytic acid, hypophosphite or tetraphenylphosphine chloride, or a combination of at least two of them.
[0038] Preferably, the atmosphere of the primary heat treatment includes a protective atmosphere, and the temperature of the primary heat treatment is 700-900°C, for example, 700°C, 750°C, 800°C, 850°C or 900°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] In the present invention, if the temperature of the primary heat treatment is too low, the graphitization degree of the carbon carrier will be reduced, while if the temperature is too high, the element doping amount will be reduced; and when the doping precursor is gaseous, the atmosphere of the primary heat treatment includes a mixed gas of a doping gas and a protective gas.
[0040] Preferably, the mixture is subjected to a thermal reduction treatment after being rotary dried.
[0041] In the present invention, in addition to rotary evaporation drying, other drying methods such as evaporation drying and freeze drying can also be used. Preferably, when rotary evaporation drying is used, the first solvent and the second solvent can be recycled and reused.
[0042] Preferably, the thermal reduction is performed under a reducing atmosphere.
[0043] Preferably, the temperature of the thermal reduction is 500-1000°C, for example, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or 1000°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0044] Preferably, the thermal reduction time is 1 to 10 h, for example 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h, etc., preferably 6 to 8 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0045] Preferably, the product after thermal reduction is subjected to secondary heat treatment.
[0046] In the present invention, the secondary heat treatment after thermal reduction plays a role in oxidizing a portion of the carbon coating layer.
[0047] Preferably, the secondary heat treatment is performed in an air atmosphere.
[0048] Preferably, the temperature of the secondary heat treatment is 100-250°C, for example 100°C, 125°C, 150°C, 175°C, 200°C, 225°C or 250°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0049] In the present invention, if the temperature of the secondary heat treatment is too low, it will be disadvantageous for the ordering of the ternary alloy; and if the temperature of the secondary heat treatment is too high, it will cause particle agglomeration.
[0050] Preferably, the product after the secondary heat treatment is subjected to acid washing, solid-liquid separation and drying.
[0051] Preferably, the dried product is subjected to three heat treatments at temperatures ranging from 200°C to 500°C, such as 200°C, 250°C, 300°C, 350°C, 400°C, 450°C or 500°C.
[0052] In the present invention, the three heat treatments are used for annealing and renormalization of surface Pt atoms.
[0053] Preferably, the pickling temperature is 40-80°C, such as 40°C, 50°C, 60°C, 70°C or 80°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0054] Preferably, the pickling time is 1 to 2 hours, such as 1 hour, 1.5 hours or 2 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0055] As a preferred technical solution, the preparation method comprises the following steps:
[0056] The doping precursor, the carrier and the second solvent are mixed, and a heat treatment is performed under a protective atmosphere to obtain a carrier doped with non-metal atoms;
[0057] A Pt precursor, an M1 precursor, an M2 precursor, a carrier and a first solvent are mixed, and thermally reduced at 500 to 1000° C. for 1 to 10 hours in a reducing atmosphere, and the thermally reduced product is subjected to a secondary heat treatment at 100 to 250° C. in an air atmosphere, acid washing, solid-liquid separation and drying, and thermally treated three times to obtain the ternary platinum-based alloy catalyst;
[0058] Wherein, the doping precursor includes an N-containing doping precursor and / or a P-containing doping precursor.
[0059] It should be noted that, except for the above-mentioned specific limitations, the selection of raw material types and the preparation process of the products and preparation methods provided by the present invention are all conventional technical means, and those skilled in the art can make adaptive selections and adjustments according to actual needs.
[0060] Optionally, the carbon support includes but is not limited to any one of commercial carbon black EC300-JD, EC600-JD, BP-2000 or XC-72;
[0061] Optionally, the Pt precursor includes but is not limited to at least one of chloroplatinic acid, potassium chloroplatinate, platinum acetylacetonate or platinous chloride;
[0062] Optionally, the M1 precursor includes but is not limited to at least one of manganese nitrate, manganese sulfate, manganese chloride, manganese acetylacetonate, ferric nitrate, ferric sulfate, ferric chloride, ferric acetylacetonate, cobalt nitrate, cobalt sulfate, cobalt chloride, cobalt acetylacetonate, nickel nitrate, nickel sulfate, nickel chloride, nickel acetylacetonate, copper nitrate, copper sulfate, copper chloride, copper acetylacetonate, zinc nitrate, zinc sulfate, zinc chloride or zinc acetylacetonate;
[0063] Optionally, the M2 precursor includes but is not limited to at least one of manganese nitrate, manganese sulfate, manganese chloride, manganese acetylacetonate, ferric nitrate, ferric sulfate, ferric chloride, ferric acetylacetonate, cobalt nitrate, cobalt sulfate, cobalt chloride, cobalt acetylacetonate, nickel nitrate, nickel sulfate, nickel chloride, nickel acetylacetonate, copper nitrate, copper sulfate, copper chloride, copper acetylacetonate, zinc nitrate, zinc sulfate, zinc chloride or zinc acetylacetonate;
[0064] Optionally, the first solvent includes but is not limited to at least one of ethanol or acetone;
[0065] Optionally, the second solvent includes but is not limited to ethanol and / or water. When it is a mixed solvent system of ethanol and water, the volume ratio of ethanol to water is 3:1;
[0066] Optionally, the protective atmosphere includes a nitrogen atmosphere or an inert gas atmosphere, and the reducing atmosphere includes hydrogen or a mixed gas of hydrogen and argon (the volume concentration of hydrogen is 2 to 10%);
[0067] Optionally, the acid used in the pickling includes but is not limited to any one of perchloric acid, sulfuric acid or acetic acid; the concentration of the acid may be 0.1 mol / L.
[0068] In a third aspect, the present invention further provides a use of the ternary platinum-based alloy catalyst as described in the first aspect, wherein the use comprises using the ternary platinum-based alloy catalyst in a fuel cell.
[0069] Compared with the prior art, the present invention has the following beneficial effects:
[0070] In the ternary platinum-based alloy catalyst provided by the present invention, non-metallic atoms (N and / or P) have a special synergistic effect on Pt, M1 and M2, and the incorporation of N / P does not reduce the amount of Pt used; on the one hand, the migration and agglomeration of nanoparticles (active particles) during the heat treatment process are suppressed, and nanoparticles with small particle sizes are obtained; on the other hand, the 3d electron orbits of the N and P elements match the outermost electron orbit of Pt, which can produce specific electron interactions, change the electronic structure of Pt, and improve the oxygen reduction reaction (ORR reaction) activity. At the same time, due to the coordination effect of N and P on Pt, M1 and M2, Pt, M1 and M2 atoms can be anchored, which suppresses the migration of atoms during the ORR process, improves the ORR reaction stability, and the active particles are evenly dispersed on the carrier surface, thereby greatly improving the activity and stability of the catalyst in the cathode of the fuel cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0071] Figure 1 This is the XRD pattern of the catalyst provided in Example 1.
[0072] Figure 2 TEM image of the catalyst provided in Example 1
[0073] Figure 3 This is a statistical distribution diagram of the particle size of the catalyst provided in Example 1.
[0074] Figure 4 This is a comparison chart of the activities of the catalysts provided for Example 1, commercial Pt / C and commercial platinum-cobalt (commercial PtCo alloy catalyst).
[0075] Figure 5 The catalyst provided for Example 1 is in O 2 Saturated 0.1 mol L -1 HClO 4 ORR forward scan polarization curves at the initial and every 10,000 cycles of stability testing in solution.
[0076] Figure 6 The mass specific activity and area specific activity of the catalyst provided for Example 1 at 0.9 V vs. RHE at the initial and after every 10,000 cycles of stability testing.
[0077] Figure 7 The cyclic voltammetry curves of the catalyst provided in Example 1 at the initial stage and after every 10,000 cycles of stability testing.
[0078] Figure 8 This is a comparison chart of ECSA data of the catalyst provided in Example 1 at the initial stage and after every 10,000 cycles of stability testing.
[0079] Fig. 9 This is the XRD pattern of the catalyst provided in Comparative Example 1.
[0080] Fig.10 This is the ORR forward scanning polarization curve of the catalyst provided in Comparative Example 1.
[0081] Fig.11 This is the XRD pattern of the catalyst provided for Comparative Example 2.
[0082] Fig.12 This is the ORR forward scanning polarization curve of the catalyst provided in Comparative Example 2.
[0083] Fig.13 This is the XRD pattern of the catalyst provided for Comparative Example 3.
[0084] Fig.14 This is the ORR forward scanning polarization curve of the catalyst provided in Comparative Example 3. DETAILED DESCRIPTION
[0085] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0086] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.
[0087] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0088] Example 1
[0089] This embodiment provides an N-doped ternary PtCoNi alloy catalyst, the catalyst comprising a carbon carrier (commercial EC300-JD) and active particles supported in the carbon carrier;
[0090] Among them, the surface of the carbon carrier is doped with N atoms; the active particles are ternary PtCoNi alloy materials; the average particle size of the catalyst and the mass proportion of each substance are shown in Table 1.
[0091] The preparation method of the catalyst is as follows:
[0092] (1) 5 g of commercial EC300-JD was placed in a tube furnace and heat treated at 800° C. for 2 h under a mixture of ammonia and argon (the concentration of ammonia in the mixed gas was 5%) to obtain N-doped carbon black;
[0093] 4 g of platinum acetylacetonate, 2.15 g of cobalt acetylacetonate (M1), and 1.08 g of nickel acetylacetonate (M2) were added to 300 mL of acetone and completely dissolved by sonication;
[0094] (2) adding 4 g of N-doped carbon black to the above solution, stirring overnight to allow it to be completely dispersed, and then removing the solvent by rotary evaporation to obtain a dry black solid powder;
[0095] (3) heat treating the black powder at 900° C. for two hours in a 5% hydrogen-argon mixed gas condition to obtain PtCoNi / NC to be treated;
[0096] (4) heat treating the above-mentioned PtCoNi / NC at 190° C. in an air atmosphere for one hour to oxidize the surface carbon coating layer;
[0097] (5) The oxidized PtCoNi / NC was placed in 0.1 mol L -1 The catalyst was then placed in a perchloric acid solution, stirred evenly, and heated to 80°C for acid washing for 1 hour to remove part of the cobalt and nickel on the surface of the nanoparticles. The catalyst was then washed with water until neutral and dried. Finally, the catalyst was heat treated at 400°C and 5% hydrogen-argon mixed gas for one hour to obtain the final PtM1M2 / XC ternary alloy catalyst.
[0098] Example 2
[0099] The difference between this embodiment and embodiment 1 is that the ternary alloy material in this embodiment is PtCoFe.
[0100] In the preparation method, nickel cobalt acetylacetonate is replaced by iron acetylacetonate.
[0101] The rest of the preparation methods and parameters were the same as those in Example 1.
[0102] Example 3
[0103] The difference between this embodiment and embodiment 1 is that in step (1) of this embodiment, diphenylphosphine and commercial carbon black EC300-JD in a mass ratio of 1:2.5 are mixed in a mixture of ethanol and water in a ratio of 3:1, and stirred overnight to allow them to be fully mixed; then all the solvent is removed to obtain a black powder, which is then heat treated at 800°C in an argon atmosphere for 2 hours to obtain a P-doped carbon carrier.
[0104] The rest of the preparation methods and parameters were the same as those in Example 1.
[0105] Example 4
[0106] The difference between this embodiment and embodiment 1 is that the ternary alloy material in this embodiment is PtMnCu.
[0107] In the preparation method, cobalt acetylacetonate is replaced by manganese acetylacetonate, and nickel acetylacetonate is replaced by copper acetylacetonate.
[0108] The rest of the preparation methods and parameters were the same as those in Example 1.
[0109] Example 5
[0110] The difference between this embodiment and embodiment 1 is that the ternary alloy material in this embodiment is PtMnZn.
[0111] In the preparation method, cobalt acetylacetonate is replaced by manganese acetylacetonate, and nickel acetylacetonate is replaced by zinc acetylacetonate.
[0112] The rest of the preparation methods and parameters were the same as those in Example 1.
[0113] Example 6
[0114] The difference between this embodiment and embodiment 1 is that the ternary alloy material in this embodiment is PtCoZn.
[0115] In the preparation method, nickel acetylacetonate is replaced by zinc acetylacetonate.
[0116] The rest of the preparation methods and parameters were the same as those in Example 1.
[0117] Example 7
[0118] The difference between this embodiment and embodiment 1 is that the ternary alloy material in this embodiment is PtNiZn.
[0119] The rest of the preparation methods and parameters were the same as those in Example 1.
[0120] Example 8
[0121] The difference between this embodiment and embodiment 1 is that N in this embodiment is doped into the active particles, and the preparation method is controlled to adjust the ammonia concentration to 10%.
[0122] The rest of the preparation methods and parameters were the same as those in Example 1.
[0123] Example 9
[0124] The difference between this embodiment and embodiment 1 is that in this embodiment, the mass proportion of N atoms in the ternary platinum-based alloy catalyst is 6wt%;
[0125] The heat treatment temperature in the preparation method is adjusted to 700°C.
[0126] The rest of the preparation methods and parameters were the same as those in Example 1.
[0127] Example 10
[0128] The difference between this embodiment and embodiment 1 is that the mass proportion of M2 in this embodiment is 5%.
[0129] In the preparation method, the amount of nickel acetylacetonate added was changed to 2.12 g.
[0130] The rest of the preparation methods and parameters were the same as those in Example 1.
[0131] Embodiment 11
[0132] The difference between this embodiment and embodiment 1 is that the temperature of the heat treatment in step (4) of this embodiment is 80°C.
[0133] The rest of the preparation methods and parameters were the same as those in Example 1.
[0134] Example 12
[0135] The difference between this embodiment and embodiment 1 is that the temperature of the heat treatment in step (4) of this embodiment is 300°C.
[0136] The rest of the preparation methods and parameters were the same as those in Example 1.
[0137] Comparative Example 1
[0138] The difference between this comparative example and Example 1 is that the catalyst provided in this comparative example does not contain Ni, that is, nickel acetylacetonate is not added in the preparation method.
[0139] The rest of the preparation methods and parameters were the same as those in Example 1.
[0140] Comparative Example 2
[0141] The difference between this comparative example and Example 1 is that the catalyst provided in this comparative example is not doped with N atoms.
[0142] In the preparation method, no N-doping process is performed, and commercial EC300-JD is directly used as a reaction carrier.
[0143] The rest of the preparation methods and parameters were the same as those in Example 1.
[0144] Comparative Example 3
[0145] The difference between this comparative example and Example 1 is that the catalyst provided in this comparative example is not doped with N atoms and does not contain Ni.
[0146] In the preparation method, no N-doping process is performed, and commercial EC300-JD is directly used as a reaction carrier; and no nickel acetylacetonate is added.
[0147] The rest of the preparation methods and parameters were the same as those in Example 1.
[0148] Comparative Example 4
[0149] The difference between this comparative example and Example 1 is that Pt is replaced by Pd in this comparative example.
[0150] In the preparation method, acetylacetonate palladium is used to replace acetylacetonate platinum.
[0151] Comparative Example 5
[0152] This embodiment provides a commercial Pt / C catalyst (manufacturer: Tanaka).
[0153] Comparative Example 6
[0154] This comparative example provides a commercial PtCo alloy catalyst (manufacturer: Umicore).
[0155] Table 1 shows the average particle size of the active particles of the catalysts provided by Examples 1-12 and Comparative Examples 1-6 and the mass percentage of each substance.
[0156] Table 1
[0157]
[0158]
[0159] [Performance Test of Catalysts Provided in Examples 1-12 and Comparative Examples 1-6]
[0160] Test method:
[0161] X-ray diffraction (XRD) test: The powder sample is evenly flattened in the groove of the quartz plate and placed in the test instrument. The instrument tube voltage and tube current are adjusted to 40kV and 15mA respectively. The test angle is 10°-90° and the scanning speed is 5°min. -1 ;
[0162] Catalyst performance test:
[0163] Take 3 mg of the catalyst and disperse it in a mixture of 780 μL isopropanol and 200 μL deionized water, add 20 μL 5% Nafion solution, and ultrasonicate for 1 hour. Apply 10 μL of the dispersed ink droplets on a disk (0.2475 cm 2 ) electrode, fully dried under a baking lamp, and made into 40ug Pt cm -2The electrode head with catalyst loading was used for testing. The specific electrochemical characterization test was carried out in a standard three-electrode system, with a carbon rod as the counter electrode and a saturated calomel electrode as the reference electrode. The test was carried out at room temperature and in O 2 Saturated 0.1M HClO 4 The ORR polarization curve measured in the electrolyte is 2 Saturated 0.1M HClO 4 Background CV curves were measured in the electrolyte; the specific scanning potential was 0.1-1.1 vs. RHE, and the scanning rate was 10 mV s -1 .
[0164] Test results:
[0165] The catalyst provided in Example 1 was characterized by XRD and TEM, and the particle size statistical distribution was performed. The characterization results were as follows: Figure 1 , Figure 2 and Figure 3 shown; from Figure 1 It can be seen that in the catalyst provided in Example 1, the alloy material is a standard ordered intermetallic alloy. Figure 2 and Figure 3 It can be seen that in the catalyst provided in Example 1, the active particles are evenly distributed on the carbon carrier, and the particles are highly dispersed and uniform.
[0166] Figure 4 The activity comparison diagram of the catalysts provided for Example 1, Comparative Example 5 and Comparative Example 6 is a comparison diagram of the activity of the catalysts provided.
[0167] Figure 5 The catalyst provided for Example 1 is in O 2 Saturated 0.1 mol L -1 HClO 4 ORR forward scan polarization curves at the initial and every 10,000 cycles of stability testing in solution.
[0168] Figure 6 The mass specific activity and area specific activity of the catalyst provided for Example 1 at 0.9 V vs. RHE at the initial and after every 10,000 cycles of stability testing.
[0169] Figure 7 The cyclic voltammetry curves of the catalyst provided in Example 1 at the initial stage and after every 10,000 cycles of stability testing.
[0170] Figure 8 This is a comparison chart of ECSA data of the catalyst provided in Example 1 at the initial stage and after every 10,000 cycles of stability testing.
[0171] from Figure 4-Figure 8It can be seen that the RDE stability test of the catalyst provided in Example 1 shows that after 30,000 cycles of accelerated decay, the half-wave potential decays by only 7.9 mV, the area specific activity (SA) decays by 30.9%, and the mass specific activity (MA) decreases from 0.88 AT mg to Pt -1 Down to 0.61A mg Pt -1 , decayed by 30.1%, which is much higher than the requirement of DOE 2025 target; in addition, the ECSA of the catalyst did not change much after 30,000 cycles of accelerated decay; the excellent ORR stability exhibited by the catalyst is due to the fact that the doping of transition metal M2 can produce a synergistic effect with X (N or P) in the catalyst, which can reduce the surface energy of Pt and M1 atoms on the surface of nanoparticles and inhibit the dissolution of Pt and M1 atoms during the ORR reaction; at the same time, the transition metal can help X (N or P) in the catalyst to strengthen the anchoring effect on alloy nanoparticles, further inhibit the agglomeration, migration and Ostwald ripening process of nanoparticles during the potential process, which is beneficial to the improvement of the ORR stability of the catalyst.
[0172] Fig. 9 The XRD pattern of the catalyst provided for Comparative Example 1; Fig.10 The ORR forward scanning polarization curve of the catalyst provided in Comparative Example 1 is as follows: Fig.10 It can be seen that when the catalyst provided in Comparative Example 1 does not contain M2, its activity and particle size are relatively poor in terms of suitability for actual fuel cell applications, indicating that doping with a single transition metal is not as effective as doping with two transition metals at the same time in regulating the catalyst particle size, activity, etc.
[0173] Fig.11 The XRD pattern of the catalyst provided for Comparative Example 2, Fig.12 The ORR forward scanning polarization curve of the catalyst provided in Comparative Example 2 is as follows: Fig.12 It can be seen that when the catalyst is not doped with non-metallic atoms, its particle size is too large and is not suitable for actual fuel cells; in the RDE performance test, the ORR half-wave potential of Control Example 2 is 0.92 V, and the performance is poor.
[0174] Fig.13 The XRD pattern of the catalyst provided for Comparative Example 3, Fig.14 The ORR forward scanning polarization curve of the catalyst provided in Comparative Example 3 is as follows: Figure 3 It can be seen that without the coordinated coordination of non-metal atoms, Pt, M1 and M2, the particle size of the active particles in the catalyst will be too large, the half-wave potential will be significantly reduced, the ORR stability of the catalyst will be reduced, and actual fuel cell applications will be impossible.
[0175] Table 2 shows the stability and catalytic activity of the catalysts provided by Examples 1-12 and Comparative Examples 1-6.
[0176] Table 2
[0177]
[0178]
[0179] Depend on Figure 1-Figure 13 And Table 1-Table 2 can be obtained:
[0180] The ternary platinum-based alloy catalyst provided by the present invention has a special synergistic effect on Pt, M1 and M2 through non-metallic atoms (N and / or P), which inhibits the migration and agglomeration of nanoparticles (active particles) during heat treatment, obtains nanoparticles with small particle size, and at the same time improves the stability and catalytic activity of the catalyst.
[0181] It can be seen from the data results of Example 1 and Example 8 that the doping of non-metal atoms into the active particles is not conducive to the formation of the alloy phase, and the ORR activity stability will decrease.
[0182] From the data results of Examples 1 and 9-10, it can be seen that in the ternary platinum-based alloy catalyst, the mass proportions of the various substances cooperate with each other. If they are too large or too small, it will lead to crystal phase mismatch, and the M1M2 metal will dissolve during the ORR process, thereby reducing stability.
[0183] From the data results of Example 1 and Examples 11-12, it can be seen that the secondary heat treatment after thermal reduction has the effect of partially oxidizing the surface coating layer of the PtM1M2 nanoparticles. If the temperature of the secondary heat treatment is too low, it will affect the insufficient oxidation of the coating layer, reduce the mass transfer of oxygen, and reduce the ORR activity. If the temperature is too high, the carbon carrier will be oxidized.
[0184] From the data results of Example 1 and Comparative Examples 1-6, it can be seen that in the present invention, non-metal atoms (N and / or P), Pt, M1 and M2 must cooperate with each other and none of them can be missing to achieve high ORR catalytic stability; the lack of any one of the substances cannot solve the deactivation problem of the cathode catalyst of the hydrogen fuel cell.
[0185] In summary, in the ternary platinum-based alloy catalyst provided by the present invention, non-metallic atoms (N and / or P) have a special synergistic effect on Pt, M1 and M2, and the incorporation of N / P does not reduce the amount of Pt used; on the one hand, the migration and agglomeration of nanoparticles (active particles) during the heat treatment process are suppressed to obtain nanoparticles with small particle size; on the other hand, the 3d electron orbits of the N and P elements match the outermost electron orbit of Pt, which can produce specific electron interactions, change the electronic structure of Pt, and improve the oxygen reduction reaction (ORR reaction) activity. At the same time, due to the coordination effect of N and P on Pt, M1 and M2, Pt, M1 and M2 atoms can be anchored, which inhibits the migration of atoms during the ORR process, improves the stability of the ORR reaction, and the active particles are evenly dispersed on the carrier surface, thereby greatly improving the activity and stability of the catalyst in the cathode of the fuel cell.
[0186] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A ternary platinum-based alloy catalyst, characterized in that: The ternary platinum-based alloy catalyst comprises a carrier and active particles supported in the carrier; The ternary platinum-based alloy catalyst is doped with non-metallic atoms, and the non-metallic atoms include N atoms and / or P atoms; the active particles include a ternary platinum-based alloy material, and the constituent elements of the ternary platinum-based alloy material include Pt, M1 and M2, and M1 and M2 are different non-precious metal elements.
2. The ternary platinum-based alloy catalyst according to claim 1, characterized in that: The non-metal atoms are doped on the surface of the carrier and / or in the active particles, preferably on the surface of the carrier; Preferably, the mass proportion of the non-metallic atoms in the ternary platinum-based alloy catalyst is 0.1 to 5 wt%, preferably 0.5 to 1 wt%; Preferably, the support comprises a carbon support.
3. The ternary platinum-based alloy catalyst according to claim 1 or 2, characterized in that: The mass proportion of Pt in the ternary platinum-based alloy catalyst is 10-50wt%, preferably 25-35wt%; Preferably, the mass proportion of M1 in the ternary platinum-based alloy catalyst is 3-20wt%, preferably 6-8wt%; Preferably, the M1 includes any one or a combination of at least two of Mn, Fe, Co, Ni, Cu or Zn; Preferably, the mass proportion of M2 in the ternary platinum-based alloy catalyst is 3-20wt%, preferably 3-4wt%; Preferably, the M2 includes any one of Mn, Fe, Co, Ni, Cu or Zn, or a combination of at least two thereof.
4. The ternary platinum-based alloy catalyst according to any one of claims 1 to 3, characterized in that: The average particle size of the active particles is 2 to 8 nm, preferably 2.5 to 4.5 nm.
5. A method for preparing a ternary platinum-based alloy catalyst as claimed in any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: Mixing a Pt precursor, an M1 precursor, an M2 precursor, a carrier and a first solvent to obtain a mixture, and thermally reducing the mixture to obtain the ternary platinum-based alloy catalyst; Wherein, non-metallic atoms are doped during the mixing process or in the carrier, and the non-metallic atoms include N atoms and / or P atoms.
6. The preparation method according to claim 5, characterized in that: The method for doping the carrier with non-metal atoms comprises: A doping precursor and a carrier are mixed to obtain a carrier mixture, and a heat treatment is performed to obtain a carrier doped with non-metal atoms, wherein the doping precursor includes an N-containing doping precursor and / or a P-containing doping precursor; Preferably, the doping precursor comprises a gaseous doping precursor and / or a non-gaseous doping precursor; Preferably, the doping precursor comprises a non-gaseous doping precursor, and the carrier mixture further comprises a second solvent; Preferably, the support comprises a carbon support; Preferably, the mass ratio of the doping precursor to the carrier is 1:1.5 to 1:4.5; Preferably, the carrier mixture is subjected to a heat treatment after being dried by rotary evaporation; Preferably, the N-doped precursor comprises any one of aniline, polyaniline, melamine or ammonia or a combination of at least two thereof; the P-doped precursor comprises any one of phytic acid, hypophosphite or tetraphenylphosphine chloride or a combination of at least two thereof; Preferably, the atmosphere of the primary heat treatment comprises a protective atmosphere, and the temperature of the primary heat treatment is 700-900°C.
7. The preparation method according to claim 5 or 6, characterized in that: The mixture is rotary evaporated to dryness and then subjected to thermal reduction treatment; Preferably, the thermal reduction is carried out under a reducing atmosphere; Preferably, the temperature of the thermal reduction is 500-1000°C; Preferably, the thermal reduction time is 1 to 10 hours, preferably 6 to 8 hours.
8. The preparation method according to any one of claims 5 to 7, characterized in that: performing secondary heat treatment on the thermally reduced product; Preferably, the secondary heat treatment is carried out in an air atmosphere; Preferably, the temperature of the secondary heat treatment is 100-250°C; Preferably, the product after the secondary heat treatment is subjected to acid washing, solid-liquid separation and drying; Preferably, the dried product is subjected to three heat treatments; Preferably, the pickling temperature is 40 to 80°C; Preferably, the pickling time is 1 to 2 hours.
9. The preparation method according to any one of claims 5 to 8, characterized in that: The preparation method comprises the following steps: The doping precursor, the carrier and the second solvent are mixed to obtain a carrier mixture, which is dried by rotary evaporation and subjected to a heat treatment under a protective atmosphere to obtain a carrier doped with non-metallic atoms; A Pt precursor, an M1 precursor, an M2 precursor, a carrier and a first solvent are mixed to obtain a mixture, the mixture is dried by rotary evaporation, and thermally reduced at 500 to 1000° C. for 1 to 10 hours in a reducing atmosphere, and the thermally reduced product is subjected to a secondary heat treatment at 100 to 250° C. in an air atmosphere, acid-washed, solid-liquid separated and dried, and thermally treated three times to obtain the ternary platinum-based alloy catalyst; Wherein, the doping precursor includes an N-containing doping precursor and / or a P-containing doping precursor.
10. Use of a ternary platinum-based alloy catalyst as claimed in any one of claims 1 to 4, characterized in that: The use includes using the ternary platinum-based alloy catalyst in a fuel cell.
Citation Information
Cited By
Preparation method of doped carbon-based nano noble metal catalyst
CN119926473A
Preparation method of doped carbon-based nano noble metal catalyst
CN119926473B
Post-treatment method of carbon-supported platinum-based catalyst
CN120033264A
ORR catalyst of fuel cell, preparation method of ORR catalyst, membrane electrode and fuel cell
CN121528937A