A high performance magnesium aluminum alloy bar extrusion method and die

By adopting a method of combining multiple extrusion deformations and upsetting deformations during the metal extrusion forming process, and utilizing the interaction of forward and back pressures of a special die structure, the problems of uneven flow and uneven mechanical properties of metal bars are solved. , achieving high-performance forming of metal rods and resource saving.

CN118699111BActive Publication Date: 2024-10-29ZHONGBEI UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411196114.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-10-29
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

During the metal extrusion forming process, the uneven flow of metal rods leads to anisotropy, coarse grains and uneven mechanical properties, which limits its wide application.

Method used

Using a method of combining multiple extrusion deformations and upsetting deformations, by designing a special extrusion die structure, including a feed cavity, a first extrusion cavity, a back pressure cavity and a second extrusion cavity, the forward extrusion and The back pressure interacts to achieve multiple refinements and uniform forming of metal materials.

Benefits of technology

Effectively refine the grains of metal rods, improve their mechanical properties and forming uniformity, reduce forming force, achieve short processes, large deformation and resource saving.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118699111B_ABST
    Figure CN118699111B_ABST
Patent Text Reader

Abstract

The invention discloses an extrusion method and die for high-performance magnesium-aluminum alloy bars, comprising a male die and a female die, wherein the female die coaxially forms a feed cavity, a first extrusion cavity, a back pressure cavity, a second extrusion cavity and a discharge cavity from top to bottom along the axis direction; the feed cavity is for blank placement and male die insertion; the bottom side of the feed cavity is inwardly contracted to the first extrusion cavity, and the bottom opening of the feed cavity extends downward to form the first extrusion cavity; the middle part of the back pressure cavity is transversely protruding, inwardly contracted upwardly to connect to the first extrusion cavity, inwardly contracted downwardly to connect to the second extrusion cavity, and the bottom side of the second extrusion cavity is downwardly connected to the discharge cavity; the cross section of the first extrusion cavity is larger than the cross section at the bottom opening of the back pressure cavity, and the extrusion method comprises: S1: casting rod feeding; S2: uniform heating of the blank; S3: the blank is extruded into the first extrusion cavity for extrusion; S4: the blank is upset in the back pressure cavity; S5: the blank is extruded into the second extrusion cavity for extrusion; S6: the formed workpiece is taken out. The invention causes the metal to produce severe plastic deformation and improves the metal performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal plastic processing technology and forming technology, and in particular to an extrusion method and a die for a high-performance magnesium-aluminum alloy bar. Background Art

[0002] Plastic deformation technology can regulate the structure and properties of alloys by introducing a large amount of strain. Extrusion deformation can significantly improve the plastic forming ability due to its strong three-dimensional compressive stress. The industrial application of extrusion deformation is mature and has become the main forming method for preparing light alloy and other metal material bars. However, there is uneven flow of metal bars during the extrusion deformation process, which will lead to significant anisotropy of metal bars, coarse grains in the middle, and uneven mechanical properties, which in turn limits its wide application. Figure 1 It is a schematic diagram of the structure of a conventional forward extrusion die, comprising a conventional male die 1' and a conventional female die 2', wherein a conventional cavity 3' is formed in the conventional female die 2'.

[0003] In order to solve the above technical problems, improve the performance of metal bars and make them more widely used, other processing technologies, such as cyclic upsetting and rotary reverse extrusion, are added on the basis of the extrusion severe plastic deformation technology of superimposing tensile, compressive and shear strains in the extrusion process. The above technologies show attractive application prospects and development potential in reducing extrusion forming force, increasing deformation amount and uniformity, and realizing complex-shaped parts.

[0004] Among them, back pressure forming technology utilizes the characteristics of plastic deformation and metal flow laws to exert a force opposite to the material flow direction on the material to regulate the material flow in different parts of the part, so as to achieve the purpose of controlling the plastic flow law of the metal material, and finally make the material accurately fill the cavity, thereby achieving the goal of short process, large deformation, low forming force, and saving resource consumption. It is a more advanced forming technology that meets actual production needs.

[0005] In view of this, this case arises. Summary of the invention

[0006] The purpose of the present invention is to provide an extrusion method and a die for high-performance magnesium-aluminum alloy rods, and the technical problem to be solved is to combine multiple extrusion deformation and upsetting deformation on the rods in one process, refine the rod grains multiple times, and improve the performance of the rods.

[0007] To achieve the above-mentioned purpose, the solution of the present invention is: an extrusion die for a high-performance magnesium-aluminum alloy bar, comprising a male die and a female die, wherein the female die is formed with a cavity which is through from top to bottom, and a feed cavity, a first extrusion cavity, a back pressure cavity, a second extrusion cavity and a discharge cavity are coaxially formed in sequence from top to bottom along the axis direction of the cavity;

[0008] The feed cavity is for the blank to be placed and the punch to be inserted downward, the blank fills the feed cavity laterally, the punch is located directly above the feed cavity, and moves up and down to press the blank downward when inserted into the feed cavity, or to rise to move away from the die;

[0009] The bottom side of the feed cavity is inwardly contracted and connected to the top side of the first extrusion cavity, so as to allow the blank to be extruded downward into the first extrusion cavity. The bottom opening of the feed cavity vertically extends downward to form the first extrusion cavity, and the cross-sections of the first extrusion cavity are equal at all locations.

[0010] The middle part of the back pressure cavity is laterally protruding, and is contracted upwards and connected to the bottom side of the first extrusion cavity, and is contracted downwards and connected to the top side of the second extrusion cavity. The bottom side of the second extrusion cavity is downwardly connected to the discharge cavity, and the discharge cavity is used for blank molding and discharge;

[0011] The cross section of the first extrusion cavity is larger than the cross section of the bottom opening of the back pressure cavity.

[0012] Furthermore, the cross-section of the cavity is circular at all locations.

[0013] Furthermore, a feeding section and an extrusion section are formed in the feeding cavity from top to bottom in sequence, the feeding section is cylindrical, and the extrusion section is an inverted truncated cone with a larger upper portion and a smaller lower portion.

[0014] Furthermore, the back pressure chamber forms a first back pressure section, a second back pressure section and a third back pressure section from top to bottom, the first back pressure section extends upwardly inclined to the bottom side of the first extrusion chamber, the third back pressure section extends downwardly inclined to the top side of the second extrusion chamber, and the second back pressure section is respectively connected to the bottom side of the first back pressure section and the top side of the third back pressure section.

[0015] Furthermore, the diameter of the feed section of the feed chamber is D, the diameter of the first extrusion chamber is d1, the maximum diameter of the cross section of the back pressure chamber is d2, and the diameter of the top inlet of the second extrusion chamber is d3, wherein:

[0016] ;

[0017] ;

[0018] .

[0019] Furthermore, the second extrusion cavity is in the shape of a right truncated cone with a small top and a large bottom, and the diameter of the opening at the bottom side of the second extrusion cavity is , the bottom opening of the second extrusion cavity extends downward to form the above-mentioned discharge cavity, wherein:

[0020] .

[0021] Furthermore, the outer contour of the punch is consistent with the inner contour of the feed cavity in shape and size.

[0022] The present invention also provides a method for extruding a high-performance magnesium-aluminum alloy bar, using the above-mentioned die, the extrusion method comprises the following steps:

[0023] S1: unloading of cast bars;

[0024] S2: homogenizing and heating each blank;

[0025] S3: First extrusion: firstly, the billet after homogenization and heating treatment is placed in the feed cavity, and the punch is inserted downward into the feed cavity to push the billet downward along the bottom wall of the feed cavity into the first extrusion cavity, and perform the first extrusion deformation;

[0026] S4: Upsetting: The punch is continuously inserted into the feed cavity to push the blank, so that the blank passes through the first extrusion cavity and enters the back pressure cavity. The blank moves downward along its axis, abuts against the bottom wall of the back pressure cavity and flows freely, and then gradually fills the back pressure cavity laterally to be upsettingly deformed. Part of the blank is squeezed into the second extrusion cavity along the opening on the bottom side of the back pressure cavity to perform the second extrusion deformation;

[0027] S5: Second extrusion: The blank completely fills the back pressure cavity, and the punch continues to move downward to push the blank downward, so that the blank in the back pressure cavity is sequentially squeezed downward into the second extrusion cavity, undergoes a second extrusion deformation, and then enters the discharge cavity;

[0028] S6: Unloading: Take out the formed workpiece.

[0029] After adopting the above scheme, the beneficial effects of the present invention are: the blank fills the feed cavity horizontally, the punch is inserted into the feed cavity downward, the blank is pushed downward, and the bottom wall of the feed cavity shrinks downward, so that when the blank is squeezed into the first extrusion cavity, the cross-sectional area is reduced, and the blank is squeezed to refine the grains; after the blank enters the back pressure cavity, since the cross section of the first extrusion cavity is larger than the cross section of the opening at the bottom side of the back pressure cavity, the blank can resist the bottom wall of the back pressure cavity and is subjected to the back pressure opposite to its flow direction, and free flow occurs. As the feed amount increases, the blank continues to expand outward and is filled with upsetting and deformed in the back pressure cavity. Under the action of the positive extrusion pressure and the back pressure, the grains are further refined. The blank is squeezed into the second extrusion cavity, extruded and deformed again, and the grains are refined again. The blank is subjected to the alternating action of secondary extrusion deformation and upsetting deformation, and the grains of the blank are refined multiple times, the stress inside the blank is uniform, and the performance of the blank is enhanced. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the punch and die structure of traditional forward extrusion.

[0031] Figure 2 It is a schematic diagram of the male and female mold structures of the present invention.

[0032] Figure 3 It is a schematic diagram of the blank entering the feeding cavity during the first blank feeding process of the present invention.

[0033] Figure 4 It is a schematic diagram of the blank of the present invention entering the back pressure chamber after the first extrusion.

[0034] Figure 5 It is a schematic diagram of the blank of the present invention being pushed into the back pressure cavity by the punch and abutting against the bottom wall of the back pressure cavity.

[0035] Figure 6 It is a schematic diagram of the blank of the present invention being pushed into the back pressure cavity by the punch and undergoing upsetting deformation.

[0036] Figure 7 It is a schematic diagram of the blank of the present invention being completely upsetting and deformed in the back pressure cavity.

[0037] Figure 8 It is a schematic diagram of the second blank feeding of the present invention.

[0038] Fig. 9 It is a schematic diagram of the back pressure generated after the blank of the present invention abuts against the bottom wall of the back pressure cavity.

[0039] Fig.10 It is the equivalent strain distribution diagram of traditional forward extrusion.

[0040] Fig.11 This is the back pressure cavity enhancement equivalent strain distribution diagram of the present invention.

[0041] Fig.12 It is the relationship curve of forward extrusion load and time of traditional forward extrusion.

[0042] Fig.13 It is a curve diagram of the relationship between the back pressure cavity strengthening load and time of the present invention.

[0043] Description of labels:

[0044] 1'-traditional punch, 2'-traditional die, 3'-traditional cavity, 1-punch, 2-die, 3-cavity, 4-feeding cavity, 5-first extrusion cavity, 6-back pressure cavity, 7-second extrusion cavity, 8-discharging cavity, 9-blank, 41-feeding section, 42-extrusion section, 61-first back pressure section, 62-second back pressure section, 63-third back pressure section. DETAILED DESCRIPTION

[0045] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0046] In the claims, specification and the above-mentioned drawings of the present invention, unless otherwise explicitly defined, directional words, such as the use of terms such as "center", "lateral", "longitudinal", "horizontal", "vertical", "top", "bottom", "inside", "outside", "up", "down", "front", "back", "left", "right", "clockwise", "counterclockwise" and the like to indicate directions or positional relationships are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation or be constructed and operated in a specific orientation, so it cannot be understood as limiting the specific protection scope of the present invention.

[0047] The present invention provides an extrusion die for a high-performance magnesium-aluminum alloy bar. Figure 2-Figure 9 As shown, it includes a punch 1 and a die 2, the die 2 is formed with a cavity 3 which passes through from top to bottom, and a feed cavity 4, a first extrusion cavity 5, a back pressure cavity 6, a second extrusion cavity 7 and a discharge cavity 8 are coaxially formed in sequence from top to bottom along the axial direction of the cavity 3; the feed cavity 4 is for the blank 9 to be placed and the punch 1 to be inserted downward, the blank 9 is specifically a large-sized magnesium-aluminum alloy ingot, the blank 9 fills the feed cavity 4 horizontally, the punch 1 is located directly above the feed cavity 4, and is lifted up and down to extrude the blank 9 downward when inserted into the feed cavity 4, or to rise to move away from the die 2; the punch 1 is specifically installed and fixed below the upper template of the press (not shown in the figure), and the die 2 is installed and fixed above the lower worktable of the press (not shown in the figure), and the press drives the upper template of the press to open and close up and down, thereby driving the punch 1 to move upward and downward. The die 1 is inserted into the die 2 or away from the die 2, and the bottom side of the feed cavity 4 is inwardly connected to the top side of the first extrusion cavity 5, so as to allow the blank 9 to be squeezed downward into the first extrusion cavity 5. The bottom opening of the feed cavity 4 extends vertically downward to form the above-mentioned first extrusion cavity 5, and the cross-sections of the first extrusion cavity 5 are equal at all places; the middle part of the back pressure cavity 6 protrudes laterally, and is inwardly connected to the bottom side of the first extrusion cavity 5 upwardly, and is inwardly connected to the top side of the second extrusion cavity 7 downwardly, and the bottom side of the second extrusion cavity 7 is downwardly connected to the discharge cavity 8, and the discharge cavity 8 is used for the blank 9 to be formed and discharged; the cross-section of the first extrusion cavity 5 is larger than the cross-section at the bottom opening of the back pressure cavity 6, so that after the blank 9 is pushed into the back pressure cavity 6 and abuts against the bottom wall of the back pressure cavity 6, it can be subjected to the back pressure and flow freely, thereby realizing upsetting deformation.

[0048] Furthermore, the cross-sections of the cavity 3 are all circular, and the punch 1 is correspondingly cylindrical. Of course, in other embodiments, the cross-section of the cavity 3 can also be square, or other shapes, but is not limited to this, as long as it can ensure that the cross-section of the first extrusion cavity 5 is larger than the cross-section at the bottom opening of the back pressure cavity 6.

[0049] Focus on combination Figure 2A feed section 41 and an extrusion section 42 are formed in the feed cavity 4 from top to bottom. The feed section 41 is cylindrical, and the extrusion section 42 is an inverted truncated cone with a larger upper portion and a smaller lower portion, that is, the extrusion section 42 adopts an inclined surface structure. When the billet 9 descends in the feed cavity 4 and is extruded into the first extrusion cavity 5 along the extrusion section 42, the cross section for the billet 9 to pass through becomes smaller, which causes lateral shearing of the billet 9 and refines the grains of the billet 9. Specifically, the first extrusion cavity 5 is a short stroke, and when the billet 9 enters the first back pressure cavity 6 after passing through the first extrusion cavity 5, radial outward expansion occurs.

[0050] Furthermore, the outer contour of the punch 1 is consistent in shape and size with the inner contour of the feed cavity 4 , and can completely push the blank from the feed section 41 into the extrusion section 42 .

[0051] In this specific embodiment, Figure 2 As shown, the included angle between the extrusion section 42 and the horizontal plane is θ1. Preferably, θ1 is 120 degrees to 130 degrees.

[0052] Focus on combination Figure 3 The back pressure chamber 6 forms a first back pressure section 61, a second back pressure section 62 and a third back pressure section 63 from top to bottom, the first back pressure section 61 extends upwardly and tilted to the bottom side of the first extrusion chamber 5, the third back pressure section 63 extends downwardly and tilted to the top side of the second extrusion chamber 7, the second back pressure section 62 is respectively connected to the bottom side of the first back pressure section 61 and the top side of the third back pressure section 63, that is, the first back pressure section 61 and the third back pressure section 63 are both inclined surfaces, preferably, the angle between the third back pressure section 63 and the horizontal plane is θ2, θ2 is preferably 120 degrees-130 degrees, and the back pressure effect is better.

[0053] The punch 1 pushes the blank 9 downward to generate a positive extrusion force F. The blank 9 enters the back pressure cavity 6, moves downward along the axis of the cavity 3, and abuts against the third back pressure section 63. The blank 9 flows freely. As the amount of blank 9 fed increases, the back pressure F generated by the third back pressure section 63 on the blank 9 increases. b , the focus here is on combining Fig. 9 , F b is the back pressure, back pressure F b The direction is opposite to the flow direction of the blank 9, and F1 and F2 are back pressure F b The decomposition force changes the flow direction of the metal material at the edge and core of the billet, continuously filling the back pressure cavity 6 (such as Figure 6As shown in the figure, the blank 9 is continuously expanded and upset in the back pressure cavity 6. When the blank 9 abuts against the first back pressure section 61, the first back pressure section 61 also squeezes the blank 9. The first back pressure section 61 and the third back pressure section 63 produce differential pressure extrusion. In addition, the blank 9 in the back pressure cavity 6 is also subjected to the positive extrusion force F. The multiple forces interact in different directions, and produce isotropic shearing effects on the blank 9, continuously refining the grains. As the blank 9 continuously fills the back pressure cavity 6, the blank 9 gradually enters a steady flow state. Here, the focus is on Figure 10-11 Compared with the traditional forward extrusion, it can be seen that when the blank 9 is filled in the back pressure cavity 6, the equivalent stress is approximately uniformly distributed, resulting in severe plastic deformation and significantly improved grain refinement. Fig.13 At the beginning of the process when the blank 9 enters the back pressure chamber 6, the strengthening load in the back pressure chamber 6 increases rapidly with time, and then enters a gentle state. Fig.12 ,Compared with the traditional forward extrusion, the maximum load required by the back pressure cavity 6 is smaller than the forward extrusion deformation.

[0054] Focus on combination Figure 6-8 The blank 9 is pushed into the back pressure chamber 6. Most of the blank 9 is squeezed into the top opening of the second extrusion chamber 7 after being upset in the back pressure chamber 6 for a second extrusion, which produces transverse shear again and refines the grains. The second extrusion chamber 7 is a right truncated cone with a small top and a large bottom. The bottom of the second extrusion chamber 7 extends downward to form the above-mentioned discharge chamber 8. The second extrusion chamber 7 is also set with a short stroke, which can quickly enter the discharge chamber 8. The focus is on Fig.10 In the discharge cavity 8 , the equivalent strain of the blank 8 is significantly increased, and the axial elongation of the blank 9 is achieved.

[0055] Preferably, the bottom opening diameter of the second extrusion cavity 7 is ,in:

[0056] .

[0057] Preferably, the diameter of the feed section 41 of the feed chamber 4 is D, the diameter of the first extrusion chamber 5 is d1, the maximum diameter of the cross section of the back pressure chamber 6 is d2, and the diameter of the top entrance of the second extrusion chamber 7 is d3, wherein:

[0058] ;

[0059] ;

[0060] .

[0061] The present invention combines multiple extrusion deformation and upsetting deformation in the same process to refine the grains multiple times, so that large-sized metal materials undergo severe plastic deformation. The process is short, the amount of metal deformation can be regulated, the grain refinement is significantly improved, the toughness of the metal material is improved, and the mold structure is simple.

[0062] The present invention also provides a method for extruding a high-performance magnesium-aluminum alloy bar, using the above-mentioned die, the extrusion method comprises the following steps:

[0063] S1: unloading of cast bars;

[0064] S2: homogenizing and heating each blank 9;

[0065] S3: First squeeze: Focus on combining Figure 3 and Figure 4 As shown, the blank 9 after homogenization and heating treatment is first placed in the feed cavity 4, and the punch 1 is inserted downward into the feed cavity 4 to push the blank 9 downward along the bottom wall of the feed cavity 4 into the first extrusion cavity 5 to perform the first extrusion deformation;

[0066] S4: Upsetting: Focus on Combination Figure 5 and Figure 6 As shown, the punch 1 is continuously inserted into the feed cavity 4 to push the blank 9, so that the blank 9 passes through the first extrusion cavity 5 and enters the back pressure cavity 6, and the blank 9 moves downward along its axial direction, abuts against the bottom wall of the back pressure cavity 6 and flows freely, and then gradually fills the back pressure cavity 6 laterally and is upsetting and deformed, and part of the blank 9 is squeezed into the second extrusion cavity 7 along the bottom opening of the back pressure cavity 6 to undergo a second extrusion deformation;

[0067] S5: Second squeeze, focus on combination Figure 7 and Figure 8 As shown: the blank 9 completely fills the back pressure cavity 6, and the punch 1 continues to move downward to push the blank 9 downward, so that the blank in the back pressure cavity 6 is sequentially squeezed downward into the second extrusion cavity 7, undergoes a second extrusion deformation, and then enters the discharge cavity 8;

[0068] S6: Unloading: Take out the formed workpiece.

[0069] The above description is only a preferred embodiment of the present invention and is not a limitation on the design of this case. Any equivalent changes made based on the design key of this case shall fall within the protection scope of this case.

Claims

1. An extrusion die for high-performance magnesium-aluminum alloy bars, characterized in that: The die comprises a male die (1) and a female die (2), wherein the female die (2) is formed with a cavity (3) which is connected from top to bottom, and a feed cavity (4), a first extrusion cavity (5), a back pressure cavity (6), a second extrusion cavity (7) and a discharge cavity (8) are coaxially formed in sequence from top to bottom along the axial direction of the cavity (3); The feed cavity (4) is for the blank (9) to be placed and the punch (1) to be inserted downwardly, the blank (9) fills the feed cavity (4) laterally, the punch (1) is located directly above the feed cavity (4) and is moved up and down to press the blank (9) downward when inserted into the feed cavity (4), or to rise to move away from the die (2); The bottom side of the feed cavity (4) is inwardly contracted and connected to the top side of the first extrusion cavity (5) so as to allow the blank (9) to be extruded downward into the first extrusion cavity (5). The bottom opening of the feed cavity (4) vertically extends downward to form the first extrusion cavity (5). The cross-sections of the first extrusion cavity (5) are equal at all locations. The middle part of the back pressure chamber (6) is laterally protruding and is retracted upwards to be connected to the bottom side of the first extrusion chamber (5), and is retracted downwards to be connected to the top side of the second extrusion chamber (7). The bottom side of the second extrusion chamber (7) is downwardly connected to the discharge chamber (8), and the discharge chamber (8) is used for forming and discharging the blank (9); The cross section of the first extrusion chamber (5) is larger than the cross section of the bottom opening of the back pressure chamber (6).

2. The extrusion die for high performance magnesium aluminum alloy bars according to claim 1, characterized in that: The cross-section of the cavity (3) is circular at all locations.

3. The extrusion die for high performance magnesium aluminum alloy bars according to claim 2, characterized in that: The feed cavity (4) has a feed section (41) and an extrusion section (42) formed in sequence from top to bottom. The feed section (41) is cylindrical, and the extrusion section (42) is an inverted truncated cone that is larger at the top and smaller at the bottom.

4. The extrusion die for high performance magnesium aluminum alloy bars according to claim 2, characterized in that: The back pressure chamber (6) is formed into a first back pressure section (61), a second back pressure section (62) and a third back pressure section (63) from top to bottom, the first back pressure section (61) extends upwardly and tilted to the bottom side of the first extrusion chamber (5), the third back pressure section (63) extends downwardly and tilted to the top side of the second extrusion chamber (7), and the second back pressure section (62) is connected to the bottom side of the first back pressure section (61) and the top side of the third back pressure section (63) respectively.

5. The extrusion die for high performance magnesium aluminum alloy bars according to claim 2, characterized in that: The diameter of the feed section (41) of the feed chamber (4) is D, the diameter of the first extrusion chamber (5) is d1, the maximum diameter of the cross section of the back pressure chamber (6) is d2, and the diameter of the top inlet of the second extrusion chamber (7) is d3, wherein: ; ; 。 6. The extrusion die for high performance magnesium aluminum alloy bars according to claim 2, characterized in that: The second extrusion cavity (7) is in the shape of a right truncated cone that is smaller at the top and larger at the bottom. The diameter of the bottom opening of the second extrusion cavity (7) is The bottom opening of the second extrusion chamber (7) extends downward to form the above-mentioned discharge chamber (8), wherein: 。 7. The extrusion die for high performance magnesium aluminum alloy rod according to claim 1, characterized in that: The outer contour of the male mold (1) is consistent in shape and size with the inner contour of the feed cavity (4).

8. A method for extruding a high-performance magnesium-aluminum alloy bar, using the die of any one of claims 1 to 7, characterized in that: The extrusion method comprises the following steps: S1: unloading of cast bars; S2: homogenizing and heating each blank (9); S3: first extrusion: firstly, the blank (9) after homogenization and heating treatment is placed in the feed cavity (4), and the punch (1) is inserted downward into the feed cavity (4) to push the blank (9) downward along the bottom wall of the feed cavity (4) into the first extrusion cavity (5), and perform the first extrusion deformation; S4: upsetting: the punch (1) is continuously inserted into the feed cavity (4) to push the blank (9), so that the blank (9) passes through the first extrusion cavity (5) and enters the back pressure cavity (6), the blank (9) moves downward along its axial direction, abuts against the bottom wall of the back pressure cavity (6) and flows freely, and then gradually fills the back pressure cavity (6) laterally to be upset and deformed, and part of the blank (9) is squeezed into the second extrusion cavity (7) along the bottom opening of the back pressure cavity (6) to undergo a second extrusion deformation; S5: Second extrusion: the blank (9) completely fills the back pressure cavity (6), the punch (1) continues to move downward to push the blank (9) downward, so that the blank in the back pressure cavity (6) is sequentially squeezed downward into the second extrusion cavity (7), undergoes a second extrusion deformation, and then enters the discharge cavity (8); S6: Unloading: Take out the formed workpiece.

Citation Information

Patent Citations

  • Differential velocity cyclic extrusion forming method for high performance rare earth magnesium alloy billet

    CN109909411A

  • High-performance magnesium-aluminum alloy variable cross-section extrusion-twisting combined machining device and preparation process thereof

    CN113560362A