A high-adhesion solvent-resistant adhesive and preparation method thereof, polyimide composite film and screen printing screen

By rationally formulating agent A and agent B in the adhesive, combined with the use of fillers, the problems of poor adhesiveness and insufficient solvent resistance are solved, high adhesion and solvent resistance are improved, and screen printing screen version is extended The service life and improve the stability of photovoltaic cells.

CN118703148BActive Publication Date: 2024-11-05KUNSHAN LEBANG PRECISION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411197988.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-05
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The existing adhesives have poor adhesiveness during screen printing, which leads to the peeling of latex and screens during metallization of photovoltaic cells, reducing the life of the screen printing screen and the performance stability of the photovoltaic cells, making it difficult to have both. High adhesion and solvent resistance.

Method used

Using a high adhesion and solvent-resistant adhesive, the curing rate and stress release are adjusted by adding epoxy resin, filler and active diluent to agent A and phenylsilane coupling agent to agent B. , combined with the addition of filler, the modulus and cross-linking density of the adhesive are increased, and solvent penetration is reduced.

Benefits of technology

It improves the adhesion and solvent resistance of the adhesive, reduces stress concentration, extends the service life of the screen printing screen, and improves the performance stability of photovoltaic cells.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present application relates to a high-adhesion solvent-resistant adhesive and a preparation method thereof, a polyimide composite film and a screen printing screen. The high-adhesion solvent-resistant adhesive comprises the following raw materials in parts by weight: comprising agent A and agent B, wherein agent A comprises the following raw materials in parts by weight: 25-40 parts of epoxy resin, 5-10 parts of filler, and 5-8 parts of active diluent; agent B comprises the following raw materials in parts by weight: 18-30 parts of phenyl silane coupling agent-modified porous calcium carbonate loaded curing agent, 3-8 parts of filler, and 1-3 parts of active diluent. The high-adhesion solvent-resistant adhesive in this application has high adhesion and solvent resistance, and is particularly suitable for bonding polyimide film and metal mesh to prepare screen printing screens.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to an adhesive, and more specifically, to a high-adhesion solvent-resistant adhesive and a preparation method thereof, a polyimide composite film and a screen printing screen. Background Art

[0002] With people's attention to clean energy, photovoltaic cells are developing rapidly. The metallization process of photovoltaic cells usually uses screen printing technology to form the positive and negative electrodes of the battery. The screen printing screen is generally made of polyester mesh, steel mesh, polyimide film, etc., which are bonded layer by layer by hot melt adhesive. The printing process is to use a scraper to apply pressure on the slurry end of the screen and move toward the other end of the screen, so that the conductive slurry containing metal is squeezed from the mesh to the substrate. However, the surface of the steel mesh and polyimide film is relatively smooth and has poor adhesion. The bonding point of the steel mesh and the polyimide film is prone to adhesion failure after soaking in slurry and repeated scraping with a scraper, causing the latex to peel off from the screen, and it is very easy to explode, reducing the life of the screen printing screen and the performance stability of the photovoltaic cell. Therefore, it is very important to provide an adhesive with high adhesion and solvent resistance. However, generally speaking, improving solvent resistance is achieved by introducing solvent-resistant segments, which are often low-polarity groups, so they will reduce the adhesion of the resin. Improving the solvent resistance of the adhesive by adding fillers generally requires adding more mass to have a better solvent resistance effect, but this will reduce the adhesion of the adhesive. Therefore, it is very challenging to prepare an adhesive with both high adhesion and solvent resistance. Summary of the invention

[0003] In order to solve the problem of high adhesion and solvent resistance of adhesives, the present application provides a high adhesion and solvent resistance adhesive and a preparation method thereof, a polyimide composite film and a screen printing screen.

[0004] In the first aspect, the present application provides a high-adhesion solvent-resistant adhesive comprising agent A and agent B in a mass ratio of 1:1, wherein agent A comprises the following raw materials in mass parts: 25-40 parts of epoxy resin, 5-10 parts of filler, and 5-8 parts of active diluent; agent B comprises the following raw materials in mass parts: 18-30 parts of phenyl silane coupling agent modified porous calcium carbonate loaded curing agent, 3-8 parts of filler, and 1-3 parts of active diluent.

[0005] By adopting the above scheme, the epoxy resin has high bonding strength and adhesion effect, and the prepared adhesive has high strength and good adhesion effect. By adding a certain mass of active diluent, the adhesive can better penetrate into the rough micro-gaps on the surface of the polyimide film and the metal mesh of the screen printing screen, and also make the internal components of the adhesive more uniform, reducing the mixing time; by adding a certain mass of silane coupling agent and active diluent to agent B, the curing rate can be adjusted, and the stress can be better released during the curing process, and the internal stress of the prepared adhesive is more uniform, the prepared adhesive has fewer internal defects, and the solvent is not easy to penetrate. By adding a certain mass of phenylsilane coupling agent to modify the porous calcium carbonate loaded curing agent, the calcium carbonate blocks the invasion of the solvent and increases the modulus of the adhesive, so that the modulus of the prepared adhesive is closer to the intermediate value of the polyimide film and the metal mesh, and the stress concentration of the bonding interface during the use of the prepared screen printing screen is reduced; by modifying the porous calcium carbonate with phenylsilane, the modified calcium carbonate not only has good compatibility with the adhesive system, but also has good The invention is better, and it may be due to the volume effect of the phenylsilane coupling agent and the electron-withdrawing characteristics of the phenylsilane, which reduces the reaction activity of the epoxy resin, thereby reducing the curing speed, further improving the full wetting of the adhesive on the substrate, releasing the internal stress of the adhesive, and having fewer internal defects and weak interface layers after curing, and having a uniform interface structure, thereby avoiding the generation of stress relaxation and cracks, and preventing the solvent from penetrating easily; the porous calcium carbonate loaded with a slow-release curing agent further reduces the curing speed, and the components of the prepared adhesive are fully infiltrated and cross-linked during the curing process, forming more and more uniform cross-linking points, thereby improving the adhesion of the adhesive, and the formed adhesive layer is dense and uniform, and the solvent is not easy to penetrate, thereby improving the solvent resistance of the prepared adhesive; after the porous calcium carbonate is modified by the phenylsilane coupling agent, on the one hand, the silane coupling agent promotes the dispersion of calcium carbonate, further promotes the full contact between the curing agent and the resin, and increases the cross-linking points, and on the other hand, the active shielding of the benzene ring on the resin chain makes it difficult for the calcium carbonate to agglomerate during the cross-linking process, thereby cross-linking to form an adhesive layer to hinder the intrusion of the solvent, and uniformly releasing the curing agent to improve the curing effect. Silane coupling agent further enhances the interaction between molecules, improves the modulus and density of the adhesive, and improves structural stability. Therefore, under the internal stable structure, the solvent is not easy to damage the adhesive structure. The addition of filler improves the modulus of the adhesive, and the addition of rigid group benzene ring further improves the modulus. The modulus of the prepared adhesive is not too high to affect adhesion, nor is it too low to cause stress concentration when bonding high modulus polyimide film and screen printing screen. It is more suitable for bonding polyimide film and metal mesh in screen printing screen.

[0006] In a specific embodiment, the preparation steps of the phenylsilane coupling agent modified porous calcium carbonate loaded curing agent include:

[0007] S1: adding porous calcium carbonate and phenylsilane coupling agent to ethanol aqueous solution, stirring evenly, ultrasonic treatment, reaction, reduced pressure distillation, suction filtration, washing, vacuum drying, to obtain phenylsilane coupling agent modified porous calcium carbonate;

[0008] S2: slowly stirring the curing agent and the porous calcium carbonate modified by the phenylsilane coupling agent evenly, and evacuating to negative pressure to obtain the phenylsilane coupling agent modified porous calcium carbonate loaded with the curing agent.

[0009] By adopting the above scheme, the preparation steps are relatively simple, the yield of the prepared phenylsilane coupling agent modified porous calcium carbonate is high, the agglomeration of porous calcium carbonate is reduced, and its compatibility with the adhesive is improved. The phenylsilane coupling agent modified porous calcium carbonate loaded curing agent is uniformly present in the adhesive, the cross-linking network density is improved, and the infiltration of solvent is reduced. The steric hindrance of the benzene ring further reduces the infiltration of the solvent, and the stable cross-linking network reduces the damage of the infiltrated solvent to the adhesive structure. Under this preparation step, the phenyl group and the porous calcium carbonate are more evenly combined, the steric hindrance reduces the curing speed of the adhesive, the stress of the prepared adhesive is more fully released, and the internal structural defects are less. The prepared phenylsilane coupling agent modified porous calcium carbonate has a good effect on improving the modulus of the adhesive, and reduces the stress concentration of the adhesive between the polyimide film and the metal mesh in the screen printing screen.

[0010] In a specific embodiment, the curing agent has an amine value of 120-200 mg KOH / g and a weight average molecular weight of 500-950 g / mol.

[0011] By adopting the above scheme, the amine value of the curing agent will not be too high, and the weight-average molecular weight is small, the viscosity is low, and the fluidity of the obtained adhesive is better. By limiting the amine value, the curing speed is slowed down, the adhesive can release stress better, the stress of the obtained adhesive is uniform, the structure is flatter, the internal defects are less, and the solvent is not easy to penetrate. On the other hand, the amine value will not be too low to seriously affect the efficiency of the curing process.

[0012] In a specific embodiment, the particle size of the porous calcium carbonate is 1-8 um.

[0013] By adopting the above scheme, porous calcium carbonate has a better loading effect on the curing agent, the curing agent has a suitable seepage rate, and the cross-linking density and curing efficiency are taken into account. The prepared adhesive can be well attached to the rough micropores on the substrate, and the modulus of the prepared adhesive is also more suitable.

[0014] In a specific embodiment, the filler in agent A is flaky aluminum oxide I modified by an epoxy silane coupling agent, and the filler in agent B is flaky aluminum oxide II modified by an amino silane coupling agent.

[0015] By adopting the above scheme, flaky aluminum oxide can make the prepared adhesive more solvent-resistant and have a higher modulus. The addition of flaky aluminum oxide I modified by epoxy silane coupling agent and flaky aluminum oxide II modified by amino silane coupling agent also makes it easy for amino and epoxy groups to bond to form crosslinks when components A and B are mixed. After modification, epoxy and amino silanes participate in curing, making the structure more uniform and tight, improving solvent resistance, and making it difficult for the adhesive structure to swell after solvent invasion, resulting in the destruction of the adhesive structure.

[0016] In a specific embodiment, the average particle size of the flaky aluminum oxide I is 2-10 μm, and the average particle size of the flaky aluminum oxide II is 0.8-1 μm.

[0017] By adopting the above scheme, different particle sizes can more evenly isolate the solvent entry path. The flake aluminum oxide I has a larger particle size and can isolate the intrusion of solvents more efficiently. The flake aluminum oxide II has a smaller particle size and can flow better in the adhesive, interspersed in the gaps of the flake aluminum oxide I to further block the intrusion of solvents. The two flake aluminum oxides of different particle sizes form an orderly arrangement under the action of epoxy and amino groups, thereby greatly improving the solvent resistance of the adhesive layer.

[0018] In a specific embodiment, the mass ratio of the epoxysilane coupling agent modified flaky aluminum oxide I to the aminosilane coupling agent modified flaky aluminum oxide II is (1.1-1.5):1.

[0019] By adopting the above scheme, the solvent can be better isolated from entering, the cross-linking effect is good, the structure will not be destroyed after the solvent enters, and the polar group content in the adhesive is increased to improve adhesion. The epoxy group and the amino group participate in the curing of the adhesive to form a more superior cross-linking effect, and the adhesive achieves better infiltration; the flaky aluminum oxide I and the flaky aluminum oxide II are distributed more evenly in the adhesive, and aluminum oxides of different particle sizes are interspersed, which can better isolate the intrusion of solvents. At the same time, the epoxy-modified epoxysilane coupling agent-modified flaky aluminum oxide I and the aminosilane coupling agent-modified flaky aluminum oxide II are better involved in cross-linking and curing, which, on the one hand, improves the distribution of aluminum oxide in the system, and on the other hand, under the above ratio, the two aluminum oxides achieve better cross-dispersion based on cross-linking, which can further promote the shielding effect of the adhesive layer on solvents.

[0020] In a second aspect, the present application provides a method for preparing a high-adhesion solvent-resistant adhesive, characterized in that it comprises the following steps:

[0021] S1: Preparation of Agent A: Mix the epoxy resin and the active diluent according to the mass ratio, stir evenly, add the remaining components, and stir for 10-25 minutes;

[0022] S2: Preparation of Agent B: Mix the curing agent, silane coupling agent and reactive diluent of Agent B, stir for 5-10 minutes, add the remaining components in two batches, and stir for 15-20 minutes;

[0023] S3: Mix agent A and agent B evenly to obtain a high-adhesion solvent-resistant adhesive.

[0024] By adopting the above scheme, the preparation method is simple, the components are mixed more evenly, and not many bubbles are introduced. The prepared adhesive layer can be more resistant to solvents and has good adhesiveness.

[0025] In a third aspect, the present application provides a polyimide composite film, comprising a polyimide film, an adhesive layer and a metal mesh, wherein the adhesive layer is composed of the above-mentioned adhesive.

[0026] By adopting the above scheme, the adhesive prepared in the present application is prepared by combining various components and adding a certain mass of filler. The modulus of the prepared adhesive is close to the intermediate value between the polyimide film and the metal mesh. The stress is not easy to concentrate during use. At the same time, it has a high adhesion effect and is suitable for use in bonding polyimide films and metal meshes.

[0027] In a fourth aspect, the present application provides a screen printing screen, comprising a frame, a polyester mesh, and a polyimide composite film, wherein the polyimide composite film is the polyimide composite film described in the third aspect above.

[0028] By adopting the above scheme, the polyimide film and the metal mesh are bonded more tightly, the bonding interface has better tolerance to solvents, and the screen printing screen is more stable and less likely to explode during use.

[0029] In summary, this application has the following beneficial effects:

[0030] Compared with the prior art, the present application has a better bonding effect through the coordination and quality setting of each component, and improves the modulus of the adhesive by adding a certain mass of phenyl silane coupling agent to modify the porous calcium carbonate loaded curing agent, thereby improving the crosslinking density and steric hindrance, thereby improving the solvent resistance from two aspects of reducing solvent penetration and reducing structural damage to the adhesive after penetration, and reducing stress concentration by increasing the modulus of the adhesive, so that it is suitable for the bonding of polyimide films and screen printing screens, and reduces the curing speed of the adhesive by increasing steric hindrance and reducing the activity of the epoxy group by electron withdrawal, and performs stress release, so that the obtained adhesive is more uniform and has fewer internal defects, thereby improving the solvent resistance.

[0031] In the present application, an epoxy silane coupling agent is added to agent A to modify flaky aluminum oxide I, and a filler amino silane coupling agent is added to agent B to modify flaky aluminum oxide II. The particle sizes of flaky aluminum oxide I and flaky aluminum oxide II are further limited, and the mass ratio of the epoxy silane coupling agent-modified flaky aluminum oxide I and the amino silane coupling agent-modified flaky aluminum oxide II is limited, so as to further improve the modulus of the adhesive and the solvent barrier effect, and the adhesive is suitable for bonding polyimide film and screen printing metal mesh. DETAILED DESCRIPTION

[0032] To further help understand the technical solution of the present invention, several specific embodiments are provided to describe the technical solution of the present invention in more detail. All the embodiments described are only partial embodiments of the present invention, not all of them; the embodiments can be combined with each other, and the same or similar concepts or processes may not be described in detail in some embodiments. The following embodiments are further explanations of the present invention, and the present invention is not limited thereto.

[0033] The components of the preparation examples used in the examples of this application all refer to the components obtained by the preparation examples. In the examples and comparative examples, the epoxy resin is KMK-42 from KMIK, the curing agent is Wuxi Xihua Chemical Polyamide 650, the active diluent is Lana White XY746, the phenyl silane coupling agent is Hengyu HY23, the cyclohexyl silane coupling agent is Rain Environmental Protection HD-104, the epoxy silane coupling agent is KH-172, the amino silane coupling agent is KH-540, the particle size of flaky aluminum oxide I is 6 μm, the particle size of flaky aluminum oxide II is 1 μm, purchased from Leyide (Shenzhen) Technology Co., Ltd., the polyethylene glycol is PEG 200, and the remaining experimental reagents, unless otherwise specified, are conventional commercial brands or obtained through conventional preparation processes.

[0034] Preparation Example

[0035] The porous calcium carbonate of the present application can be purchased or prepared, and conventional porous calcium carbonate preparation methods can be used to prepare porous calcium carbonate. The present application prepares porous calcium carbonate by using existing porous preparation processes.

[0036] The present invention prepares the silane coupling agent modified filler by conventional hydrolysis and dehydration method.

[0037] Preparation Example 1: Phenylsilane coupling agent modified porous calcium carbonate loaded curing agent:

[0038] Add 10g of silicon dioxide to 200ml of 5%wt sodium citrate solution and stir evenly, add 50g of polyethylene glycol, heat to 80°C, stir evenly, cool to room temperature, add 25g of sodium bicarbonate, adjust the pH to 12 with 20%wt NaOH, add 33g of calcium chloride (CaCl2), ultrasonically disperse for 10min, power 300W, then transfer to a reactor for hydrothermal reaction at 170°C for 6h, centrifuge to remove the supernatant to obtain a solid, heat the obtained solid to 90°C in 1000ml of 5%wt NaOH solution, stir for 3h, centrifuge to remove the supernatant to obtain a precipitate, and wash the obtained precipitate three times with deionized water and ethanol respectively, and dry to obtain porous calcium carbonate.

[0039] 50 g of porous calcium carbonate and 40 g of phenylsilane coupling agent were added to 200 ml of 25% wt ethanol aqueous solution, stirred at 80° C. for 1 hour, ultrasonically treated for 70 minutes, stirred, heated to 80° C., reacted, and distilled under reduced pressure after 20 hours, filtered, washed, and vacuum dried for 24 hours to obtain phenylsilane coupling agent modified porous calcium carbonate.

[0040] 200 g of curing agent was dripped onto 100 g of porous calcium carbonate modified by phenyl silane coupling agent, the mixture was slowly stirred at 100 rpm, and vacuum was evacuated to a negative pressure of -0.10 MPa to obtain a phenyl silane coupling agent modified porous calcium carbonate loaded with a curing agent.

[0041] Preparation Example 2: Cyclohexylsilane coupling agent modified porous calcium carbonate loaded curing agent:

[0042] Add 10g of silicon dioxide to 200ml of 5%wt sodium citrate solution and stir evenly, add 50g of polyethylene glycol, heat to 80°C, stir evenly, cool to room temperature, add 25g of sodium bicarbonate, adjust the pH to 12 with 20%wt NaOH, add 33g of calcium chloride (CaCl2), ultrasonically disperse for 10min, power 300W, then transfer to a reactor for hydrothermal reaction at 170°C for 6h, centrifuge to remove the supernatant to obtain a solid, heat the obtained solid to 90°C in 1000ml of 5%wt NaOH solution, stir for 3h, centrifuge to remove the supernatant to obtain a precipitate, and wash the obtained precipitate three times with deionized water and ethanol respectively, and dry to obtain porous calcium carbonate.

[0043] 50 g of porous calcium carbonate and 40 g of cyclohexylsilane coupling agent were added to 150 ml of 25% wt ethanol aqueous solution, stirred at 85° C. for 1.5 hours, filtered, then washed with deionized water for 3 times, and dried at 50° C. to obtain cyclohexylsilane coupling agent modified porous calcium carbonate.

[0044] 200 g of curing agent was dropped onto 100 g of porous calcium carbonate modified by cyclohexylsilane coupling agent, the mixture was slowly stirred at 100 rpm, and vacuum was evacuated to a negative pressure of -0.10 MPa to obtain a cyclohexylsilane coupling agent modified porous calcium carbonate loaded with a curing agent.

[0045] Preparation Example 3: Epoxysilane Coupling Agent Modified Flake Alumina I:

[0046] 75 g of flaky aluminum oxide I was added to 200 ml of 25% wt ethanol aqueous solution, stirred evenly, and epoxy silane coupling agent was added, followed by ultrasonic dispersion for 30 minutes at an ultrasonic dispersion power of 350 W, heated to 90° C., reacted, filtered, and dried to obtain epoxy silane coupling agent-modified flaky aluminum oxide I.

[0047] Preparation Example 4: Epoxysilane coupling agent modified flaky aluminum oxide II:

[0048] 75 g of flaky aluminum oxide II was added to 200 ml of 25% wt ethanol aqueous solution, stirred evenly, epoxy silane coupling agent was added, and then ultrasonic dispersion was performed for 30 minutes with an ultrasonic dispersion power of 350 W, heated to 90° C., reacted, filtered, and dried to obtain epoxy silane coupling agent-modified flaky aluminum oxide II.

[0049] Aminosilane coupling agent modified flake alumina II:

[0050] 15 g of flaky aluminum oxide II and 20 g of aminosilane coupling agent were added to 200 ml of 25% wt ethanol aqueous solution, mixed, heated to 85° C., stirred for 2 hours, filtered, washed with deionized water 3 times, and dried to obtain aminosilane coupling agent modified flaky aluminum oxide II. Example Example 1

[0051] The mass of each component in this embodiment is: Agent A: 250g of epoxy resin, 50g of flaky aluminum oxide, and 50g of active diluent; Agent B: 180g of the phenylsilane coupling agent modified porous calcium carbonate loaded curing agent of Preparation Example 1, 30g of flaky aluminum oxide, and 10g of active diluent.

[0052] S1: Preparation of Agent A: Mix the epoxy resin and the active diluent according to the mass ratio, stir evenly, add the remaining components, and stir for 15 minutes;

[0053] S2: Preparation of Agent B: Mix the curing agent and active diluent of Agent B, stir for 10 minutes, add the remaining components in two batches, and stir for 20 minutes;

[0054] S3: Mix agent A and agent B in a mass ratio of 1:1 to obtain a high-adhesion solvent-resistant adhesive. Example 2

[0055] The mass of each component in this embodiment is: Agent A: 400g of epoxy resin, 50g of flaky aluminum oxide, and 80g of active diluent; Agent B: 180g of the phenylsilane coupling agent modified porous calcium carbonate loaded curing agent of Preparation Example 1, 30g of flaky aluminum oxide, and 10g of active diluent.

[0056] S1: Preparation of Agent A: Mix the epoxy resin and the active diluent according to the mass ratio, stir evenly, add the remaining components, and stir for 15 minutes;

[0057] S2: Preparation of Agent B: Mix the curing agent and active diluent of Agent B, stir for 10 minutes, add the remaining components in two batches, and stir for 20 minutes;

[0058] S3: Mix agent A and agent B in a mass ratio of 1:1 to obtain a high-adhesion solvent-resistant adhesive. Example 3

[0059] The masses of the components in this embodiment are as follows: Agent A: 400 g of epoxy resin, 50 g of flaky aluminum oxide, and 50 g of reactive diluent; Agent B: 180 g of the phenylsilane coupling agent-modified porous calcium carbonate-loaded curing agent of Preparation Example 1, 80 g of flaky aluminum oxide, and 30 g of reactive diluent.

[0060] S1: Preparation of Agent A: Mix the epoxy resin and the active diluent according to the mass ratio, stir evenly, add the remaining components, and stir for 15 minutes;

[0061] S2: Preparation of Agent B: Mix the curing agent and active diluent of Agent B, stir for 10 minutes, add the remaining components in two batches, and stir for 20 minutes;

[0062] S3: Mix agent A and agent B in a mass ratio of 1:1 to obtain a high-adhesion solvent-resistant adhesive. Example 4

[0063] The masses of the components in this embodiment are as follows: Agent A: 250 g of epoxy resin, 50 g of flaky aluminum oxide modified by epoxy silane coupling agent in Preparation Example 3, and 50 g of reactive diluent; Agent B: 180 g of porous calcium carbonate loaded curing agent modified by phenyl silane coupling agent in Preparation Example 1, 30 g of flaky aluminum oxide modified by epoxy silane coupling agent in Preparation Example 3, and 10 g of reactive diluent.

[0064] S1: Preparation of Agent A: Mix the epoxy resin and the active diluent according to the mass ratio, stir evenly, add the remaining components, and stir for 15 minutes;

[0065] S2: Preparation of Agent B: Mix the curing agent and active diluent of Agent B, stir for 10 minutes, add the remaining components in two batches, and stir for 20 minutes;

[0066] S3: Mix agent A and agent B in a mass ratio of 1:1 to obtain a high-adhesion solvent-resistant adhesive. Example 5

[0067] The mass of each component in this embodiment is: Agent A: 250g of epoxy resin, 50g of flaky aluminum oxide I modified by epoxy silane coupling agent in Preparation Example 3, and 50g of reactive diluent; Agent B: 180g of porous calcium carbonate loaded curing agent modified by phenyl silane coupling agent in Preparation Example 1, 30g of flaky aluminum oxide II modified by epoxy silane coupling agent in Preparation Example 4, and 10g of reactive diluent.

[0068] S1: Preparation of Agent A: Mix the epoxy resin and the active diluent according to the mass ratio, stir evenly, add the remaining components, and stir for 15 minutes;

[0069] S2: Preparation of Agent B: Mix the curing agent and active diluent of Agent B, stir for 10 minutes, add the remaining components in two batches, and stir for 20 minutes;

[0070] S3: Mix agent A and agent B in a mass ratio of 1:1 to obtain a high-adhesion solvent-resistant adhesive. Example 6

[0071] The mass of each component in this embodiment is: Agent A: 250g of epoxy resin, 50g of flaky aluminum oxide I modified by epoxysilane coupling agent in Preparation Example 3, and 50g of reactive diluent; Agent B: 180g of porous calcium carbonate loaded curing agent modified by phenylsilane coupling agent in Preparation Example 1, 30g of flaky aluminum oxide II modified by aminosilane coupling agent in Preparation Example 4, and 10g of reactive diluent.

[0072] S1: Preparation of Agent A: Mix the epoxy resin and the active diluent according to the mass ratio, stir evenly, add the remaining components, and stir for 15 minutes;

[0073] S2: Preparation of Agent B: Mix the curing agent and active diluent of Agent B, stir for 10 minutes, add the remaining components in two batches, and stir for 20 minutes;

[0074] S3: Mix agent A and agent B in a mass ratio of 1:1 to obtain a high-adhesion solvent-resistant adhesive. Example 7

[0075] The mass of each component in this embodiment is: Agent A: 250g of epoxy resin, 42g of flaky aluminum oxide I modified by epoxysilane coupling agent in Preparation Example 3, and 50g of reactive diluent; Agent B: 180g of porous calcium carbonate loaded curing agent modified by phenylsilane coupling agent in Preparation Example 1, 38g of flaky aluminum oxide II modified by aminosilane coupling agent in Preparation Example 4, and 10g of reactive diluent.

[0076] S1: Preparation of Agent A: Mix the epoxy resin and the active diluent according to the mass ratio, stir evenly, add the remaining components, and stir for 15 minutes;

[0077] S2: Preparation of Agent B: Mix the curing agent and active diluent of Agent B, stir for 10 minutes, add the remaining components in two batches, and stir for 20 minutes;

[0078] S3: Mix agent A and agent B in a mass ratio of 1:1 to obtain a high-adhesion solvent-resistant adhesive. Example 8

[0079] The mass of each component in this embodiment is: Agent A: 250g of epoxy resin, 48g of flaky aluminum oxide I modified by epoxysilane coupling agent in Preparation Example 3, and 50g of reactive diluent; Agent B: 180g of porous calcium carbonate loaded curing agent modified by phenylsilane coupling agent in Preparation Example 1, 32g of flaky aluminum oxide II modified by aminosilane coupling agent in Preparation Example 4, and 10g of reactive diluent.

[0080] S1: Preparation of Agent A: Mix epoxy resin and active diluent according to mass ratio, stir evenly, add remaining components, stir for 15 minutes,

[0081] S2: Preparation of Agent B: Mix the curing agent and active diluent of Agent B, stir for 10 minutes, add the remaining components in two batches, and stir for 20 minutes;

[0082] S3: Mix agent A and agent B in a mass ratio of 1:1 to obtain a high-adhesion solvent-resistant adhesive. Example 9

[0083] The mass of each component in this embodiment is: Agent A: 250g of epoxy resin, 54g of flaky aluminum oxide I modified by epoxysilane coupling agent in Preparation Example 3, and 50g of reactive diluent; Agent B: 180g of porous calcium carbonate loaded curing agent modified by phenylsilane coupling agent, 26g of flaky aluminum oxide II modified by aminosilane coupling agent in Preparation Example 4, and 10g of reactive diluent.

[0084] S1: Preparation of Agent A: Mix the epoxy resin and the active diluent according to the mass ratio, stir evenly, add the remaining components, and stir for 15 minutes;

[0085] S2: Preparation of Agent B: Mix the curing agent and active diluent of Agent B, stir for 10 minutes, add the remaining components in two batches, and stir for 20 minutes;

[0086] S3: Mix agent A and agent B in a mass ratio of 1:1 to obtain a high-adhesion solvent-resistant adhesive. Example 10

[0087] The screen printing screen is prepared by bonding the frame, polyester mesh, metal mesh and polyimide film using the high adhesion solvent-resistant adhesive prepared in Example 1. The preparation steps include:

[0088] S1: Stretch the net: Use adhesive to stick the polyester net at a position of 600mm*600mm according to a certain tension requirement;

[0089] S2: Compounding: PE hot melt adhesive film is used to compound the steel wire mesh onto the polyester mesh at about 100°C in a compounding machine, and the polyester mesh in the middle is removed to obtain a false frame screen;

[0090] S3: Top frame: The composite false frame screen is placed on the fixture, and the top frame machine uses a certain air pressure to push the 450mm*450mm main frame to the center of the false frame, and then adheres it with adhesive to form a 450mm*450mm main frame screen;

[0091] S4: Degreasing: Use cleaning agent to wipe and clean the screen of this frame;

[0092] S5: wire drawing: cutting part of the steel wire with laser;

[0093] S6: Degreasing: Wipe and clean with a cleaning agent;

[0094] S7: bonding: coating the polyimide film with adhesive and pressing it on the center of the steel mesh at a temperature of 200°C;

[0095] S8: The photosensitive adhesive covers the area outside the pattern to prevent ink leakage at the edge of the wire mesh;

[0096] S9: Graphics: Through graphic conversion, the polyimide film is cut by laser to form a pattern;

[0097] S10: The formed screen is packaged with tapes of various specifications to achieve the effects of wear resistance, protection and ink blocking.

[0098] Comparative Example

[0099] Comparative Example 1

[0100] The masses of the components in this embodiment are as follows: Agent A: 250 g of epoxy resin, 50 g of flaky aluminum oxide, and 50 g of reactive diluent; Agent B: 60 g of porous calcium carbonate modified with phenyl silane coupling agent, 120 g of curing agent, 30 g of flaky aluminum oxide, and 10 g of reactive diluent.

[0101] S1: Preparation of Agent A: Mix the epoxy resin and the active diluent according to the mass ratio, stir evenly, add the remaining components, and stir for 15 minutes;

[0102] S2: Preparation of Agent B: Mix the curing agent and active diluent of Agent B, stir for 10 minutes, add the remaining components in two batches, and stir for 20 minutes;

[0103] S3: Mix agent A and agent B in a mass ratio of 1:1 to obtain a high-adhesion solvent-resistant adhesive.

[0104] Comparative Example 2

[0105] The masses of the components in this embodiment are as follows: Agent A: 250 g of epoxy resin, 50 g of flaky aluminum oxide, and 50 g of reactive diluent; Agent B: 180 g of cyclohexylsilane coupling agent-modified porous calcium carbonate-loaded curing agent, 30 g of flaky aluminum oxide, and 10 g of reactive diluent.

[0106] S1: Preparation of Agent A: Mix the epoxy resin and the active diluent according to the mass ratio, stir evenly, add the remaining components, and stir for 15 minutes;

[0107] S2: Preparation of Agent B: Mix the curing agent and active diluent of Agent B, stir for 10 minutes, add the remaining components in two batches, and stir for 20 minutes;

[0108] S3: Mix agent A and agent B in a mass ratio of 1:1 to obtain a high-adhesion solvent-resistant adhesive.

[0109] Performance testing

[0110] Test 1: Referring to the standard GB / T6329-1996 "Determination of tensile strength of adhesive butt joints", the surfaces of two test bars were respectively coated with a polyimide film and a steel mesh, and the tensile strength 1 of the adhesives prepared in each embodiment and comparative example was tested. The test results are summarized in Table 1.

[0111] Test 2: Referring to the standard GB / T6329-1996 "Determination of tensile strength of adhesive butt joints", the surfaces of two test bars were respectively coated with a polyimide film and a steel mesh, and immersed in the ink Merida UV 9000 for 10 hours. Then, the tensile strength 2 of the adhesives prepared in each embodiment and comparative example was tested, and the tensile strength retention rate was calculated. The calculation method is: tensile strength 2 / tensile strength 1×100%. The test results are summarized in Table 1.

[0112] Table 1

[0113] Tensile strength (MPa) Tensile strength retention rate (%) Example 1 20.1 93.1 Example 2 20.3 93.1 Example 3 20.2 93.0 Example 4 22.3 94.7 Example 5 22.7 95.1 Example 6 23.1 96.0 Example 7 23.3 96.3 Example 8 23.4 96.4 Example 9 23.0 95.7 Comparative Example 1 15.1 70.0 Comparative Example 2 17.5 87.9

[0114] In combination with Examples 1-3, Comparative Examples 1-2 and Table 1, the present application increases the fluidity of the adhesive and improves the wetting on the substrate by adding a certain mass of diluent to the adhesive, adds a certain mass of phenylsilane coupling agent to modify the porous calcium carbonate loaded curing agent, improves the uniformity of the filler from the aspects of steric hindrance, sustained release, and electron withdrawal to reduce the activity of the epoxy group, reduces the curing speed of the adhesive, further fully wets the substrate, improves the curing effect, has high tensile strength, releases stress and reduces the weak interface layer, thereby reducing the penetration of solvents; the internal structure is not easy to change after the solvent penetrates, and the tensile strength retention rate is high after soaking in ink; the addition of the porous calcium carbonate loaded curing agent modified by the phenylsilane coupling agent also improves the modulus while ensuring the tensile strength, further avoids stress concentration at the bonding interface in the polyimide film and the steel mesh, and improves the tensile strength performance.

[0115] In combination with Example 1, Examples 4-9 and Table 1, the present application further constructs an isolation network for solvents by limiting the filler to a certain mass of epoxy silane coupling agent modified flaky aluminum oxide I and amino silane coupling agent modified flaky aluminum oxide II and limiting the particle size and mass ratio, and participates in the curing of the adhesive by performing epoxy and amino modifications respectively, further improving the tensile strength and solvent resistance while improving the modulus, and the tensile strength retention rate is high.

[0116] This specific embodiment of the present application is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, a person skilled in the art may make modifications to the embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A high adhesion solvent resistant adhesive, characterized in that: The invention comprises an agent A and an agent B in a mass ratio of 1:1, wherein the agent A comprises the following raw materials in mass parts: 25-40 parts of epoxy resin, 5-10 parts of filler, and 5-8 parts of active diluent; the agent B comprises the following raw materials in mass parts: 18-30 parts of phenylsilane coupling agent modified porous calcium carbonate loaded curing agent, 3-8 parts of filler, and 1-3 parts of active diluent; the preparation steps of the phenylsilane coupling agent modified porous calcium carbonate loaded curing agent include: S1: adding porous calcium carbonate and phenylsilane coupling agent to ethanol aqueous solution, stirring evenly, ultrasonic treatment, reaction, reduced pressure distillation, suction filtration, washing, vacuum drying, to obtain phenylsilane coupling agent modified porous calcium carbonate; S2: slowly stirring the curing agent and the porous calcium carbonate modified by the phenylsilane coupling agent evenly, and evacuating to negative pressure to obtain the phenylsilane coupling agent modified porous calcium carbonate loaded with the curing agent.

2. The high adhesion and solvent resistant adhesive according to claim 1, characterized in that: The curing agent has an amine value of 120-200 mg KOH / g and a weight average molecular weight of 500-950 g / mol.

3. The high adhesion and solvent resistant adhesive according to claim 1, characterized in that: The particle size of the porous calcium carbonate is 1-8 μm.

4. The high adhesion and solvent resistant adhesive according to claim 1, characterized in that: The filler in the agent A is flaky aluminum oxide I modified by an epoxy silane coupling agent, and the filler in the agent B is flaky aluminum oxide II modified by an amino silane coupling agent.

5. The high adhesion and solvent resistant adhesive according to claim 4, characterized in that: The average particle size of the flaky aluminum oxide I is 2-10 μm, and the average particle size of the flaky aluminum oxide II is 0.8-1 μm.

6. The high adhesion and solvent resistant adhesive according to claim 5, characterized in that: The mass ratio of the epoxysilane coupling agent modified flaky aluminum oxide I to the aminosilane coupling agent modified flaky aluminum oxide II is (1.1-1.5):

1.

7. A method for preparing the high-adhesion solvent-resistant adhesive according to any one of claims 1 to 6, characterized in that: The steps include: S1: Preparation of Agent A: Mix the epoxy resin and the active diluent according to the mass ratio, stir evenly, add the remaining components, and stir for 10-25 minutes; S2: Preparation of Agent B: Mix the curing agent and active diluent of Agent B, stir for 5-10 minutes, add the remaining components twice, and stir for 15-20 minutes; S3: Mix agent A and agent B evenly to obtain a high-adhesion solvent-resistant adhesive.

8. A polyimide composite film, characterized in that: The invention comprises a polyimide film, an adhesive layer and a metal mesh, wherein the adhesive layer is composed of the adhesive according to any one of claims 1 to 6.

9. A screen printing screen, characterized in that: The invention comprises the frame, a polyester net and a polyimide composite film, wherein the polyimide composite film is the polyimide composite film as claimed in claim 8.