Bio-based fabric, clothing and preparation method thereof
By modifying the impregnation treatment and coordinating the materials, the flame retardancy, thermal insulation and stain resistance of bio-based fabrics are improved, and the problem of difficult fabric performance coordination in the prior art is solved, which significantly improves the water washing and heat resistance of the fabrics. stability.
Patent Information
- Application Number
- CN202411196121.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The flame retardant properties, thermal insulation and soil resistance of existing bio-based fabrics are difficult to coordinate and improve, and the water washing resistance and heat resistance are poor, which limits the efficiency of the product.
Polyester fiber, modified bio-based polyamide fiber and blended yarn are treated with modified impregnation liquid and are woven into knitted fabrics. They are made of nano-silica, glass fiber, magnesium hydroxide and other materials in the modified liquid. Coordinate the coordination to improve the performance of the fibers through ultrasonic modification and ball milling treatment.
It significantly improves the flame retardancy, thermal insulation and stain resistance of bio-based fabrics, and improves the water washing and heat resistance of the fabrics, achieving coordinated improvement in performance.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bio-based knitted fabrics, and in particular to a bio-based fabric, clothing and a preparation method thereof. Background Art
[0002] Knitted fabrics generally have good elasticity and elastic recovery, so they are often used to make tight, close-fitting clothing such as underwear and outerwear, or other functional clothing. Fabrics based on bio-based polyamides, a new type of material made from plant-derived carbohydrates and fatty acids, can effectively alleviate the oil crisis and have great development potential in the field of fiber, fabric and other textile preparation.
[0003] Existing bio-based fabrics have poor flame retardancy, and the thermal insulation and anti-fouling properties of fabric products are average. It is difficult to achieve coordinated improvements in flame retardancy, thermal insulation and anti-fouling properties of the products. In addition, the fabrics have poor water resistance and heat stability, which further limits the efficiency of product use. Summary of the invention
[0004] In view of the defects of the prior art, the object of the present invention is to provide a bio-based fabric, clothing and a preparation method thereof to solve the problems raised in the above background technology.
[0005] The present invention solves the technical problem by adopting the following technical solution:
[0006] The present invention provides a method for preparing a bio-based fabric, comprising the following steps:
[0007] Step 1: Weigh the raw materials by weight: 40-45 parts of polyester fiber, 30-35 parts of modified bio-based polyamide fiber, and 10-15 parts of blended yarn; wherein the blended yarn is made by spinning polyester fiber and carbon fiber in a weight ratio of 2:1;
[0008] Step 2: respectively immersing the polyester fiber, modified bio-based polyamide fiber, and blended yarn in the step 1 into the impregnation liquid for modification and impregnation treatment, taking out and drying after the impregnation, to obtain the impregnated polyester fiber, modified bio-based polyamide fiber, and blended yarn;
[0009] Step 3: Weaving the impregnated polyester fiber, modified bio-based polyamide fiber, and blended yarn into a knitted fabric body using a large circular machine;
[0010] Step 4: Roll up the knitted fabric and store it in storage to obtain the bio-based fabric.
[0011] Preferably, the impregnation pressure of the modified impregnation treatment is 10-15 MPa, and the impregnation time is 1-2 h.
[0012] Preferably, the preparation method of the modified bio-based polyamide fiber is:
[0013] S01: mixing the bio-based polyamide 56 slices and the regulator in a weight ratio of 5:2 to obtain regulated bio-based polyamide 56 slices;
[0014] S02: Preparation of modified solution:
[0015] S021: 3-5 parts of nano-silicon dioxide, 1-3 parts of sodium silicate solution with a mass fraction of 5-7%, and 2-5 parts of phosphate buffer solution with a pH value of 5.5 are uniformly mixed by weight, and then 2-4 parts of glass fiber are added by weight to mix and ball-milled at a ball-milling speed of 1000-1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a nano-silicon dioxide coordinator;
[0016] S022: 2-5 parts of chitosan solution and 2-4 parts of nano-silicon dioxide coordinator are mixed and added to 4-7 parts of lanthanum chloride solution, and then 3-5 parts of magnesium hydroxide flame retardant and 2-4 parts of silane coupling agent KH560 are added and mixed sufficiently to obtain a modified solution;
[0017] S03: Then, the adjusted bio-based polyamide 56 slices are ultrasonically modified in a modification liquid of 4 to 7 times the total weight of the adjusted bio-based polyamide 56 slices. After the modification is completed, the modified polyamide body is filtered and dried to obtain the modified polyamide body. Finally, the modified polyamide body is subjected to melt spinning technology to obtain modified bio-based polyamide fibers.
[0018] Preferably, the ultrasonic power of the ultrasonic modification treatment is 400-500 W, and the ultrasonic time is 20-30 min.
[0019] Preferably, the mass fraction of the chitosan solution is 2-5%; the mass fraction of the lanthanum chloride solution is 3-6%.
[0020] Preferably, the preparation method of the regulator is:
[0021] The nano-bentonite is first heat-treated at 250-270°C for 5-10 minutes, and then cooled to 55°C at a rate of 2-5°C / min and heat-treated to obtain heat-treated nano-bentonite;
[0022] 4-7 parts of heat-treated nano-bentonite, 1-3 parts of sodium dodecylbenzene sulfonate, and 2-5 parts of graphene are added by weight to 6-10 parts of 5% yttrium nitrate solution, and then 1-3 parts of citric acid are added by weight, and the mixture is mixed and stirred at a stirring speed of 750-850 r / min for 35-45 minutes. After the stirring is completed, the mixture is washed with water and dried to obtain a regulator.
[0023] Preferably, the preparation method of the impregnation solution is:
[0024] S11: irradiating the hydroxyapatite in a proton irradiation box for 10-15 minutes at an irradiation power of 350-400W, and obtaining irradiated hydroxyapatite after the irradiation is completed;
[0025] The irradiated hydroxyapatite is immersed in a sufficient amount of sodium alginate solution, the ultrasonic power is 400-450W, the immersion time is 20-30min, and the immersion is completed to obtain the immersed hydroxyapatite agent;
[0026] S12: 3-5 parts of the impregnated hydroxyapatite agent, 1-3 parts of stearic acid, 4-7 parts of sodium lignin sulfonate solution and 2-3 parts of silane coupling agent KH550 are uniformly mixed to obtain an impregnation solution.
[0027] Preferably, the mass fraction of the sodium alginate solution is 4-6%; the mass fraction of the sodium lignin sulfonate solution is 5-8%.
[0028] The present invention also provides a bio-based fabric, which is prepared by the above-mentioned method for preparing a bio-based fabric.
[0029] The present invention also provides a garment made from the above-mentioned bio-based fabric.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The bio-based fabric of the present invention adopts polyester fiber, modified bio-based polyamide fiber, and blended yarn to be modified and impregnated with an impregnation liquid, and finally woven into a knitted fabric body by a large circular machine. The modified bio-based polyamide fiber is coordinated with the impregnation liquid for modification and impregnation, and the flame retardancy, heat preservation and anti-fouling properties of the obtained product are coordinated and improved, and the fabric has remarkable effects on water resistance and heat resistance stability;
[0032] 2. The modified bio-based polyamide fiber adopts the existing stable bio-based polyamide 56 slices and the regulator for coordination treatment, and then undergoes ultrasonic modification treatment in the modification liquid, and obtains the modified bio-based polyamide fiber through the existing melt spinning technology. The regulator is first heat-treated at 250-270°C for 5-10 minutes with nano-bentonite, and then cooled to 55°C at a rate of 2-5°C / min, and heat-insulated to obtain heat-treated nano-bentonite. The active efficiency and interlaminar spacing of the nano-bentonite are optimized through the thermal improvement treatment of the nano-bentonite. Sodium dodecylbenzene sulfonate, graphene, 5% by mass yttrium nitrate solution and citric acid are mixed and stirred. Through the coordination and coordination between the raw materials, the raw materials in the regulator are adjusted with graphene, and the coordination and synergy are achieved. Graphite is used as a flaky structure to assemble the interlaminar spacing of the nano-bentonite, thereby improving the stability of the regulator in the bio-based polyamide fiber, optimizing the performance stability of the product, and providing a strong foundation for the thermal insulation of the product.
[0033] 3. The modified liquid is treated by ball milling with nano-silicon dioxide, sodium silicate solution with a mass fraction of 5-7%, phosphate buffer solution with a pH value of 5.5 and glass fiber. The use of nano-silicon dioxide with a high specific surface area can optimize the interface of the system raw materials. At the same time, glass fiber is used as a needle-like structure to strengthen the system performance, and can coordinate as a needle-like point structure to optimize the anti-fouling and easy-to-clean performance of the product. The obtained nano-silicon dioxide coordinator is fully blended with chitosan solution, lanthanum chloride solution, magnesium hydroxide flame retardant and silane coupling agent KH560. Through the coordination between the raw materials, the flame retardancy, heat preservation and anti-fouling coordination of the product, as well as the stability of product performance, are optimized. The raw materials in the modified liquid are coordinated and matched with each other to enhance the mutual matching and mutual assistance between the raw materials, further play the synergistic effect between the product raw materials, and enhance the performance effect of the product system;
[0034] 4. The hydroxyapatite used in the impregnation liquid is irradiated in a proton irradiation box for 10-15 minutes with an irradiation power of 350-400W to optimize the activity of hydroxyapatite. The point adsorption effect of hydroxyapatite is combined with sufficient immersion in the sodium alginate solution to enhance the dispersion of hydroxyapatite. At the same time, stearic acid, sodium lignin sulfonate solution and silane coupling agent KH550 are evenly blended to obtain the impregnation liquid. Through the mutual coordination and adjustment of the impregnation liquids and the synergistic effect of the raw materials, the interface between the fibers is further improved, the matching effect between the fibers is optimized, and the overall performance of the product is improved, thereby further improving the performance of the product. DETAILED DESCRIPTION
[0035] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] A method for preparing a bio-based fabric in this embodiment comprises the following steps:
[0037] Step 1: Weigh the raw materials by weight: 40-45 parts of polyester fiber, 30-35 parts of modified bio-based polyamide fiber, and 10-15 parts of blended yarn; wherein the blended yarn is made by spinning polyester fiber and carbon fiber in a weight ratio of 2:1;
[0038] Step 2: respectively immersing the polyester fiber, modified bio-based polyamide fiber, and blended yarn in the step 1 into the impregnation liquid for modification and impregnation treatment, taking out and drying after the impregnation, to obtain the impregnated polyester fiber, modified bio-based polyamide fiber, and blended yarn;
[0039] Step 3: Weaving the impregnated polyester fiber, modified bio-based polyamide fiber, and blended yarn into a knitted fabric body using a large circular machine;
[0040] Step 4: Roll up the knitted fabric and store it in storage to obtain the bio-based fabric.
[0041] The impregnation pressure of the modified impregnation treatment in this embodiment is 10-15 MPa, and the impregnation time is 1-2 hours.
[0042] The preparation method of the modified bio-based polyamide fiber of this embodiment is:
[0043] S01: mixing the bio-based polyamide 56 slices and the regulator in a weight ratio of 5:2 to obtain regulated bio-based polyamide 56 slices;
[0044] S02: Preparation of modified solution:
[0045] S021: 3-5 parts of nano-silicon dioxide, 1-3 parts of sodium silicate solution with a mass fraction of 5-7%, and 2-5 parts of phosphate buffer solution with a pH value of 5.5 are uniformly mixed by weight, and then 2-4 parts of glass fiber are added by weight to mix and ball-milled at a ball-milling speed of 1000-1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a nano-silicon dioxide coordinator;
[0046] S022: 2-5 parts of chitosan solution and 2-4 parts of nano-silicon dioxide coordinator are mixed and added to 4-7 parts of lanthanum chloride solution, and then 3-5 parts of magnesium hydroxide flame retardant and 2-4 parts of silane coupling agent KH560 are added and mixed sufficiently to obtain a modified solution;
[0047] S03: Then, the adjusted bio-based polyamide 56 slices are subjected to ultrasonic modification in a modification liquid of 4 to 7 times the total weight of the adjusted bio-based polyamide 56 slices, and after the modification is completed, the modified polyamide body is filtered and dried to obtain a modified polyamide body, and finally the modified polyamide body is subjected to melt spinning technology to obtain a modified bio-based polyamide fiber;
[0048] The bio-based polyamide 56 slicing and melt spinning technology both adopt the existing technology of a high-stability bio-based polyamide 56 fiber disclosed in the patent with publication number CN114045562A, and the existing technology is omitted here.
[0049] The ultrasonic power of the ultrasonic modification treatment in this embodiment is 400-500W, and the ultrasonic time is 20-30min.
[0050] The mass fraction of the chitosan solution in this embodiment is 2-5%; the mass fraction of the lanthanum chloride solution is 3-6%.
[0051] The preparation method of the regulator of this embodiment is:
[0052] The nano-bentonite is first heat-treated at 250-270°C for 5-10 minutes, and then cooled to 55°C at a rate of 2-5°C / min and heat-treated to obtain heat-treated nano-bentonite;
[0053] 4-7 parts of heat-treated nano-bentonite, 1-3 parts of sodium dodecylbenzene sulfonate, and 2-5 parts of graphene are added by weight to 6-10 parts of 5% yttrium nitrate solution, and then 1-3 parts of citric acid are added by weight, and the mixture is mixed and stirred at a stirring speed of 750-850 r / min for 35-45 minutes. After the stirring is completed, the mixture is washed with water and dried to obtain a regulator.
[0054] The preparation method of the impregnation liquid of this embodiment is:
[0055] S11: irradiating the hydroxyapatite in a proton irradiation box for 10-15 minutes at an irradiation power of 350-400W, and obtaining irradiated hydroxyapatite after the irradiation is completed;
[0056] The irradiated hydroxyapatite is immersed in a sufficient amount of sodium alginate solution, the ultrasonic power is 400-450W, the immersion time is 20-30min, and the immersion is completed to obtain the immersed hydroxyapatite agent;
[0057] S12: 3-5 parts of the impregnated hydroxyapatite agent, 1-3 parts of stearic acid, 4-7 parts of sodium lignin sulfonate solution and 2-3 parts of silane coupling agent KH550 are uniformly mixed to obtain an impregnation solution.
[0058] The mass fraction of the sodium alginate solution in this embodiment is 4-6%; the mass fraction of the sodium lignin sulfonate solution is 5-8%.
[0059] This embodiment also provides a bio-based fabric, which is prepared by the above-mentioned method for preparing a bio-based fabric.
[0060] This embodiment also provides a garment made of bio-based fabrics.
[0061] Embodiment 1: A method for preparing a bio-based fabric, comprising the following steps:
[0062] Step 1: Weigh the raw materials by weight: 40 parts of polyester fiber, 30 parts of modified bio-based polyamide fiber, and 10 parts of blended yarn; wherein the blended yarn is made by spinning polyester fiber and carbon fiber in a weight ratio of 2:1;
[0063] Step 2: respectively immersing the polyester fiber, modified bio-based polyamide fiber, and blended yarn in the step 1 into the impregnation liquid for modification and impregnation treatment, taking out and drying after the impregnation, to obtain the impregnated polyester fiber, modified bio-based polyamide fiber, and blended yarn;
[0064] Step 3: Weaving the impregnated polyester fiber, modified bio-based polyamide fiber, and blended yarn into a knitted fabric body using a large circular machine;
[0065] Step 4: Roll up the knitted fabric and store it in storage to obtain the bio-based fabric.
[0066] The impregnation pressure of the modified impregnation treatment in this embodiment is 10 MPa, and the impregnation time is 1 hour.
[0067] The preparation method of the modified bio-based polyamide fiber of this embodiment is:
[0068] S01: mixing the bio-based polyamide 56 slices and the regulator in a weight ratio of 5:2 to obtain regulated bio-based polyamide 56 slices;
[0069] S02: Preparation of modified solution:
[0070] S021: 3 parts of nano-silicon dioxide, 1 part of 5% sodium silicate solution by weight, and 2 parts of phosphate buffer solution with a pH value of 5.5 are uniformly mixed, and then 2 parts of glass fiber are added by weight to mix and ball-milled at a ball-milling speed of 1000 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a nano-silicon dioxide coordinator;
[0071] S022: 2 parts of chitosan solution and 2 parts of nano-silica coordinator are mixed and added to 4 parts of lanthanum chloride solution, and then 3 parts of magnesium hydroxide flame retardant and 2 parts of silane coupling agent KH560 are added and mixed thoroughly to obtain a modified solution;
[0072] S03: Then, the adjusted bio-based polyamide 56 slices are subjected to ultrasonic modification in a modification liquid of 4 times the total weight of the adjusted bio-based polyamide 56 slices, and after the modification is completed, the modified polyamide body is filtered and dried to obtain a modified polyamide body, and finally the modified polyamide body is subjected to melt spinning technology to obtain a modified bio-based polyamide fiber;
[0073] Among them, the bio-based polyamide 56 slicing and melt spinning technology both adopt the existing technology of a high-stability bio-based polyamide 56 fiber disclosed in the patent with publication number CN114045562A. This is the existing technology and is omitted.
[0074] The ultrasonic power of the ultrasonic modification treatment in this embodiment is 400 W, and the ultrasonic time is 20 min.
[0075] The mass fraction of the chitosan solution in this embodiment is 2%; the mass fraction of the lanthanum chloride solution is 3%.
[0076] The preparation method of the regulator of this embodiment is:
[0077] The nano-bentonite is first heat-treated at 250°C for 5 minutes, and then cooled to 55°C at a rate of 2°C / min and heat-treated to obtain heat-treated nano-bentonite;
[0078] 4 parts of heat-treated nano-bentonite, 1 part of sodium dodecylbenzene sulfonate, and 2 parts of graphene are added by weight to 6 parts of 5% by weight yttrium nitrate solution, and then 1 part of citric acid is added by weight and mixed and stirred at a stirring speed of 750 r / min for 35 minutes. After the stirring is completed, the agent is washed with water and dried to obtain a regulator.
[0079] The preparation method of the impregnation liquid of this embodiment is:
[0080] S11: irradiating the hydroxyapatite in a proton irradiation box for 10 minutes at an irradiation power of 350 W, and obtaining irradiated hydroxyapatite after the irradiation is completed;
[0081] The irradiated hydroxyapatite is immersed in a sufficient amount of sodium alginate solution, the ultrasonic power is 400W, the immersion time is 20 minutes, and the immersion is completed to obtain an immersed hydroxyapatite agent;
[0082] S12: 3 parts of the impregnated hydroxyapatite agent, 1 part of stearic acid, 4 parts of sodium lignin sulfonate solution and 2 parts of silane coupling agent KH550 are mixed evenly to obtain an impregnation solution.
[0083] The mass fraction of the sodium alginate solution in this embodiment is 4%; the mass fraction of the sodium lignin sulfonate solution is 5%.
[0084] This embodiment also provides a bio-based fabric, which is prepared by the above-mentioned method for preparing a bio-based fabric.
[0085] This embodiment also provides a garment made of bio-based fabrics.
[0086] Embodiment 2: A method for preparing a bio-based fabric, comprising the following steps:
[0087] Step 1: Weigh the raw materials by weight: 45 parts of polyester fiber, 35 parts of modified bio-based polyamide fiber, and 15 parts of blended yarn; wherein the blended yarn is made by spinning polyester fiber and carbon fiber in a weight ratio of 2:1;
[0088] Step 2: respectively immersing the polyester fiber, modified bio-based polyamide fiber, and blended yarn in the step 1 into the impregnation liquid for modification and impregnation treatment, taking out and drying after the impregnation, to obtain the impregnated polyester fiber, modified bio-based polyamide fiber, and blended yarn;
[0089] Step 3: Weaving the impregnated polyester fiber, modified bio-based polyamide fiber, and blended yarn into a knitted fabric body using a large circular machine;
[0090] Step 4: Roll up the knitted fabric and store it in storage to obtain the bio-based fabric.
[0091] The impregnation pressure of the modified impregnation treatment in this embodiment is 15 MPa, and the impregnation time is 2 h.
[0092] The preparation method of the modified bio-based polyamide fiber of this embodiment is:
[0093] S01: mixing the bio-based polyamide 56 slices and the regulator in a weight ratio of 5:2 to obtain regulated bio-based polyamide 56 slices;
[0094] S02: Preparation of modified solution:
[0095] S021: 5 parts of nano-silicon dioxide, 3 parts of sodium silicate solution with a mass fraction of 7%, and 5 parts of phosphate buffer solution with a pH value of 5.5 are mixed uniformly by weight, and then 4 parts of glass fiber are added by weight to mix and ball-milled at a ball-milling speed of 1500r / min for 2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a nano-silicon dioxide coordinator;
[0096] S022: 5 parts of chitosan solution and 4 parts of nano-silica coordinator are mixed and added to 7 parts of lanthanum chloride solution, and then 5 parts of magnesium hydroxide flame retardant and 4 parts of silane coupling agent KH560 are added and mixed thoroughly to obtain a modified solution;
[0097] S03: Then, the adjusted bio-based polyamide 56 slices are subjected to ultrasonic modification in a modification liquid of 7 times the total weight of the adjusted bio-based polyamide 56 slices, and after the modification is completed, the modified polyamide body is filtered and dried to obtain a modified polyamide body, and finally the modified polyamide body is subjected to melt spinning technology to obtain a modified bio-based polyamide fiber;
[0098] Among them, the bio-based polyamide 56 slicing and melt spinning technology both adopt the existing technology of a high-stability bio-based polyamide 56 fiber disclosed in the patent with publication number CN114045562A. This is the existing technology and is omitted.
[0099] The ultrasonic power of the ultrasonic modification treatment in this embodiment is 500 W, and the ultrasonic time is 30 min.
[0100] The mass fraction of the chitosan solution in this embodiment is 5%; the mass fraction of the lanthanum chloride solution is 6%.
[0101] The preparation method of the regulator of this embodiment is:
[0102] The nano-bentonite is first heat-treated at 270°C for 10 minutes, and then cooled to 55°C at a rate of 5°C / min and heat-treated to obtain heat-treated nano-bentonite;
[0103] 7 parts of heat-treated nano-bentonite, 3 parts of sodium dodecylbenzene sulfonate, and 5 parts of graphene are added by weight to 10 parts of 5% yttrium nitrate solution, and then 3 parts of citric acid are added by weight and mixed and stirred at a stirring speed of 850 r / min for 45 minutes. After the stirring is completed, the agent is washed with water and dried to obtain a regulator.
[0104] The preparation method of the impregnation liquid of this embodiment is:
[0105] S11: irradiating the hydroxyapatite in a proton irradiation box for 15 minutes at an irradiation power of 400 W, and obtaining irradiated hydroxyapatite after the irradiation is completed;
[0106] The irradiated hydroxyapatite is immersed in a sufficient amount of sodium alginate solution, the ultrasonic power is 450W, the immersion time is 30 minutes, and the immersion is completed to obtain an immersed hydroxyapatite agent;
[0107] S12: 5 parts of the impregnated hydroxyapatite agent, 3 parts of stearic acid, 7 parts of sodium lignin sulfonate solution and 3 parts of silane coupling agent KH550 are mixed evenly to obtain an impregnation solution.
[0108] The mass fraction of the sodium alginate solution in this embodiment is 6%; the mass fraction of the sodium lignin sulfonate solution is 8%.
[0109] This embodiment also provides a bio-based fabric, which is prepared by the above-mentioned method for preparing a bio-based fabric.
[0110] This embodiment also provides a garment made of bio-based fabrics.
[0111] Embodiment 3: A method for preparing a bio-based fabric, comprising the following steps:
[0112] Step 1: Weigh the raw materials by weight: 42.5 parts of polyester fiber, 32.5 parts of modified bio-based polyamide fiber, and 12.5 parts of blended yarn; wherein the blended yarn is a blend of polyester fiber and carbon fiber in a weight ratio of 2:1 by spinning;
[0113] Step 2: respectively immersing the polyester fiber, modified bio-based polyamide fiber, and blended yarn in the step 1 into the impregnation liquid for modification and impregnation treatment, taking out and drying after the impregnation, to obtain the impregnated polyester fiber, modified bio-based polyamide fiber, and blended yarn;
[0114] Step 3: Weaving the impregnated polyester fiber, modified bio-based polyamide fiber, and blended yarn into a knitted fabric body using a large circular machine;
[0115] Step 4: Roll up the knitted fabric and store it in storage to obtain the bio-based fabric.
[0116] The impregnation pressure of the modified impregnation treatment in this embodiment is 12.5 MPa, and the impregnation time is 1.5 h.
[0117] The preparation method of the modified bio-based polyamide fiber of this embodiment is:
[0118] S01: mixing the bio-based polyamide 56 slices and the regulator in a weight ratio of 5:2 to obtain regulated bio-based polyamide 56 slices;
[0119] S02: Preparation of modified solution:
[0120] S021: 4 parts of nano-silicon dioxide, 2 parts of 6% sodium silicate solution, and 3.5 parts of phosphate buffer solution with a pH value of 5.5 are mixed uniformly by weight, and then 3 parts of glass fiber are added by weight for ball milling. The ball milling speed is 1250r / min, and the ball milling is performed for 2h. After the ball milling is completed, the mixture is washed with water and dried to obtain a nano-silicon dioxide coordinator;
[0121] S022: 3.5 parts of chitosan solution and 3 parts of nano-silica coordinator are mixed and added to 5.5 parts of lanthanum chloride solution by weight, and then 4 parts of magnesium hydroxide flame retardant and 3 parts of silane coupling agent KH560 are added by weight and mixed thoroughly to obtain a modified solution;
[0122] S03: Then, the adjusted bio-based polyamide 56 slices are subjected to ultrasonic modification in a modification liquid with a weight of 5.5 times the total weight of the adjusted bio-based polyamide 56 slices. After the modification is completed, the modified polyamide body is filtered and dried to obtain a modified polyamide body. Finally, the modified polyamide body is subjected to melt spinning technology to obtain a modified bio-based polyamide fiber.
[0123] Among them, the bio-based polyamide 56 slicing and melt spinning technology both adopt the existing technology of a high-stability bio-based polyamide 56 fiber disclosed in the patent with publication number CN114045562A. This is the existing technology and is omitted.
[0124] The ultrasonic power of the ultrasonic modification treatment in this embodiment is 450W, and the ultrasonic time is 25min.
[0125] The mass fraction of the chitosan solution in this embodiment is 3.5%; the mass fraction of the lanthanum chloride solution is 4.5%.
[0126] The preparation method of the regulator of this embodiment is:
[0127] The nano-bentonite is first heat-treated at 260°C for 7.5 minutes, and then cooled to 55°C at a rate of 3.5°C / min and heat-treated to obtain heat-treated nano-bentonite;
[0128] 5.5 parts of heat-treated nano-bentonite, 2 parts of sodium dodecylbenzene sulfonate, and 3.5 parts of graphene were added by weight to 8 parts of 5% yttrium nitrate solution, and then 2 parts of citric acid were added by weight and mixed and stirred at a stirring speed of 800 r / min for 40 minutes. After stirring, the mixture was washed with water and dried to obtain a regulator.
[0129] The preparation method of the impregnation liquid of this embodiment is:
[0130] S11: irradiating the hydroxyapatite in a proton irradiation box for 12.5 minutes at an irradiation power of 370 W, and obtaining irradiated hydroxyapatite after the irradiation is completed;
[0131] The irradiated hydroxyapatite is immersed in a sufficient amount of sodium alginate solution, the ultrasonic power is 425W, the immersion time is 25 minutes, and the immersion is completed to obtain an immersed hydroxyapatite agent;
[0132] S12: 4 parts of the impregnated hydroxyapatite agent, 2 parts of stearic acid, 5.5 parts of sodium lignin sulfonate solution and 2.5 parts of silane coupling agent KH550 are mixed uniformly to obtain an impregnation solution.
[0133] The mass fraction of the sodium alginate solution in this embodiment is 5%; the mass fraction of the sodium lignin sulfonate solution is 6.5%.
[0134] This embodiment also provides a bio-based fabric, which is prepared by the above-mentioned method for preparing a bio-based fabric.
[0135] This embodiment also provides a garment made of bio-based fabrics.
[0136] Comparative Example 1:
[0137] The difference from Example 3 is that the modified bio-based polyamide fiber is prepared directly by using the existing bio-based polyamide 56 chips and melt spinning technology without any improvement or treatment.
[0138] Comparative Example 2:
[0139] The difference from Example 3 is that no regulator is added in the preparation of the modified bio-based polyamide fiber.
[0140] Comparative Example 3:
[0141] The difference from Example 3 is that no heat-treated nano-bentonite is added in the preparation of the regulator.
[0142] Comparative Example 4:
[0143] The difference from Example 3 is that no graphene is added in the preparation of the regulator.
[0144] Comparative Example 5:
[0145] The difference from Example 3 is that in the preparation of the regulator, the yttrium nitrate solution is replaced by deionized water, and sodium dodecylbenzene sulfonate is not added.
[0146] Comparative Example 6:
[0147] The difference from Example 3 is that no modification liquid treatment is used in the preparation of the modified bio-based polyamide fiber.
[0148] Comparative Example 7:
[0149] The difference from Example 3 is that no nano-silicon dioxide coordinator is added to the modified liquid.
[0150] Comparative Example 8:
[0151] The difference from Example 3 is that no nano-silicon dioxide and 6% by mass sodium silicate solution were added in the preparation of the nano-silicon dioxide coordinating agent.
[0152] Comparative Example 9:
[0153] The difference from Example 3 is that no phosphate buffer solution and glass fiber are added in the preparation of the nano-silicon dioxide coordinator.
[0154] Comparative Example 10:
[0155] The difference from Example 3 is that no lanthanum chloride solution and silane coupling agent KH560 are added to the modified solution.
[0156] Comparative Example 11:
[0157] The difference from Example 3 is that no impregnation liquid treatment is used.
[0158] Comparative Example 12:
[0159] The difference from Example 3 is that no hydroxyapatite agent is added to the impregnation solution.
[0160] Comparative Example 13:
[0161] The difference from Example 3 is that no sodium lignin sulfonate solution and silane coupling agent KH550 are added to the impregnation liquid.
[0162] The bio-based fabric products of Examples 1 to 3 and Comparative Examples 1 to 13 were subjected to conventional performance tests on flame retardancy, thermal insulation and stain resistance. The test results are shown in Table 1.
[0163] Table 1: Performance test results of bio-based fabric products of Examples 1 to 3 and Comparative Examples 1 to 13
[0164]
[0165] It can be seen from Table 1 that the product of Example 3 has an excellent limiting oxygen index, and at the same time has excellent thermal insulation rate and oil repellency. The thermal insulation, flame retardancy and oil resistance of the product can be coordinated and improved. The products of Comparative Examples 1-13 are not as good as the product of Example 3 of the present invention.
[0166] The test product was washed 20 times in water at 65°C to test the heat resistance and water washing resistance, and then washed 50 times in water at 65°C to test the water washing stability. The test results are shown in Table 2.
[0167] Table 2: Test results of water-washing stability of products of Examples 1 to 3 and Comparative Examples 1 to 13
[0168]
[0169] As can be seen from Table 2, the product of Example 3 has a significant effect on product performance stability under the conditions of 20 and 50 washings at 65°C, and a significant effect on water washing resistance stability in the change from 20 to 50 times;
[0170] The modified bio-based polyamide fiber was directly made by using the existing bio-based polyamide 56 chips and melt spinning technology without any improvement or impregnation treatment. The performance of the product showed a significant deterioration trend.
[0171] No regulator was added in the preparation of the modified bio-based polyamide fiber, no heat-treated nano-bentonite was added in the preparation of the regulator, no graphene was added in the preparation of the regulator, deionized water was used instead of yttrium nitrate solution in the preparation of the regulator, and no sodium dodecylbenzene sulfonate was added; the performance of the products showed a trend of deterioration, and the performance effects of the products obtained by different methods showed a trend of deterioration;
[0172] The modified bio-based polyamide fiber was not treated with a modifying liquid, the modified liquid was not added with a nano-silica coordinator, the nano-silica and 6% sodium silicate solution were not added in the preparation of the nano-silica coordinator, the phosphate buffer solution and glass fiber were not added in the preparation of the nano-silica coordinator, and the lanthanum chloride solution and silane coupling agent KH560 were not added in the modified liquid. The performance of the products showed a trend of deterioration to varying degrees.
[0173] In addition, when no regulator was added in the preparation of modified bio-based polyamide fibers, the performance stability of the products showed a significant deterioration trend under the conditions of 20 and 50 washes at 65°C. The treatment with the regulator had a significant improvement effect on the performance stability of the products.
[0174] The modified bio-based polyamide fiber obtained by combining the modified liquid obtained by the method of the present invention with the regulator of the present invention has the most significant performance effect of the product, and other methods are not as obvious as the effect of the present invention;
[0175] The performance of the products tended to deteriorate when no hydroxyapatite agent, sodium lignin sulfonate solution and silane coupling agent KH550 were added to the impregnation liquid. The impregnation liquid obtained by the specific method of the present invention had the most significant product performance effect.
[0176] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0177] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a bio-based fabric, characterized in that: The following steps are involved: Step 1: Weigh the raw materials by weight: 40-45 parts of polyester fiber, 30-35 parts of modified bio-based polyamide fiber, and 10-15 parts of blended yarn; wherein the blended yarn is made by spinning polyester fiber and carbon fiber in a weight ratio of 2:1; Step 2: respectively immersing the polyester fiber, modified bio-based polyamide fiber, and blended yarn in the step 1 into the impregnation liquid for modification and impregnation treatment, taking out and drying after the impregnation, to obtain the impregnated polyester fiber, modified bio-based polyamide fiber, and blended yarn; Step 3: Weaving the impregnated polyester fiber, modified bio-based polyamide fiber, and blended yarn into a knitted fabric body using a large circular machine; Step 4: Roll up the knitted fabric and store it in storage to obtain the bio-based fabric; The preparation method of the modified bio-based polyamide fiber is: S01: mixing the bio-based polyamide 56 slices and the regulator in a weight ratio of 5:2 to obtain regulated bio-based polyamide 56 slices; S02: Preparation of modified solution: S021: 3-5 parts of nano-silicon dioxide, 1-3 parts of sodium silicate solution with a mass fraction of 5-7%, and 2-5 parts of phosphate buffer solution with a pH value of 5.5 are uniformly mixed by weight, and then 2-4 parts of glass fiber are added by weight to mix and ball-milled at a ball-milling speed of 1000-1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a nano-silicon dioxide coordinator; S022: 2-5 parts of chitosan solution and 2-4 parts of nano-silicon dioxide coordinator are mixed and added to 4-7 parts of lanthanum chloride solution, and then 3-5 parts of magnesium hydroxide flame retardant and 2-4 parts of silane coupling agent KH560 are added and mixed sufficiently to obtain a modified solution; S03: Then, the adjusted bio-based polyamide 56 slices are subjected to ultrasonic modification in a modification liquid of 4 to 7 times the total weight of the adjusted bio-based polyamide 56 slices, and after the modification is completed, the modified polyamide body is filtered and dried to obtain a modified polyamide body, and finally the modified polyamide body is subjected to melt spinning technology to obtain a modified bio-based polyamide fiber; The preparation method of the regulator is: The nano-bentonite is first heat-treated at 250-270°C for 5-10 minutes, and then cooled to 55°C at a rate of 2-5°C / min and heat-treated to obtain heat-treated nano-bentonite; 4-7 parts of heat-treated nano-bentonite, 1-3 parts of sodium dodecylbenzene sulfonate, and 2-5 parts of graphene are added to 6-10 parts of 5% by weight yttrium nitrate solution, and then 1-3 parts of citric acid are added to the mixture and stirred at a stirring speed of 750-850 r / min for 35-45 minutes. After the stirring is completed, the mixture is washed with water and dried to obtain a conditioning agent; The preparation method of the impregnation solution is: S11: irradiating the hydroxyapatite in a proton irradiation box for 10-15 minutes at an irradiation power of 350-400W, and obtaining irradiated hydroxyapatite after the irradiation is completed; The irradiated hydroxyapatite is immersed in a sufficient amount of sodium alginate solution, the ultrasonic power is 400-450W, the immersion time is 20-30min, and the immersion is completed to obtain the immersed hydroxyapatite agent; S12: 3-5 parts of the impregnated hydroxyapatite agent, 1-3 parts of stearic acid, 4-7 parts of sodium lignin sulfonate solution and 2-3 parts of silane coupling agent KH550 are uniformly mixed to obtain an impregnation solution.
2. The method for preparing a bio-based fabric according to claim 1, characterized in that: The impregnation pressure of the modified impregnation treatment is 10-15 MPa, and the impregnation time is 1-2 hours.
3. The method for preparing a bio-based fabric according to claim 1, characterized in that: The ultrasonic power of the ultrasonic modification treatment is 400-500W, and the ultrasonic time is 20-30min.
4. The method for preparing a bio-based fabric according to claim 1, characterized in that: The mass fraction of the chitosan solution is 2-5%; the mass fraction of the lanthanum chloride solution is 3-6%.
5. The method for preparing a bio-based fabric according to claim 1, characterized in that: The mass fraction of the sodium alginate solution is 4-6%; the mass fraction of the sodium lignin sulfonate solution is 5-8%.
6. A bio-based fabric, characterized in that: The bio-based fabric is prepared by the preparation method of any one of claims 1 to 5.
7. A garment, characterized in that: It is made from the bio-based fabric as claimed in claim 6.