Preparation method and application of a light-adjustable thermochromic film with information pattern

By combining reversible photochromic Stanhouse adduct with reversible thermochromic cholesteric liquid crystal, the problem of difficult to adjust the color temperature range of traditional thermochromic liquid crystals is solved, and flexible adjustment and simplified preparation is achieved, suitable for a variety of applications. application.

CN118707778BActive Publication Date: 2024-11-19GUANGDONG UNIV OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411196930.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-19
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The color discoloration temperature range of traditional thermochromic liquid crystals is difficult to adjust, and the preparation method is complex and costly, which limits its application flexibility and breadth.

Method used

The photo-regulated thermochromic Stanhouse adduct (DASAs) is combined with reversible thermochromic cholesteric liquid crystals and polymers, and the discoloration temperature range is regulated by light irradiation to prepare a photo-regulated thermochromic with information patterns. film.

Benefits of technology

It realizes flexible adjustment of the discoloration temperature range of thermochromic liquid crystals, simplifies the preparation process, reduces costs, improves the application applicability and pattern clarity of the film, and is suitable for the fields of anti-counterfeiting and decoration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118707778B_ABST
    Figure CN118707778B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of optical anti-counterfeiting technology, and discloses a light-adjustable thermochromic film with information patterns, and a preparation method and application thereof, wherein the method comprises: mixing chiral nematic liquid crystal, polymer and photochromic monomer in a good solvent of the three to prepare a mixed solution; coating the mixed solution on a substrate, drying, and forming a film; and marking the target pattern on the surface of the thermochromic film by covering the surface of the film with a light-transmissive mask plate having a target pattern, selectively irradiating the film with visible light or ultraviolet light, or marking the film surface with a target pattern as a marking pattern by an ultraviolet laser marker. The present invention achieves a response to thermal stimulation by cleverly combining a reversible photochromic monomer with a reversible thermochromic cholesteric liquid crystal and a polymer matrix. This composite material not only has excellent color-changing properties, but also has the characteristics of simple preparation and wide applicability, providing a new solution for the fields of anti-counterfeiting and decoration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of optical anti-counterfeiting, and in particular to a preparation method and application of a light-adjustable thermochromic film with an information pattern. Background Art

[0002] In the field of thermochromic liquid crystals, although the traditional preparation method can achieve the characteristic that the color of liquid crystals changes with temperature, its color change temperature range is often difficult to adjust after the preparation is completed, which greatly limits its flexibility and extensiveness in practical applications. In addition, the traditional preparation method may involve a complex chemical reaction polymerization process, which has high requirements for operating technology and high costs; or although the method is relatively simple, the required instruments are expensive, which is not conducive to large-scale production and promotion. Summary of the invention

[0003] In order to overcome the above technical difficulties, the present invention proposes a method for preparing a light-adjustable thermochromic film with information patterns, and realizes flexible adjustment of the color change temperature range by doping photochromic donor-acceptor Steinhaus adducts (DASAs). As a new type of photoresponsive molecule, DASAs have the characteristics of being able to undergo reversible configuration changes under light irradiation, accompanied by color changes, which provides a new way to adjust the color change temperature range of thermochromic liquid crystals.

[0004] To achieve the above object, on the one hand, the present invention provides a method for preparing a light-adjustable thermochromic film with an information pattern, which comprises the following steps:

[0005] S1. Mixing chiral nematic liquid crystal, polymer and photochromic monomer in a good solvent of the three to prepare a mixed solution, wherein:

[0006] The chiral nematic liquid crystal is a reversible thermochromic cholesteric liquid crystal, which is formed by mixing a chiral dopant with a nematic liquid crystal, wherein the chiral dopant is selected from at least one of S811, R811, CB15, R5011, and S5011, and the nematic liquid crystal is selected from at least one of E7, 5CB, 8CB, ZLI-4792, and TEB300;

[0007] The polymer is a material containing hydroxyl groups and capable of forming hydrogen bonds, and the preferred good solvent is water;

[0008] The structure of the photochromic monomer is shown in formula (1):

[0009] (1);

[0010] S2, coating the mixed solution on a base material, and drying to form a light-adjustable thermochromic film;

[0011] S3, by covering the surface of the thermochromic film with a light-transmissive mask plate having a target pattern, and then selectively irradiating the surface with visible light or ultraviolet light, or marking the surface of the thermochromic film with the target pattern as a marking pattern by a UV laser marking machine, so that the target pattern is marked on the surface of the thermochromic film.

[0012] As a further preferred technical solution of the present invention, the polymer is selected from at least one of polyurethane, polyvinyl alcohol, hydroxypropyl methylcellulose, sodium alginate and chitosan.

[0013] As a further preferred technical solution of the present invention, the amounts of the components of the mixed solution prepared in step S1 are as follows: the photochromic monomer accounts for 0.1-30wt%, the chiral nematic liquid crystal accounts for 1-50wt%, the total amount of the polymer and the solvent accounts for 50-99wt%, and the polymer and the solvent can form a polymer solution with a mass percentage concentration of 5-15%.

[0014] As a further preferred technical solution of the present invention, in step S2, the mixed solution is coated into a film by one of spin coating, blade coating and casting.

[0015] As a further preferred technical solution of the present invention, in step S2, the coating thickness of the mixed solution is 10-1000 μm.

[0016] As a further preferred technical solution of the present invention, in step S3, the exposure time when using a mask plate is 1 to 60 minutes, and the marking power of the ultraviolet laser marking machine is 0.05 to 3W.

[0017] As a further preferred technical solution of the present invention, in step S3, the wavelength of the ultraviolet light is 100-400 nanometers.

[0018] As a further preferred technical solution of the present invention, the target pattern is text, pattern, or a combination of text and pattern.

[0019] According to another aspect of the present invention, the present invention also provides a light-adjustable thermochromic film with information patterns, which is prepared by the above method.

[0020] According to another aspect of the present invention, the present invention also provides an application of a light-adjustable thermochromic film with an information pattern as an anti-counterfeiting label. Preferably, the target pattern is a barcode or a two-dimensional code with encrypted information, and the film can clearly display a recognizable barcode or two-dimensional code only at a specific temperature, thereby achieving anti-counterfeiting. Of course, the light-adjustable thermochromic film with an information pattern can also be used as a color-changing pattern decoration, such as a mural, a sticker, and the like.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention achieves the response to thermal stimulation by cleverly combining reversible photochromic donor-acceptor Steinhaus adducts (DASAs) with reversible thermochromic cholesteric liquid crystals (CLC) and polymer matrix. This composite material not only has excellent color-changing properties, but also has the characteristics of simple preparation and wide applicability, providing new solutions for the fields of anti-counterfeiting and decoration.

[0023] The light-adjustable thermochromic film with information patterns of the present invention is a mixture of chiral nematic liquid crystal, polymer and photochromic monomer, and can be coated on the surface of a variety of substrate materials, and the substrate materials have a wide range of applicability. After being irradiated with visible light, the photochromic monomer in the film will change from a strongly colored line to a colorless ring, or after being irradiated with ultraviolet light, the photochromic monomer will degrade, so that when the film temperature changes, before and after being irradiated with visible light or ultraviolet light mask, the film will present two different color change temperature ranges, so that the patterned area and the non-patterned area have different color changes with temperature changes, thereby achieving patterning; the film is placed under an ultraviolet laser marking machine, and laser marking is used, based on the same mechanism as ultraviolet light, and patterning can also be achieved.

[0024] The light-adjustable thermochromic film with information patterns of the present invention has clear, bright and rich patterns, and can present a variety of different colors depending on the temperature. It has a simple preparation method and a wide range of substrate applicability, and has broad application prospects in the fields of anti-counterfeiting and decoration. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0026] Figure 1 This is a comparison chart of the reflection spectra of the films doped with different contents of DASA in Examples 1-3 and Comparative Example 1 that change color with temperature.

[0027] Figure 2 This is a comparison diagram of the actual color change of the thin films doped with different contents of DASA in Examples 1-3 with temperature after exposure through a visible light mask.

[0028] Figure 3 The following are actual pictures of the films with 20 wt% DASA content in Examples 3 and 4 changing color with temperature after being exposed to visible light and ultraviolet light masks, respectively.

[0029] Figure 4 These are the actual pictures of the thin films obtained by ultraviolet laser etching with different powers in Examples 5-7, as well as the corresponding POM pictures.

[0030] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION

[0031] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0032] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0033] The structure of the photochromic monomer (DASA) used in the present invention is as follows (1):

[0034] (1).

[0035] The photochromic monomer DASA can be synthesized by conventional techniques, or by the following route:

[0036] .

[0037] The present invention provides a method for synthesizing the photochromic monomer DASA, which comprises the following specific steps:

[0038] S1. Synthesis of Compound A

[0039] S1-1. Add 6.5 g of aniline to a two-necked flask equipped with a reflux condenser and a constant pressure dropping funnel, and add 100 ml of anhydrous ethanol. Add 10 g of anhydrous potassium carbonate, 0.6 g of potassium iodide and 1.6 g of tetrabutylammonium bromide under magnetic stirring;

[0040] S1-2. Under nitrogen protection, the solution was magnetically stirred and heated to reflux, and a mixed solution of 6 g ethyl bromide and 50 ml anhydrous ethanol was added dropwise through a constant pressure dropping funnel at a dropping rate of 2 drops / s. After the addition was completed, the solution was magnetically stirred and refluxed for 12 hours;

[0041] S1-3. After the reaction is completed, the temperature of the reaction solution is lowered to room temperature, the filtrate is filtered and then spin-dried, and the compound A (ie, N-ethylaniline) is obtained as a white powder by recrystallization through ethyl acetate. The yield is measured to be 91.1%.

[0042] S2. Synthesis of Compound B

[0043] S2-1. Add 7.8 g N,N-dimethylbarbituric acid and 200 ml deionized water into a beaker and stir magnetically to dissolve.

[0044] S2-2. Slowly add 6 ml of 2-furan carboxaldehyde to the dimethyl barbituric acid solution. After the addition is complete, stir magnetically at room temperature for 1 h.

[0045] S2-3. After the reaction is completed, the residue is filtered out by suction and washed with water for several times to obtain compound B in the form of a yellow powder. The yield is measured to be 98.9%.

[0046] S3. Synthesis of reversible photochromic monomers

[0047] S3-1. Add 2.3 g of compound B and 20 ml of dichloromethane to a single-necked bottle and dissolve under magnetic stirring;

[0048] S3-2. Add 2 g of compound A to the above solution and react at room temperature with magnetic stirring for 12 h;

[0049] S3-3. After the reaction is completed, the mixture is concentrated by rotary evaporation, redissolved with a small amount of tetrahydrofuran, and then dropped into 50 times the volume of n-hexane. The mixture is filtered, and the filter residue is washed with tetrahydrofuran, deionized water, and ether in sequence to obtain a dark blue reversible photochromic monomer with a yield of 72.5%.

[0050] The photochromic monomer DASA structure of the present invention can achieve reversible configuration changes as shown below. Under the stimulation of visible light, linear DASA will isomerize to cyclic DASA; and cyclic DASA can be restored to linear DASA under heating conditions.

[0051] .

[0052] Based on the above characteristics of the photochromic monomer DASA, the present invention proposes a light-adjustable thermochromic film with information patterns. In order to allow those skilled in the art to further understand the technical solution of the present invention, the technical solution of the present invention is further described in detail below through specific embodiments and comparative examples.

[0053] Examples 1-3: 0.1wt%, 10wt%, 20wt% DASA content respectively

[0054] Three groups of examples were used to prepare light-adjustable thermochromic films with information patterns, and the only difference between them was the DASA content. The specific steps were as follows:

[0055] 1) DASA, 200 mg CLC (2.8 wt% R5011-8CB) and 20 g 10 wt% polyvinyl alcohol (PVA) aqueous solution were stirred at 1000 rpm for 5 h at 20-90 °C to obtain a uniformly mixed blue solution;

[0056] In the three groups of embodiments, the mass fraction of DASA in the whole material is 0.1wt%, 10wt% and 20wt% respectively (corresponding to 20mg, 200mg and 400mg respectively).

[0057] 2) At room temperature and away from light, the obtained blue solution was filtered and defoamed before being evenly coated on a clean glass. The solvent was then evaporated on a heating device at 50 degrees for 1 hour to remove the solvent, thereby obtaining a thermochromic film with a thickness of 100 microns.

[0058] 3) A mask containing a target pattern (composed of capital letters -GDUT) and only the pattern portion is light-transmissive is covered on the surface of the thermochromic film, and after irradiation with a strong flashlight for 0.5 hours, a thermochromic film with the target pattern is obtained.

[0059] Comparative Example 1:

[0060] As a control experiment of Example 3, a preparation method substantially the same as that of Example 3 was adopted, except that DASA in Example 3 was omitted, and only 200 mg CLC (2.8 wt % R5011-8CB) and 20 g of 10 wt % PVA aqueous solution were used as raw materials.

[0061] Example 1-3 The reflection spectrum of the film obtained in Comparative Example 1 as a function of temperature is shown in FIG. Figure 1 The three groups of thermochromic films obtained in Examples 1-3 can be observed to have obvious color changes with temperature under natural light. The patterns of the films changing with temperature are shown in Figure 2 As shown, by making the exposed area and the unexposed area present different colors at a specific temperature, the marked pattern can be clearly displayed. However, no pattern can be obtained in Comparative Example 1 because there is no photoresponsive material in the film prepared by this formula, and it is impossible to form an exposed area and an unexposed area with obvious color difference, so patterning cannot be achieved.

[0062] In Examples 1-3, as the DASA content increases, the film discoloration temperature range decreases (e.g. Figure 1 ), and the color change temperature range of the patterned part after exposure through the mask is larger than that before exposure. The color of the film comes from the Bragg reflection of the incident light by the spiral structure of CLC, and the pattern comes from the color difference caused by the change of DASA from a strong colored line to a colorless ring after visible light irradiation. Therefore, after the visible light irradiation of the mask plate, the present invention will present two areas of different colors that change with temperature, so that the marked target pattern can be displayed, and more patterns of different colors at the same temperature can be obtained by adjusting the DASA content.

[0063] In order to further demonstrate the beneficial technical effect of the present invention, the light-adjustable thermochromic film with information pattern of the present invention is used as an anti-counterfeiting label, and the target pattern in Example 3 (DASA is 20wt%) is replaced with a more complex two-dimensional code with encrypted information. If the two-dimensional code information is to be read, the anti-counterfeiting label needs to be at a specific temperature (20°C or 25°C) so that the two-dimensional code can be clearly displayed and scanned and read (see Figure 2 ). According to the different DASA contents in Examples 1-3, under the same exposure conditions, the temperature corresponding to the pattern being clearly displayed varies with the temperature, and an anti-counterfeiting label that can clearly display the QR code information at different predetermined temperatures can be designed according to the needs. Of course, the light-adjustable thermochromic film with information patterns can also be used as a thermochromic patterned ornament.

[0064] Example 4: 20wt% DASA content

[0065] The preparation method is substantially the same as that in Example 3, except that the irradiation with a strong flashlight for 0.5 hour in step 2) is replaced with irradiation with 365 nm ultraviolet light for 5 minutes.

[0066] The light-adjustable thermochromic films with information patterns obtained in Examples 3 and 4 are compared. Figure 3 As shown, it can be seen that Example 4 obtains a pattern that varies with temperature and has a larger difference in background color and brighter color than Example 3. The reason is that after DASA is irradiated with ultraviolet light, its molecular structure will be destroyed, resulting in photodegradation. Therefore, after irradiation with ultraviolet light through the mask plate, a more obvious pattern that varies with temperature will appear, which can be better applied to anti-counterfeiting labels.

[0067] Embodiment 5-7:

[0068] The preparation method is basically the same as that in Example 3, except that the obtained film is etched by 365 nm ultraviolet laser to form a pattern, and the excess dust is blown off the etched film with a hair dryer to obtain Figure 4 The photo-adjustable thermochromic film with information pattern and its POM image are shown with three different UV laser etching powers (0.05W, 2.5W and 5W). Figure 4 It can be seen that as the power of the UV laser etching increases, the patterning becomes more and more obvious, but the power is too high (5W), and the patterned part of the film is carbonized so that it does not change color.

[0069] Comparative Example 2:

[0070] As a control experiment of Example 3, a preparation method substantially the same as that of Example 3 was used, except that the photochromic monomer (DASA) was replaced with the structure of the following formula (2):

[0071] .

[0072] Comparative Example 2 will not be able to obtain any pattern, and no pattern can be obtained by changing the amount of formula (2) to 0.1-20%. The reason is that the structure of formula (2) has a strong absorbance, and it is difficult to change from a strongly colored line to a colorless ring under visible light irradiation, and no pattern can be obtained, so it is difficult to obtain an exposed area and an unexposed area with obvious color differences.

[0073] Comparative Example 3:

[0074] As a control experiment of Example 3, a preparation method substantially the same as that of Example 3 was used, except that the photochromic monomer (DASA) was replaced with the structure of the following formula (3):

[0075] .

[0076] Comparative Example 2 will not be able to obtain any pattern because the monomer of the structure of formula (3) interacts with hydrogen bonds in the material, making it easier for it to change from a strongly colored line to a colorless ring under visible light irradiation. Therefore, even by changing the exposure conditions, it is impossible to obtain an exposed area and an unexposed area with obvious color differences, thereby achieving patterning.

[0077] Based on Example 3 and Comparative Examples 2 and 3, it can be seen that one of the keys to achieving patterning in the present invention is to select a specific photochromic monomer (DASA) so that under visible light, ultraviolet light and ultraviolet laser marking, the color difference between the exposed area and the unexposed area is obvious, thereby preparing a photochromic film that can be cleaned and reveal a pattern at a specific temperature.

[0078] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a light-adjustable thermochromic film with information patterns, characterized in that: The following steps are involved: S1. Mixing chiral nematic liquid crystal, polymer and photochromic monomer in a good solvent of the three to prepare a mixed solution, wherein: The chiral nematic liquid crystal is a mixture of a chiral dopant and a nematic liquid crystal, the chiral dopant is selected from at least one of S811, R811, CB15, R5011, and S5011, and the nematic liquid crystal is selected from at least one of E7, 5CB, 8CB, ZLI-4792, and TEB300; The polymer is a material containing hydroxyl groups and capable of forming hydrogen bonds; The structure of the photochromic monomer is shown in formula (1): (1); S2, coating the mixed solution on a base material, and drying to form a light-adjustable thermochromic film; S3, by covering the surface of the thermochromic film with a light-transmissive mask plate having a target pattern, and then selectively irradiating the surface with visible light or ultraviolet light, or marking the surface of the thermochromic film with the target pattern as a marking pattern by a UV laser marking machine, so that the target pattern is marked on the surface of the thermochromic film.

2. The method for preparing a light-adjustable thermochromic film with information patterns according to claim 1, characterized in that: The polymer is selected from at least one of polyurethane, polyvinyl alcohol, hydroxypropyl methylcellulose, sodium alginate and chitosan.

3. The method for preparing a light-adjustable thermochromic film with information patterns according to claim 1, characterized in that: The amounts of the components of the mixed solution prepared in step S1 are as follows: the photochromic monomer accounts for 0.1-30wt%, the chiral nematic liquid crystal accounts for 1-50wt%, the total amount of the polymer and the solvent accounts for 50-95wt%, wherein the chiral dopant accounts for 2-5wt% of the chiral nematic liquid crystal, and the polymer and the solvent can form a polymer solution with a mass percentage concentration of 5-15%.

4. The method for preparing a light-adjustable thermochromic film with information patterns according to claim 1, characterized in that: In step S2, the mixed solution is coated into a film by one of spin coating, blade coating and casting.

5. The method for preparing a light-adjustable thermochromic film with information patterns according to claim 1, characterized in that: In step S2, the coating thickness of the mixed solution is 10-1000 μm.

6. The method for preparing a light-adjustable thermochromic film with information patterns according to claim 1, characterized in that: In step S3, the exposure time when using the mask plate is 1 to 60 minutes, and the marking power of the ultraviolet laser marking machine is 0.05 to 3W.

7. The method for preparing a light-adjustable thermochromic film with information patterns according to claim 1, characterized in that: Step S3, the wavelength of the ultraviolet light is 100-400 nanometers.

8. The method for preparing a light-adjustable thermochromic film with information patterns according to any one of claims 1 to 7, characterized in that: The target pattern is text, a pattern, or a combination of text and a pattern.

9. A light-adjustable thermochromic film with information patterns, characterized in that: The method is prepared by any one of claims 1 to 8.

10. Use of the light-adjustable thermochromic film with information pattern as claimed in claim 9 as an anti-counterfeiting label.