A method for formulating an optimized production process for sodium ion batteries

By using different magnification and free electrolyte measurements in sodium ion batteries, the optimization process is determined, and the problem of not being able to quickly form an excellent SEI film in the prior art is solved, and the goal of shortening process time and improving production efficiency is achieved.

CN118712544BActive Publication Date: 2024-11-05PINGYU ZHONGXING ENERGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411196136.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-05
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

Existing methods cannot quickly determine the optimal process for forming excellent SEI films, affecting the performance and production efficiency of sodium ion batteries.

Method used

By using different magnifications to charge to cut-off voltage at the preset temperature, dQ/dV-V curve chart is drawn, and combined with the free electrolyte measurement results, the optimization process is analyzed and determined, and the optimization process is formulated to shorten the process time. and reduce energy consumption.

Benefits of technology

Quickly and accurately determine the process steps, current and cut-off voltages, ensure the formation of excellent SEI films, improve equipment utilization, reduce energy consumption, and is suitable for various battery systems and material formulations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118712544B_ABST
    Figure CN118712544B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for formulating an optimized formation process of a sodium ion battery, which includes: taking the battery to be tested after the same batch of liquid injection and high temperature standing, charging to a cut-off voltage using different rate current formation at a preset temperature; making dQ / dV-V curves for different rate current formation batteries respectively; disassembling the sodium ion battery after charging with different rate current formation and measuring the free electrolyte; analyzing in combination with the dQ / dV-V curve and the measurement result, formulating the formation process of the sodium ion battery; wherein the measurement result includes the disassembly interface and the electrolyte retention amount. The present invention only needs to compare the dQ / dV-V curves of the different rate current formation charging process and a small amount of disassembly to quickly and accurately determine the optimal charging current and cut-off voltage range of each step of the formation process, thereby formulating the optimized formation process, which is highly reliable and simple to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a method for formulating an optimized production process of a sodium ion battery. Background Art

[0002] The formation process is an essential step in the production of sodium-ion batteries, which has the functions of activating electrode materials, improving the interface of sodium batteries, self-discharge, and circulation. When sodium-ion batteries are formed, a small amount of polar aprotic solvent in the electrolyte undergoes a reduction reaction after obtaining some electrons, and reacts with sodium ions to form an interface film with a thickness of about 100-120nm, which is the SEI film.

[0003] The formation of SEI film is mainly affected by factors such as the size of the formation current, vacuum degree and temperature. When the formation charging current is large, the high potential inorganic components are formed first, followed by the insertion of sodium ions, and finally the formation of organic components. When the formation current is small, the organic components of the SEI film begin to form quickly. In addition, when the battery is charged for the first time, the electrolyte is consumed and reacts, and a large amount of gas will be generated at different potentials. The gas discharge effect directly affects the battery interface and battery performance. Therefore, the formulation of the optimal formation process depends on whether the current size, vacuum degree and temperature parameter settings are optimal.

[0004] Existing methods cannot quickly determine the optimal formation process for forming a good SEI film. Summary of the invention

[0005] The present application proposes a method for formulating an optimized formation process for sodium ion batteries, which can quickly and accurately determine the formation steps, current and cut-off voltage, and formulate an optimal formation process, which can ensure that the process time is shortened, the equipment utilization rate is improved, and the energy consumption is reduced under the premise of forming an excellent SEI film.

[0006] The present invention discloses a method for formulating an optimized production process of a sodium ion battery, which comprises:

[0007] Step 1: Take the batteries to be tested from the same batch after injection and high temperature standing, and charge them to the cut-off voltage at different current rates at the preset temperature;

[0008] Step 2: Draw dQ / dV-V curves for the batteries formed by current at different rates in step 1;

[0009] Step 3: Disassembly of the sodium ion battery after charging at different current rates and measurement of free electrolyte;

[0010] Step 4: Analyze the dQ / dV-V curve and measurement results to develop a formation process for sodium-ion batteries; the measurement results include the disassembly interface and electrolyte retention.

[0011] Furthermore, the step 1 comprises:

[0012] Take multiple sodium ion batteries from the same batch, inject liquid into them and let them stand at high temperature for a preset time period. After standing, the batteries to be tested are charged at different rates to a cut-off voltage. The different rate currents are preset values, and the cut-off voltage is the designed upper limit voltage of the battery to be tested, which is determined according to the sodium ion battery material system.

[0013] Furthermore, the step 1 specifically includes:

[0014] Take 2n sodium ion batteries from the same batch, inject them with liquid and let them stand at high temperature for 24 to 36 hours. After standing, the batteries to be tested are charged at different rates to the cut-off voltage. The different rate currents are 0.01C to 1C. The cut-off voltage is the design upper limit voltage of the battery to be tested, which is determined according to the sodium ion battery material system.

[0015] Furthermore, the formation temperature in step 1 is 25-60°C.

[0016] Furthermore, the step 2 comprises:

[0017] The voltage capacity of the charging process at different rates in step 1 is differentiated, and a dQ / dV-V curve of the battery charging and discharging process is drawn with dQ / dV as the ordinate and voltage as the abscissa.

[0018] Furthermore, the step 3 comprises:

[0019] Disassemble and measure the free electrolyte in order from small to large charging rate current. When a battery with a bad interface is found, stop disassembling and measuring the remaining batteries charged with a higher rate current.

[0020] Furthermore, the step 4 comprises:

[0021] According to the dQ / dV-V curve drawn in step 2, the potentials and areas of the reaction peaks corresponding to the charge film-forming reaction peaks and sodium deintercalation reaction peaks at different current rates are compared to obtain the optimal charge current and cut-off voltage for formation. Combined with the disassembly situation in step 3, the optimal formation process is comprehensively formulated.

[0022] Furthermore, the optimization process is formulated comprehensively based on the disassembly situation in step 3, including:

[0023] Within the preset formation charging current range, as the formation charging rate increases, the intensities and potentials of the film-forming reaction peak and the sodium deintercalation reaction peak tend to be consistent, and there is no abnormality in the interface. At this time, the maximum current within the preset formation charging current range is determined as the optimal formation current, and the voltage corresponding to the reaction peak is determined as the optimal cutoff voltage of the film-forming reaction and the sodium deintercalation reaction. According to the determined optimal formation current and optimal cutoff voltage, an optimized formation process is formulated.

[0024] Due to the adoption of the above technical scheme, the present invention has the following advantages: the method proposed by the present invention can quickly and accurately determine the optimal formation charging current and cut-off voltage range of each step of the formation process by comparing the dQ / dV-V curves of the formation charging process with different current rates and only requires a small amount of disassembly, and formulates the optimized formation process, which can better solve the problem of determining the formation step, current and cut-off voltage of the sodium ion battery system, has high reliability and is simple to operate; at the same time, it has good universality and can be applied to various battery systems and various material formulations; it can also provide direction for optimizing the formation process, and achieve the goals of shortening the process time, improving equipment utilization, and reducing energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the embodiments of the present invention. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.

[0026] Figure 1 dQ / dV-V curves of different current rates of the battery of the embodiment of the present invention;

[0027] FIG. 2( a ), FIG. 2( b ), FIG. 2( c ), and FIG. 2( d ) are respectively disassembly interface diagrams of different current rate formation of a battery according to an embodiment of the present invention;

[0028] FIG2( e ) is a graph showing the relationship between different formation currents and liquid retention amounts according to an embodiment of the present invention;

[0029] Figure 3 Formulate a method flow chart for optimizing the sodium ion battery process of the present invention;

[0030] FIG. 4( a ) and FIG. 4( b ) are respectively diagrams of the negative electrode sheet interface of a battery fully charged after formation and fully charged and disassembled after capacity division according to an embodiment of the present invention. DETAILED DESCRIPTION

[0031] The present invention is further described in conjunction with the accompanying drawings and embodiments, and the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. All other embodiments obtained by ordinary technicians in this field should fall within the scope of protection of the embodiments of the present invention.

[0032] See also Figure 3 The present invention provides an embodiment of a method for formulating a sodium ion battery optimization process, which comprises the following steps:

[0033] S1. Take the batteries to be tested from the same batch after injection and high temperature standing, and charge them to the cut-off voltage at different current rates at the specified temperature; the specified temperature range is 25~60℃. The high temperature is 40℃ to 50℃.

[0034] In this embodiment, a plurality of sodium ion batteries from the same batch are taken, injected with liquid and left to stand at high temperature for a preset period of time. The batteries to be tested after standing are charged at different rates to a cut-off voltage. The currents at different rates are preset values, and the cut-off voltage is the designed upper limit voltage of the battery to be tested, which is determined according to the sodium ion battery material system.

[0035] In an optional embodiment, 2n sodium ion batteries from the same batch are taken, injected with liquid and left to stand at high temperature for 24 to 36 hours. The batteries to be tested after standing are charged at different rates to a cut-off voltage, and the different rate currents are 0.01C to 1C. The cut-off voltage is the design upper limit voltage of the battery to be tested, which is determined according to the sodium ion battery material system.

[0036] In an optional embodiment, the formation temperature of the battery is 25-60°C.

[0037] The purpose of standing at high temperature after liquid injection is to ensure that the electrolyte is fully infiltrated, increase the contact area and reaction activity between the electrolyte and the electrode, and promote the formation of a more stable SEI film on the surface of the negative electrode. In addition, due to the effect of temperature during the standing period, the unstable substances will further react or transform, which is conducive to the internal structure of the battery to be more stable and reduce the probability of side reactions in the subsequent charging and discharging process. The formation temperature of the battery affects the formation effect by affecting the viscosity and conductivity of the electrolyte and the diffusion rate of the ions of the electrode material. Generally speaking, the higher the formation temperature, the lower the viscosity of the electrolyte, the higher the conductivity of the electrolyte, and the faster the diffusion rate of the ions of the electrode material. Therefore, the smaller the polarization, the better the formation effect.

[0038] However, when the temperature is too high, the structure of the SEI film that has been formed will be destroyed and its composition will be changed; at the same time, the electrolyte is an organic solvent solution, and too high a temperature will accelerate the volatilization rate of the low-boiling point components in the electrolyte, affecting the formation effect; conversely, if the temperature is too low, it will also affect the viscosity and conductivity of the electrolyte and the ion diffusion rate of the electrode material, which is not conducive to the formation effect. The formation temperature of 25°C to 60°C can achieve the viscosity and conductivity of the electrolyte and the ion diffusion rate of the electrode material to meet the test requirements. Therefore, for the battery optimal formation process formulation technology of the present invention, in step S2, high-temperature formation or room-temperature formation can be selected as needed, and the corresponding temperature can be selected at room temperature and above, and high temperature such as 60°C.

[0039] The current density is the most critical factor in determining the quality of the SEI. A high SEI current density and a fast nucleus formation rate will lead to a loose structure of the SEI film and weak adhesion to the negative electrode surface. On the contrary, at low current density, the nucleus formation rate is slow, and the structure of the SEI film is more compact. The ionic conductivity of the SEI film formed at a high current density is greater than that of the SEI film formed at a low current density. Long-term testing has found that the current for sodium-ion batteries to form a good SEI film is usually 0.01C~0.03C. In addition, in order to ensure that sodium ions are completely deintercalated during the formation charging process, the charging current does not exceed 1C. Therefore, the formation charging rate current can be selected from 0.01C. The specific rate currents to be implemented depend on the situation.

[0040] S2, making dQ / dV-V curves for the batteries formed by current at different rates in step S1;

[0041] In this embodiment, the voltage capacity of S1 in the charging process at different rates is differentiated, and a dQ / dV-V curve of the battery charging and discharging process is drawn with dQ / dV as the ordinate and voltage as the abscissa; Q represents capacity; dQ / dV represents the capacity contained in the material within the unit voltage range, which is dimensionless.

[0042] The physical meaning of the dQ / dV curve is the capacity of the material within a unit voltage range. For the positive and negative electrode materials of sodium-ion batteries, there is a voltage platform. The negative electrode capacity is higher on the voltage platform, which means that there is a lot of capacity within a very small voltage fluctuation range, so it is represented by a characteristic peak on the curve. Each peak on the curve represents an electrochemical reaction. Since the reaction potentials of different materials are different, the position and height in the dQ / dV curve will also be different. The peak position represents the potential of the electrochemical reaction, and the peak intensity represents the strength of the electrochemical reaction. By comparing and analyzing the film-forming reaction peaks and the sodium deintercalation reaction peak positions and the intensities of each reaction peak in the formation charging process at different current rates, the charging cutoff voltage and current range of each step of the formation can be determined.

[0043] As charging proceeds, the internal voltage of the battery increases, accompanied by gas generation. Once the gas production rate is higher than the exhaust rate of the injection hole, the gas will gather between the diaphragms inside the battery, resulting in uneven contact between the diaphragm and the negative electrode surface, thereby affecting the embedding process of sodium ions on the negative electrode surface, making the sodium ions unevenly distributed on the negative electrode surface during the electrochemical reaction, causing metallic sodium or sodium compounds to deposit on the negative electrode surface. Therefore, a suitable formation cutoff voltage can improve the initial charge and discharge efficiency of the battery, reduce the internal resistance of the battery, and improve the battery cycle performance. In addition, the higher the voltage, the more unstable the electrolyte, and there will be more sodium for the reduction reaction, reducing the sodium content of the sodium ion battery. In actual production, selecting the lowest voltage and maximum current according to the determined cutoff voltage and current range can reduce the formation time, save electricity costs, and improve production efficiency.

[0044] The dQ / dV-V curve is as follows Figure 1 shown.

[0045] S3, disassembling the sodium ion battery after being charged by current formation at different rates;

[0046] In this embodiment, the free electrolyte is disassembled and measured in order from small to large charging rate currents. When a battery with a bad interface is found, the disassembly and measurement of the remaining batteries charged with higher rate currents can be stopped.

[0047] By comparing and analyzing the dQ / dV curves of different current rate formation charging, the charging cutoff voltage and current range of each step of the formation are determined. The results are all based on theoretical analysis, but in actual production, they will be affected by factors such as environmental fluctuations. Further comparative analysis of the disassembly interface is needed to see if it is consistent with the theoretical results. Among them, according to the effect of the formation current density on SEI mentioned above, it is only necessary to disassemble the battery after the minimum current rate formation charging. As the current increases, the interface gradually changes from good to various abnormalities. When the disassembly interface becomes bad, stop disassembling. The measurement comparison of the free electrode liquid is also direct evidence of whether the reaction SEI is good. The loosely structured SEI film can infiltrate more electrolyte, and the free electrolyte is correspondingly less.

[0048] S4. Analyze the dQ / dV-V curve and disassembly interface data to develop the formation process of sodium-ion batteries.

[0049] In this implementation, based on the dQ / dV-V curve drawn by S2, the potentials and areas of the reaction peaks corresponding to the charging film-forming reaction peaks and the sodium deintercalation reaction peaks at different current rates are compared to obtain the optimal charging current and cut-off voltage for formation, and the optimal formation process is comprehensively formulated in combination with the disassembly of S3.

[0050] Among them, the optimal process is formulated comprehensively based on the disassembly of S3, including:

[0051] Within the preset formation charging current range, as the formation charging rate increases, the intensities and potentials of the film-forming reaction peak and the sodium deintercalation reaction peak tend to be consistent, and there is no abnormality in the interface. At this time, the maximum current within the preset formation charging current range is determined as the optimal formation current, and the voltage corresponding to the reaction peak is determined as the optimal cutoff voltage of the film-forming reaction and the sodium deintercalation reaction. According to the determined optimal formation current and optimal cutoff voltage, an optimized formation process is formulated.

[0052] The turning current of poor interface and free electrolyte amount is the upper limit current for the formation of good SEI. The current of the film-forming reaction potential of the optimized process can be selected to be lower than this upper limit current. The voltage and current of other reactions such as sodium deintercalation are directly determined according to the reaction peak intensity and area, thereby formulating the optimized process of sodium ion battery.

[0053] The present invention can quickly and accurately determine the optimal charging current and cut-off voltage range of each step of the formation process by simply comparing dQ / dV-V curves of formation charging processes with different current rates and a small amount of disassembly, thereby formulating an optimized formation process with high reliability and simple operation; at the same time, it has good universality and can be applied to various battery systems and various material formulations; it can also provide direction for optimization of the formation process, and achieve the goals of shortening the process time, improving equipment utilization, and reducing energy consumption.

[0054] Example 1

[0055] This example uses a 50mm laminate (59 positive layers and 60 negative layers) 160mm 119mm polyanion + hard carbon system aluminum shell sodium ion battery, the battery design capacity is 56Ah, the electrolyte is LG6085 model of Blue Solid manufacturer, the injection volume is 390g, and it is left at high temperature for 24 hours after injection. 16 batteries from the same batch are selected and divided into 8 groups, 2 batteries in each group.

[0056] Eight groups of batteries were charged at different current rates: 0.01C, 0.02C, 0.03C, 0.05C, 0.075C, 0.1C, 0.2C, 0.33C constant current charging was performed at a temperature of 45°C and a vacuum environment of -60KPa, and the charging cut-off voltage was 3.4V. The voltage capacity of the formation charging process was differentiated, and a dQ / dV-V curve of the battery formation charging and discharging process was drawn with dQ / dV as the ordinate and voltage as the abscissa.

[0057] Analyze and formulate the optimal formation process: dQ / dV-V curves from different current rates ( Figure 1As shown in the figure, it can be seen that the film-forming reaction peak near 1.65V and the reaction peak near 2.2V both shift to the right with the increase of current, and the reaction intensity increases, indicating that the film-forming reaction is greatly affected by the current density, and as the current density increases, the intensity of the electrochemical reaction peak gradually increases under the influence of battery polarization. When the current is ≤0.03C before 1.65V and the current is ≤0.1C before 2.2V, the reaction peak position and intensity are basically the same, so the current before 1.65V is max0.03C, and the current before 2.2V is max0.1C; 2.85V and 3.18V are sodium deintercalation reaction peaks. When the current is ≤0.1C, the potential and intensity of the 2.85V reaction peak do not change significantly. Therefore, the current at 2.85V is max0.1C, and the reaction peak at 3.18V is less affected by the current density, so the current after 2.85V can be appropriately increased. Combined with the results of current formation disassembly and free electrolyte testing at different rates, as shown in Figures 2(a), 2(b), 2(c), 2(d) and 2(e), when the current is lower than 0.03C, the SEI film is dense and uniform as a whole. When the current is higher than 0.03C, the quality of the SEI film deteriorates significantly (dark spots, sodium precipitation), and areas with obvious color differences appear. The electrolyte also infiltrates more significantly. Therefore, the SEI film formed by large current (≥0.03C) has a loose structure and poor quality.

[0058] Based on all the above results, the optimal charging current of this embodiment can be formulated as follows: the first step charging current is 0.03C, and the cut-off voltage is 1.65V; the second step charging current is 0.1C, and the cut-off voltage is 2.85V; the third step charging current is slightly less than 0.03C, and the cut-off voltage is 3.4V.

[0059] To further confirm the reliability of the present method, an interface evaluation was performed on the sodium-ion battery formed by the optimized process provided in this embodiment: the battery was fully charged and disassembled to observe the interface state of the negative electrode sheet after formation, as shown in Figures 4(a) and 4(b).

[0060] The test results show that the full charge interface after formation and capacity separation is very good, without any abnormalities such as black spots, sodium precipitation, wrinkles, and color difference.

[0061] The above results show that the formation process determined by the sodium-ion battery optimization process formulation method is very accurate and reliable.

[0062] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for formulating an optimized production process for a sodium ion battery, characterized in that: include: Step 1: Take the batteries to be tested from the same batch after injection and high temperature standing, and charge them to the cut-off voltage at different current rates at the preset temperature; Step 2: Draw dQ / dV-V curves for the batteries formed by current at different rates in step 1; Step 3: Disassembly of the sodium ion battery after charging at different current rates and measurement of free electrolyte; Step 4: Analyze the dQ / dV-V curve and the measurement results to develop a formation process for the sodium-ion battery; the measurement results include the disassembly interface and the electrolyte retention volume; The step 3 comprises: Disassemble and measure the free electrolyte in order from small to large charging rate currents. When a battery with a bad interface is found, stop disassembling and measuring the remaining batteries charged with higher rate currents. The step 4 comprises: According to the dQ / dV-V curve drawn in step 2, the potentials and the areas of the reaction peaks corresponding to the charge film formation reaction peaks and the sodium deintercalation reaction peaks at different current rates are compared to obtain the optimal charge current and cut-off voltage for formation, and the optimal formation process is comprehensively formulated in combination with the disassembly situation in step 3; The optimization process is formulated comprehensively based on the disassembly situation in step 3, including: Within the preset formation charging current range, as the formation charging rate increases, the intensities and potentials of the film-forming reaction peak and the sodium deintercalation reaction peak tend to be consistent, and there is no abnormality in the interface. At this time, the maximum current within the preset formation charging current range is determined as the optimal formation current, and the voltage corresponding to the reaction peak is determined as the optimal cutoff voltage of the film-forming reaction and the sodium deintercalation reaction. According to the determined optimal formation current and optimal cutoff voltage, an optimized formation process is formulated.

2. The method for formulating an optimized production process for a sodium ion battery according to claim 1, characterized in that: The step 1 comprises: Take multiple sodium ion batteries from the same batch, inject liquid into them and let them stand at high temperature for a preset time period. After standing, the batteries to be tested are charged at different rates to a cut-off voltage. The different rate currents are preset values, and the cut-off voltage is the designed upper limit voltage of the battery to be tested, which is determined according to the sodium ion battery material system.

3. The method for formulating an optimized production process for a sodium ion battery according to claim 1, characterized in that: The step 1 specifically includes: Take 2n sodium ion batteries from the same batch, inject them with liquid and let them stand at high temperature for 24 to 36 hours. After standing, the batteries to be tested are charged at different rates to the cut-off voltage. The different rate currents are 0.01C to 1C. The cut-off voltage is the design upper limit voltage of the battery to be tested, which is determined according to the sodium ion battery material system.

4. The method for formulating an optimized production process for a sodium ion battery according to claim 1, characterized in that: The formation temperature in step 1 is 25-60°C.

5. The method for formulating an optimized production process for a sodium ion battery according to claim 1, characterized in that: The step 2 comprises: The voltage capacity of the charging process at different rates in step 1 is differentiated, and a dQ / dV-V curve of the battery charging and discharging process is drawn with dQ / dV as the ordinate and voltage as the abscissa.