High-strength directional porous bone repair scaffold material and preparation method thereof

By introducing silk fibroin into calcium alginate scaffolds and using directional freeze-drying technology to form a directional porous structure, the problem of insufficient mechanical properties of calcium alginate scaffold materials is solved, and a balance between high strength and high porosity of bone defect repair materials is achieved. Improved biocompatibility and biological induction effect.

CN118718113APending Publication Date: 2024-10-01CHANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410799817.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing calcium alginate scaffold materials have insufficient mechanical properties and osteogenic induction capabilities, and it is difficult to balance good mechanical strength and high porosity, resulting in insufficient biocompatibility and biological induction effects of bone defect repair materials.

Method used

By blending silk fibroin with a calcium ion solution and then introducing it into a sodium alginate solution, directional freeze-drying technology is used to arrange the silk fibroin along the microchannels in the calcium alginate-based scaffold to form a directional porous structure, improving the mechanical properties and performance of the material. Porosity balance.

Benefits of technology

A silk fibroin composite calcium alginate scaffold material with high strength, good biocompatibility and physical and chemical properties was obtained, which is suitable for bone defect repair and has excellent mechanical properties and biological induction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004903028680000011
    Figure HDA0004903028680000011
  • Figure HDA0004903028680000012
    Figure HDA0004903028680000012
  • Figure HDA0004903028680000021
    Figure HDA0004903028680000021
Patent Text Reader

Abstract

The invention discloses a high-strength directional porous bone repair scaffold material and a preparation method thereof, and belongs to the field of tissue engineering scaffold materials. The preparation method comprises the following steps: uniformly blending a silk fibroin solution and a calcium chloride solution, introducing the mixture into a sodium alginate solution, placing the mixture on a metal substrate, carrying out liquid nitrogen directional freezing, and freeze-drying the pre-frozen composite material in a vacuum freeze-drying machine. Finally, the silk fibroin composite calcium alginate scaffold material with the high-strength oriented porous structure is obtained. The material obtained by the invention has the characteristics of excellent mechanical properties, good water absorption, porosity and biocompatibility, and provides a new choice for tissue engineering scaffold materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of tissue engineering scaffold materials, and specifically relates to a high-strength directional porous bone repair scaffold material and a preparation method thereof, and particularly relates to a silk fibroin composite calcium alginate scaffold material with a directional porous structure and a preparation method thereof. Background Art

[0002] Bones are important organs that maintain body movement and protect internal organs. Bone defects are common orthopedic diseases in clinical work. Due to the long treatment cycle and great damage to the body, bone defects are still one of the main challenges in clinical practice. Nowadays, with the increase in the incidence of bone diseases in the elderly population, the demand for bone repair materials has also increased. Clinical treatments for bone defects include non-invasive and invasive treatments. Surgical treatment is the most effective method for treating bone defects, such as bone transplantation, Masquelet technique, Ilizarov technique, etc. Bone transplantation in traditional treatment methods has disadvantages such as immune rejection and insufficient donors. At this stage, the treatment method of implanting metal stents faces problems such as bioincompatibility, so it is very important to find a suitable bone defect repair material.

[0003] Alginate-based scaffolds can provide excellent carriers for cells and growth factors due to their good biocompatibility, excellent plasticity, and wide sources, and are widely used in bone tissue engineering research. Sodium alginate is the main source of alginate. It is a high-molecular polysaccharide, a linear polymer formed by β-D-mannuronic acid and α-L-guluronic acid connected by glycosidic bonds. However, in the process of preparing calcium alginate scaffolds, single calcium alginate scaffold materials have problems with insufficient mechanical strength or osteogenic induction ability, so it is very important to improve the mechanical properties of calcium alginate scaffolds. Silk fibroin is a natural fiber material extracted from silk. It is similar in structure to collagen in the extracellular matrix, has low immunogenicity and high mechanical properties, and can promote the adhesion and growth of osteoblasts in the scaffold. Silk fibroin molecules with good mechanical properties can be used to improve the brittle shortcomings of calcium alginate materials. Silk fibroin is composed of eighteen kinds of amino acids, which contain a large number of amino, hydroxyl and amide groups. Calcium alginate contains a large number of hydroxyl and carbonyl groups. The hydrogen bonding between hydroxyl-hydroxyl, hydroxyl-amide and amino-carbonyl groups can be used to increase the interaction between silk fibroin and calcium alginate molecules and enhance the mechanical properties of the material.

[0004] At present, there is a study on mixing silk fibroin (SF) and sodium alginate (SA) and freeze-drying them, and soaking them in calcium chloride to obtain a scaffold material with high porosity and mechanical strength ( A novel silk fibroin / sodium alginate hybrid Scaffolds ), or adding octacalcium phosphate as a mineralization precursor of bone apatite crystals to increase the compressive strength of silk fibroin and sodium alginate composite scaffold materials ( Biocompatible octacalcium phosphate / sodium alginate / silk fibroin composite scaffolds for bone regeneration ). However, these preparation methods still have problems such as insufficient mechanical strength, complex preparation methods, or unsatisfactory bone vascularization.

[0005] The ideal scaffold material for bone defect repair should have good biocompatibility, reasonable internal space structure, excellent mechanical properties, constant degradation rate and effective bioinduction. However, in the development of actual materials science, it is often difficult to balance good mechanical strength and high porosity. How to control the balance between mechanical strength and the porosity and internal connectivity of the material is still a major problem in the research of scaffold materials for bone defect repair. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a high-strength directional porous bone repair scaffold material and a preparation method thereof. The present invention introduces silk fibroin into a sodium alginate solution after being blended with a calcium ion solution, and the silk fibroin molecules are uniformly dispersed in the sodium alginate solution by calcium ion migration, and the silk fibroin is guided to be arranged and distributed along the microchannels in the calcium alginate-based scaffold by directional freeze drying technology, and finally freeze dried to prepare a silk fibroin composite calcium alginate scaffold (SA / SF) with a directional porous structure.

[0007] The purpose of the present invention is achieved through the following technical solutions: A method for preparing a high-strength oriented porous silk fibroin composite calcium alginate bone repair scaffold material comprises the following specific steps: (1) Providing silk fibroin solution, calcium chloride solution and sodium alginate solution; (2) pouring the sodium alginate solution into the mold, mixing the silk fibroin solution and the calcium chloride solution evenly, and then dropping them into the sodium alginate solution to obtain a mixed solution, which is then placed on a metal substrate, and the bottom of the assembled device is immersed in liquid nitrogen for directional freezing; (3) The mold and the sample after directional freezing are quickly placed in a vacuum freeze dryer for freeze drying to obtain an directional porous silk fibroin composite calcium alginate scaffold material.

[0008] Furthermore, in the silk fibroin solution in step (1), the mass fraction of silk fibroin is 4-7%. The silk fibroin solution is prepared by dissolving natural silk after degumming in a lithium bromide solution, and dialyzing to obtain a silk fibroin solution of a certain concentration.

[0009] Furthermore, in the sodium alginate solution in step (1), the mass fraction of sodium alginate is 2-5%.

[0010] Furthermore, the concentration of calcium chloride in step (1) is 0.3 mol / mL to 0.5 mol / mL.

[0011] Furthermore, the mass fraction of silk fibroin in the mixed solution in step (2) is 10% to 30%.

[0012] Furthermore, in step (2), the ratio of sodium alginate to calcium chloride is m=[Ca 2 + ] / [COO - ]=0.15~0.2.

[0013] Furthermore, the mold in step (2) is a hollow columnar structure, and its material is a high-density polytetrafluoroethylene polymer with excellent low-temperature resistance, and its size is a cross-sectional area of ​​5~15cm 2 , height is 0.5~2.5cm.

[0014] Furthermore, the metal substrate in step (2) includes a metal plate with high thermal conductivity such as a copper plate, a gold plate, an aluminum plate, etc., and its thickness is less than 1 mm.

[0015] Furthermore, the liquid nitrogen directional freezing time in step (2) is more than 3 minutes. During the freeze-drying process, as the solid ice crystals sublimate, the silk fibroin composite calcium alginate scaffold presents a directional porous structure. Preferably, the liquid nitrogen directional freezing time in step (2) is 3 to 4 minutes.

[0016] Furthermore, the freeze-drying time of step (3) is 46 to 48 hours.

[0017] Furthermore, the preparation method of the above-mentioned high-strength oriented porous silk fibroin composite calcium alginate bone repair scaffold material also includes step (4), treating the scaffold with calcium chloride to prevent the scaffold material from gelling too quickly after absorbing water, and then soaking it in deionized water, and finally obtaining the oriented porous silk fibroin composite calcium alginate scaffold material after freeze-drying.

[0018] The present invention aims at the problem of insufficient mechanical stability of calcium alginate scaffolds. The silk fibroin solution is creatively blended with a calcium ion solution and then added to a sodium alginate solution. The silk fibroin molecules are evenly dispersed in the sodium alginate solution by calcium ion migration. The growth process of ice crystals is controlled by liquid nitrogen to drive the silk fibroin to grow in a specific direction so that the silk fibroin composite calcium alginate scaffold presents a directional arrangement. The present invention combines directional freezing technology with the preparation of silk fibroin composite calcium alginate scaffold materials, thereby improving the mechanical properties of the calcium alginate scaffold material while maintaining an ideal pore structure, thereby obtaining a silk fibroin composite calcium alginate scaffold material with good physical and chemical properties and biocompatibility. The directional porous silk fibroin composite calcium alginate scaffold material obtained by the present invention has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1This is a diagram of the preparation of silk fibroin composite calcium alginate scaffold material; Figure 2 This is the finished product of silk fibroin composite calcium alginate scaffold material (SA / SF-DF); Figure 3 Fluorescence microscopy images of the cross section (left) and longitudinal section (right) of the silk fibroin composite calcium alginate scaffold material (SA / SF-DF); Figure 4 is the porosity of SA / SF-GC scaffold and SA / SF-DF scaffold; Figure 5 is the water absorption rate of SA / SF-GC scaffold and SA / SF-DF; Figure 6 Stress-strain curves of SA / SF-GC scaffolds and SA / SF-DF. DETAILED DESCRIPTION

[0020] In order to better understand the present invention, the present invention is further described below in conjunction with embodiments, but the scope of protection claimed by the present invention is not limited to the scope represented by the mentioned embodiments. Example 1

[0021] Sodium alginate, silk fibroin, calcium chloride, lithium bromide and acetic acid were used as raw materials to prepare a high-strength oriented porous silk fibroin composite calcium alginate scaffold material (SA / SF-DF). The preparation steps are as follows: (1) First, the natural silk was degummed and dissolved in a lithium bromide solution. After dialysis, a silk fibroin solution of a certain concentration was obtained. The concentration was tested by the loss on drying method, and then a silk fibroin solution with a mass fraction of 6.5% was obtained through concentration or dilution. (2) Then, 2 mL of a 2.5% mass fraction sodium alginate solution was prepared and poured into a specific mold. Then, a 0.3 mol / mL calcium chloride solution was prepared. The silk fibroin solution obtained in step 1) was mixed with the calcium chloride solution and then introduced into the sodium alginate solution at a rate of 20 μL per drop and 30 s intervals. The mass fraction of silk fibroin in the mixed solution was controlled to be 10% and [Ca 2 + ] / [COO - ]=0.18, and then place it on a specific metal substrate, immerse the bottom of the assembled device in liquid nitrogen for directional freezing for 3 minutes, and finally place the pre-frozen composite material in a vacuum freeze dryer for freeze drying. After 48 hours, take out the dry columnar scaffold, treat the scaffold with calcium chloride for 12 hours, and then soak it in deionized water. After freeze drying, the directional porous silk fibroin composite calcium alginate scaffold material SA / SF-DF is finally obtained. Example 2

[0022] Sodium alginate, silk fibroin, calcium chloride, lithium bromide and acetic acid are used as raw materials to prepare a high-strength oriented porous silk fibroin composite calcium alginate scaffold material. The preparation steps are as follows: (1) First, the natural silk was degummed and dissolved in a lithium bromide solution. After dialysis, a silk fibroin solution of a certain concentration was obtained. The concentration was tested by the loss on drying method, and then a 7% mass fraction silk fibroin solution was obtained through concentration or dilution. (2) Then, 2.5 ml of a 4% sodium alginate solution was prepared and poured into a specific mold. Then, a 0.5 mol / mL calcium chloride solution was prepared. The silk fibroin solution obtained in step 1) was mixed with the calcium chloride solution and then introduced into the sodium alginate solution. The mass fraction of silk fibroin in the mixed solution was controlled to be 20% and [Ca 2 + ] / [COO - ]=0.18, and then placed it on a specific metal substrate, and the bottom of the assembled device was immersed in liquid nitrogen for directional freezing for 3 minutes. Finally, the pre-frozen composite material was placed in a vacuum freeze dryer for freeze drying. After 48 hours, the dried columnar scaffold was taken out, the scaffold was treated with calcium chloride for 12 hours, and then soaked in deionized water. After freeze drying, a high-strength directional porous silk fibroin composite calcium alginate scaffold material SA / SF was finally obtained. 20 -DF. Comparative Example 1

[0023] The difference between this comparative example and the embodiment is that the silk fibroin composite calcium alginate scaffold material (SA / SF-GC) is prepared by the traditional gradient cooling method, that is, the sample mold is placed in a -20°C refrigerator and frozen for 6 hours and then moved into a -80°C refrigerator and frozen for 24 hours. Finally, the pre-frozen composite material is placed in a vacuum freeze dryer and freeze-dried for 48 hours to finally obtain a silk fibroin composite calcium alginate scaffold material.

[0024] In order to obtain the morphology, pore size and distribution of silk fibroin in the scaffold, the scaffold was observed using a digital camera and an optical microscope.

[0025] The porosity of the scaffold was calculated by the liquid replacement method. The pycnometer was filled with anhydrous ethanol and weighed, which was recorded as M0; then the SA / SF-DF and SA / SF-GC scaffolds with a mass of M1 were immersed in anhydrous ethanol solution, vacuum degassed, and anhydrous ethanol was filled in the pores of the three groups of scaffolds. The mass of the pycnometer was weighed again, which was recorded as M2; finally, the scaffold was taken out of the pycnometer and the mass of the pycnometer was weighed again, which was recorded as M3; each group of scaffolds was measured 3 times and the average value was taken. The porosity formula is as follows:

[0026] Where: M0 is the total mass of the pycnometer after it is filled with ethanol; M1 is the original mass of the bracket; M2 is the total mass of the pycnometer after the bracket is completely immersed in anhydrous ethanol; M3 is the total mass of the remaining anhydrous ethanol and the pycnometer after the bracket is taken out of anhydrous ethanol.

[0027] High-porosity materials can provide sufficient space and absorb sufficient nutrients, which is beneficial to the exchange of substances in the body and the growth of bone tissue. Figure 4 We can see that the SA / SF-DF scaffold has a higher porosity than the SA / SF-GCCS scaffold.

[0028] The water absorption test of the scaffolds was carried out in PBS buffer solution. The SA / SF-DF and SA / SF-GC scaffolds with a dry mass of M0 were placed in PBS (PH = 7.4) solution and soaked for a certain time interval. Then, the residual water on the surface of the scaffold was gently wiped with filter paper, and then the mass after water absorption and swelling was weighed on a precision electronic balance, recorded as M0. W (n=5), and calculate its water absorption rate according to the following formula:

[0029] Where: M W is the wet weight of the scaffold material after absorbing water; M0 is the mass of the scaffold material in dry state.

[0030] Water absorption rate is an important indicator used to examine the moisture retention performance of the scaffold. Figure 5 It is the water absorption rate of the scaffold after being continuously immersed in PBS solution for 24 hours and saturated with water. The main detection time nodes are 0.5h, 3h, 6h, 9h, 12h and 24h. It can be seen from the figure that with the passage of time, the water absorption rate of the scaffold shows an upward trend. At 12h, the water absorption rate tends to be stable and reaches water absorption saturation. The water absorption rate is maintained at about 90%, showing good moisturizing performance.

[0031] Good mechanical properties are very important for scaffold materials used to treat bone defects. This study used the Bose ELF3200 biomaterial mechanical material testing system to test the compressive strength of the scaffold. The compression speed of the compression probe was controlled to 0.5 mm / min, and each group consisted of 5 samples. Figure 6 As shown in the figure, the stress of SA / SF-DF and SA / SF-GC scaffolds gradually increases with strain. Compared with the SA / SF-GC scaffold, the SA / SF-DF scaffold has a greater stress when deformed to 50%, which can meet the compressive strength required for the scaffold to repair bone defects.

[0032] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a high-strength directional porous bone repair scaffold material, characterized in that: The specific steps include: (1) Providing silk fibroin solution, calcium chloride solution and sodium alginate solution; (2) pouring the sodium alginate solution into the mold, mixing the silk fibroin solution and the calcium chloride solution evenly, and then dropping them into the sodium alginate solution to obtain a mixed solution, which is then placed on a metal substrate, and the bottom of the assembled device is immersed in liquid nitrogen for directional freezing; (3) The mold and the sample after directional freezing are quickly placed in a vacuum freeze dryer for freeze drying to obtain an directional porous silk fibroin composite calcium alginate scaffold material.

2. The method for preparing the high-strength directional porous bone repair scaffold material according to claim 1, characterized in that: In the silk fibroin solution in step (1), the mass fraction of silk fibroin is 4-7%.

3. The method for preparing the high-strength directional porous bone repair scaffold material according to claim 1, characterized in that: The mass fraction of the sodium alginate solution in step (1) is 2-5%.

4. The method for preparing the high-strength directional porous bone repair scaffold material according to claim 1, characterized in that: The concentration of calcium chloride in step (1) is 0.3 mol / mL to 0.5 mol / mL.

5. The method for preparing the high-strength directional porous bone repair scaffold material according to claim 1, characterized in that: The mass fraction of silk fibroin in the mixed solution in step (2) is 10% to 30%.

6. The method for preparing the high-strength directional porous bone repair scaffold material according to claim 1, characterized in that: The ratio of sodium alginate to calcium chloride in step (2) is m=[Ca 2 + ] / [COO - ]=0.15~0.

2.

7. The method for preparing the high-strength directional porous bone repair scaffold material according to claim 1, characterized in that: The time of liquid nitrogen directional freezing in step (2) is more than 3 minutes.

8. The method for preparing the high-strength directional porous bone repair scaffold material according to claim 7, characterized in that: The time of liquid nitrogen directional freezing in step (2) is 3 to 4 minutes.

9. The method for preparing the high-strength directional porous bone repair scaffold material according to claim 1, characterized in that: The freeze-drying time of step (3) is 46 to 48 hours.

10. The method for preparing the high-strength directional porous bone repair scaffold material according to claim 1, characterized in that: The preparation method further comprises step (4), wherein the scaffold is treated with calcium chloride, then soaked in deionized water, and freeze-dried to obtain a directional porous silk fibroin composite calcium alginate scaffold material.