Fluorine removal agent as well as preparation method and application thereof
By using natural zeolite-loaded calcium-aluminum-iron layered three-metallic oxide as a fluoride removal agent in sewage treatment, the problems of inconvenient storage and transportation and limited applicability of existing fluoride removal agents are solved, and efficient fluoride ion adsorption removal is achieved. And reused multiple times, reducing costs.
Patent Information
- Application Number
- CN202410548867.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-06
- Publication Date
- 2024-10-01
AI Technical Summary
Existing fluoride removers are inconvenient to store and transport, some contain toxic substances, and have limited applicability. Different types of fluoride removers have different applicability to different water qualities, concentrations, and temperatures, resulting in more development problems in sewage treatment. Type of defluoridator required.
The layered three-metallic oxide formed by loading calcium, aluminum and iron on natural zeolite is used as a defluoridation agent. It is prepared by mixing calcium salt, aluminum salt and iron salt with natural zeolite under alkaline conditions and calcining it at high temperature. It solves the problem of layered The trimetallic oxide particles are prone to agglomeration, have low specific surface area, and have low surface positive charge density, which improves the adsorption and removal rate of fluoride ions and enables multiple reuse through elution with alkaline solutions.
It improves the adsorption and removal rate of fluoride ions, simplifies the use method, reduces the cost of defluoridating water, and enhances the adsorption capacity and reusability of layered three-metal oxides by introducing natural zeolite as a carrier.
Smart Images

Figure BDA0004823626370000051 
Figure BDA0004823626370000061
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sewage treatment, and in particular to a defluorination agent and a preparation method and application thereof. Background Art
[0002] Defluoridation agent is an important chemical agent used to remove fluoride ions from water, which is of great significance to water quality and human health. Common defluoridation agents on the market include aluminum hydroxide defluoridation agents, zirconium titanium defluoridation agents, ion exchange resin defluoridation agents, and electrolytic defluoridation agents. Aluminum hydroxide and zirconium titanium defluoridation agents are easy to react with other chemical agents and water quality, and are inconvenient to store and transport. Some defluoridation agents contain toxic substances, which may affect the water ecological environment and need to be used with caution. Different types of defluoridation agents have different applicability to different water quality, water concentration and water temperature, and it is necessary to select a suitable defluoridation agent according to the actual situation. Therefore, the development of more types of defluoridation agents is of great significance in the field of sewage treatment.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a natural zeolite-loaded calcium aluminum iron layered trimetallic oxide defluorinating agent and a preparation method and application thereof.
[0005] Specifically, the technical solution of the present invention is as follows:
[0006] In the first aspect, the present invention provides a defluorinating agent, which is a layered trimetallic oxide formed by loading calcium, aluminum and iron with natural zeolite as a carrier; the layered trimetallic oxide is obtained by adding natural zeolite to a mixed solution of calcium salt, aluminum salt and iron salt, and calcining the precipitate formed under alkaline conditions at 300-600°C; wherein the mass ratio of calcium salt, aluminum salt and iron salt is 1:1-5:1-5.
[0007] In the present invention, the metals constituting the layered trimetallic oxide are calcium, aluminum and iron. The calcium element can increase the affinity for fluoride ions; the interlaminar spacing and specific surface area of the aluminum-iron composition are larger. The introduction of natural zeolite as a carrier solves the defects of the layered trimetallic oxide particles being easy to agglomerate, having a low specific surface area, and having limited adsorption sites due to low surface positive charge density.
[0008] In the present invention, calcium salt, aluminum salt and iron salt are compounded in a specific mass ratio, and the obtained defluoridation agent has a high adsorption removal rate for fluoride ions. The method of using the defluoridation agent is simple, and the defluoridation agent is wrapped with a geotextile and hung in a water pool. After the adsorption is completed, an alkaline solution can be used for elution, and the defluoridation agent can be repeatedly used, thereby greatly reducing the cost of defluoridation of water bodies.
[0009] Preferably, the alkaline condition is a pH value of 10-12.
[0010] Preferably, the natural zeolite is 10-25 mesh clinoptilolite. The crystallization mode of clinoptilolite is different from that of common zeolite, and its crystal structure presents mutually staggered cutting, which makes the pore system of clinoptilolite more complex and rich.
[0011] Preferably, based on 5 parts by weight of the total weight of the calcium salt, the aluminum salt and the iron salt, the weight of the natural zeolite is 1-3 parts.
[0012] Preferably, the precipitate is vacuum dried at 50-60°C before calcination.
[0013] Preferably, the vacuum drying treatment is performed for 12-24 hours.
[0014] Preferably, the calcination time is 2-3 hours.
[0015] In a second aspect, the present invention provides a method for preparing the defluorination agent, comprising the following steps:
[0016] S1, placing natural zeolite in a mixed solution of calcium salt, aluminum salt and iron salt to obtain a mixed liquid;
[0017] S2, adjusting the pH value of the mixed liquid to alkaline, stirring, and standing for aging to allow precipitation to adhere to the surface of the natural zeolite;
[0018] S3, washing the precipitate with deionized water, vacuum drying, and calcining to obtain the defluorinating agent.
[0019] Preferably, the stirring speed in step S2 is 100-200 r / min (preferably 100-150 r / min), and the stirring time is 30-60 min.
[0020] Preferably, the static aging time in step S2 is 6-12 hours.
[0021] In a third aspect, the present invention also provides the use of the defluorinating agent, or the defluorinating agent prepared by the preparation method, in defluorinating water.
[0022] Beneficial effects:
[0023] The present invention provides a defluorinating agent of a natural zeolite loaded calcium aluminum iron layered trimetallic oxide, and a preparation method and application thereof. The defluorinating agent is a layered trimetallic oxide formed by loading calcium aluminum iron with natural zeolite as a carrier; the layered trimetallic oxide is obtained by adding natural zeolite to a mixed solution of calcium salt, aluminum salt and iron salt, and calcining the precipitate formed under alkaline conditions at 300-600°C; wherein the mass ratio of calcium salt, aluminum salt and iron salt is 1:1-5:1-5. The defluorinating agent provided by the present invention has the advantages of simple preparation method and high defluorination rate. After defluorinating a water body with the defluorinating agent provided by the present invention, its own defluorination capacity can be restored by eluting with an alkaline solution, and then reused at a lower cost. DETAILED DESCRIPTION
[0024] The present invention provides a natural zeolite-loaded calcium aluminum iron layered trimetallic oxide defluorinating agent and its preparation method and application. The preparation method of the defluorinating agent mainly comprises: 2+ 、Al 3+ , Fe 3+ The salt is dissolved in deionized water, natural zeolite is added, and mixed alkali solution is added to adjust the pH value, stirred, allowed to stand for aging, filtered, and calcined at high temperature to obtain a layered trimetallic oxide composite material with natural zeolite as a carrier. The defluoridation agent is mainly used in the following ways: the obtained layered trimetallic oxide composite material with natural zeolite as a carrier is wrapped with a geotextile and hung in a pool. The metals constituting the layered trimetallic oxide are calcium, aluminum, and iron. The calcium element can increase the affinity for fluoride ions; the interlamellar spacing and specific surface area of the aluminum-iron composition are larger. The introduction of natural zeolite as a carrier solves the defects of the layered trimetallic oxide particles being easy to agglomerate, having low specific surface area, and having limited adsorption sites due to low surface positive charge density. The adsorption removal rate of fluoride ions is high, the method is simple, and after the adsorption is completed, an alkaline solution can be used for elution, which can be reused and has low cost.
[0025] In a more specific embodiment provided by the present invention, the preparation method of the defluorination agent is as follows:
[0026] 1) Ca 2+ 、Al 3+ , Fe 3+ The salt is dissolved in deionized water to obtain a mixed solution;
[0027] 2) adding natural zeolite to the mixed solution, mixing and stirring to obtain a mixed liquid;
[0028] 3) adding a mixed alkali solution dropwise to the mixed liquid, adjusting the pH to 10-12, stirring vigorously and then standing to age to obtain a precipitate;
[0029] 4) The above precipitate is filtered, washed, vacuum dried, and calcined at 300-600° C. to obtain a natural zeolite composite material loaded with calcium aluminum iron layered trimetallic oxides.
[0030] Among them, the Ca 2+ 、Al 3+ , Fe 3+ The salt may be one or more of nitrate, sulfate, and chloride, and the mass ratio of calcium aluminum iron salt is 1:1-5:1-5.
[0031] Preferably, the mass ratio of natural zeolite to the total amount of metal salts is 1-3:5.
[0032] Preferably, the stirring time in step 3) is 30 to 60 minutes, and the standing aging time is 6 to 12 hours.
[0033] Preferably, in step 4), deionized water is used for filtering and washing 3-4 times.
[0034] Preferably, in step 4), vacuum drying is performed at 50-60° C. for 12-24 hours.
[0035] Preferably, in step 4), the calcination is carried out at 300-500° C. for 2-3 hours.
[0036] The technical solutions provided by the present invention are described in detail below in conjunction with the examples, but they should not be understood as limiting the scope of protection of the present invention. Unless otherwise specified, the experimental methods used in the examples are conventional methods; the materials and reagents used can be obtained from commercial sources.
[0037] Example 1
[0038] (I) This embodiment provides a novel composite material defluorination agent, the raw materials for its preparation include:
[0039] 10 grams of aluminum sulfate, 10 grams of aluminum chloride, 20 grams of iron sulfate, 10 grams of calcium chloride, and 10 grams of natural zeolite.
[0040] (II) This embodiment provides a method for preparing the defluorination agent, which is as follows:
[0041] (1) Dissolve 10 g of aluminum sulfate, 10 g of aluminum chloride, 20 g of ferric sulfate, and 10 g of calcium chloride in 100 g of deionized water to obtain a mixed solution.
[0042] (2) Add 10 g of 10-25 mesh clinoptilolite to the above mixed solution and stir to obtain a mixed liquid.
[0043] (3) Add a mixed alkaline solution of sodium carbonate and sodium hydroxide to the mixed liquid, adjust the pH value to 10.0, stir vigorously for 30 minutes, and then let it stand for 6 hours to obtain a precipitate.
[0044] (4) The precipitate was filtered and washed three times with deionized water, then vacuum dried at 50° C. for 12 hours, and then calcined at 500° C. for 2 hours to obtain a new composite material defluorination agent.
[0045] (III) In this example, the fluoride ion removal rate of the obtained new composite material defluoridation agent is measured, and the specific operation and measurement results are as follows:
[0046] A fluoride solution with an initial concentration of 10 mg / L was prepared using sodium fluoride stock solution and deionized water as raw materials. Two 100 mL portions of 10 mg / L fluoride solution were taken, and 1 gram of the new composite material defluoridant and 1 gram of natural zeolite were added respectively. After magnetic stirring for 0.5 hour and 1 hour, the supernatant was taken to determine the fluoride concentration.
[0047] The results showed that when the initial fluoride ion concentration was 2 mg / L, the fluoride ion removal rate was 91% after 0.5 hours of adding the new composite material defluoridation agent, and the fluoride ion removal rate was 96% after 1 hour. The fluoride ion removal rate was 31% after 0.5 hours of adding the natural zeolite fluoride ion, and the fluoride ion removal rate was 35% after 1 hour.
[0048] (IV) This example tests the effect of repeated use of the obtained new composite material:
[0049] Take the new composite material defluoridation agent used in the above (III) and elute it with 0.8 mol / L sodium hydroxide solution until no fluoride ions are detected in the eluate, then dry and roast it for the next defluoridation experiment. After repeated use - elution for 5 times, the defluoridation rate can still reach 90%.
[0050] Embodiment 2-6
[0051] Compared with Example 1, the only difference between Examples 2-6 is that the raw materials are different.
[0052] The raw materials for preparing each example are shown in Table 1.
[0053] Table 1
[0054]
[0055]
[0056] The performance of the defluorination agent products obtained in Examples 2-6 was measured, and the results are shown in Table 2.
[0057] Table 2
[0058] Example 2 Example 3 Example 4 Example 5 Example 6 0.5 hour defluorination rate 88.2% 89.3% 90% 87.6% 87% 1 hour defluorination rate 93.8% 94% 95% 93% 92.5%
[0059] Embodiment 7-8
[0060] Compared with Example 1, the only difference between Example 7-8 is that the clinoptilolite in the preparation raw material is replaced by mordenite and chabazite.
[0061] The performance of the defluorination agent products obtained in Examples 7-8 was measured, and the results are shown in Table 3.
[0062] Table 3
[0063] Example 7 (Mordenite) Example 8 (Chabazite) 0.5 hour defluorination rate 70% 65% Fluoride removal rate in 1 hour 75.8% 72%
[0064] After being regenerated and reused for 5 times, the performance was measured and the fluorine removal rates of the products of Example 7 and Example 8 were 63% and 58% respectively.
[0065] Comparative Example 1
[0066] The only difference between Comparative Example 1 and Example 1 is that in step (4) of the preparation method, the novel composite material defluorinating agent is obtained by calcining at 800° C. for 2 hours.
[0067] Compared with Example 1, the defluorination efficiency of the new composite material defluoridation agent obtained in Comparative Example 1 is greatly reduced, and the fluoride ion removal rate after 0.5 hours is 53%, and the fluoride ion removal rate after 1 hour is 58%. After being regenerated and reused for 5 times, the defluorination rate reaches about 40%.
[0068] The above-described embodiments only express several implementation methods of the present invention, which are convenient for understanding the technical solution of the present invention in detail, but cannot be understood as limiting the scope of protection of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the scope of protection of the present invention.
Claims
1. A defluorination agent, characterized in that: The defluoridation agent is a layered trimetallic oxide formed by using natural zeolite as a carrier and loading calcium, aluminum and iron; the layered trimetallic oxide is obtained by adding natural zeolite to a mixed solution of calcium salt, aluminum salt and iron salt, and calcining the precipitate formed under alkaline conditions at 300-600°C; wherein the mass ratio of calcium salt, aluminum salt and iron salt is 1:1-5:1-5.
2. The defluorination agent according to claim 1, characterized in that: The alkaline condition is a pH value of 10-12.
3. The defluorination agent according to claim 1 or 2, characterized in that: The natural zeolite is 10-25 mesh clinoptilolite.
4. The defluorination agent according to any one of claims 1 to 3, characterized in that: Based on the total mass parts of calcium salt, aluminum salt and iron salt being 5 parts, the mass parts of the natural zeolite are 1-3 parts.
5. The defluorination agent according to any one of claims 1 to 4, characterized in that: The precipitate is subjected to vacuum drying treatment at 50-60° C. before calcination; preferably, the vacuum drying treatment time is 12-24 hours.
6. The defluorination agent according to any one of claims 1 to 5, characterized in that: The calcination time is 2-3h.
7. The method for preparing the defluorination agent according to any one of claims 1 to 6, characterized in that: The steps include: S1, placing natural zeolite in a mixed solution of calcium salt, aluminum salt and iron salt to obtain a mixed liquid; S2, adjusting the pH value of the mixed liquid to alkaline, stirring, and standing for aging to allow precipitation to adhere to the surface of the natural zeolite; S3, washing the precipitate with deionized water, vacuum drying, and calcining to obtain the defluorinating agent.
8. The preparation method according to claim 7, characterized in that: The stirring speed in step S2 is 100-200 r / min, and the stirring time is 30-60 min.
9. The preparation method according to claim 7 or 8, characterized in that: The standing and aging time in step S2 is 6-12 hours.
10. Use of the defluorinating agent according to any one of claims 1 to 6, or the defluorinating agent prepared by the preparation method according to any one of claims 7 to 9 in defluorinating water.
Citation Information
Patent Citations
Defluoridation adsorbent material and preparation method thereof
CN102600797A
Preparation method and application of transition metal doped magnesium-aluminum layered double-metal hydroxide material
CN115845792A
System and method for simultaneous removal of arsenic and fluoride from aqueous solutions
CN1450978A
Cited By
Preparation method and application of fluorine removal agent
CN121244185A