Claus tail gas incineration catalyst as well as preparation method and application thereof
By using high-purity silica carrier and scandium oxide and chromium oxide in the Claus tail gas incineration catalyst, the generation of sulfur trioxide is avoided, the corrosion and waste water problems of the tail gas treatment device in high-temperature incineration are solved, and efficient sulfurization is achieved Hydrogen and organic sulfur oxidation effects.
Patent Information
- Application Number
- CN202310324501.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Under high-temperature incineration conditions, catalytic incineration technology failed to effectively suppress the generation of sulfur trioxide, resulting in severe corrosion of the tail gas treatment device and a large amount of salty wastewater, which could not meet the requirements of subsequent treatment processes.
Using high-purity silica with ultra-low iron impurity content as the carrier, the Claus tail gas incineration catalyst loaded with scandium oxide and chromium oxide can avoid the deep oxidation of sulfur dioxide into sulfur trioxide caused by iron oxide, and achieve sulfur dioxide at 300-350°C. Efficiently catalyzes the oxidation of hydrogen sulfide and organic sulfur into sulfur dioxide.
Effectively inhibits the generation of sulfur trioxide. The concentration of sulfur trioxide in the gas after incineration is less than 1ppm, which improves the oxidation effect of organic sulfur. The concentration of organic sulfur in the gas after incineration is less than 5ppm, which solves the problems of device corrosion and waste water, and meets the follow-up requirements. Processing requirements.
Smart Images

Figure BDA0004153798010000091 
Figure HDA0004153798020000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of natural gas, refinery gas and coal chemical gas processing, and particularly relates to a Claus tail gas incineration catalyst capable of effectively inhibiting the generation of sulfur trioxide, and a preparation method and application thereof. Background Art
[0002] Natural gas purification plants, oil refineries and coal chemical plants generally use Claus sulfur recovery process technology to recover sulfur from hydrogen sulfide acid gas. This technology can generally recover 90-97% of hydrogen sulfide in acid gas and convert it into sulfur. The tail gas after sulfur recovery generally contains 0.5-2% hydrogen sulfide, 0.01-0.5% organic sulfur, 0.02-0.1% elemental sulfur and 0.2-1% sulfur dioxide by volume. For those without subsequent tail gas treatment processes, the tail gas is generally incinerated at 500-600℃ by adding an appropriate amount of air, and the non-sulfur dioxide sulfides are oxidized to sulfur dioxide before being discharged. This is conventional incineration. For exhaust gas treatment processes that use oxidation absorption (such as the Consol process), the exhaust gas is also thermally incinerated by adding an appropriate amount of air. The non-sulfur dioxide sulfides are oxidized into sulfur dioxide before the next step of treatment. Because there are strict requirements on the concentration of residual hydrogen sulfide and organic sulfur in the exhaust gas after incineration, the incineration temperature is 750-850°C, which is high-temperature incineration.
[0003] Thermal incineration usually consumes a large amount of fuel gas. In order to achieve energy conservation, Claus tail gas catalytic incineration technology has been developed. By loading the catalyst in the incinerator, a thermal incineration effect of 500-600°C can be achieved at 300-350°C. Catalytic incineration catalysts usually use silica gel or silica-alumina as carriers, and chromium oxide and iron oxide as active components. For conventional incineration, it is usually required that the volume concentration of hydrogen sulfide in the gas after incineration is <10ppm, the volume concentration of organic sulfur is <20ppm, and there is no requirement for the concentration of sulfur trioxide. Both catalytic incineration and thermal incineration can achieve this indicator, so catalytic incineration technology has been widely used in Claus tail gas conventional incineration devices. As for high-temperature incineration, if catalytic incineration is used instead of thermal incineration, then under the premise of ensuring that the volume concentration of hydrogen sulfide in the gas after incineration is <10ppm and the volume concentration of organic sulfur is <20ppm, there will be a volume concentration of 100-200ppm of sulfur trioxide in the gas after incineration, which cannot meet the requirement of sulfur trioxide volume concentration <10ppm proposed by the subsequent tail gas treatment process, and will cause serious corrosion of the tail gas treatment device and the generation of a large amount of salt-containing wastewater. Therefore, catalytic incineration technology has not been industrially applied in high-temperature incineration devices. The core issue in promoting the industrial application of catalytic incineration technology in oxidation absorption tail gas treatment process devices is to develop a catalytic incineration catalyst that can effectively inhibit the formation of sulfur trioxide. Summary of the invention
[0004] The purpose of the present invention is to provide a Claus tail gas incineration catalyst that can effectively inhibit the generation of sulfur trioxide (devices with a detection limit of 1 ppm cannot detect the presence of sulfur trioxide), as well as a preparation method and application thereof. The catalyst is suitable for catalytic incineration of tail gas from a sulfur recovery device, and can oxidize hydrogen sulfide, elemental sulfur and organic sulfur in the gas into sulfur dioxide under low temperature conditions of 300-350°C, while avoiding the problem that ordinary incineration catalysts deeply oxidize part of the sulfur dioxide into sulfur trioxide, resulting in a small amount of sulfur trioxide in the gas after incineration, and can effectively solve the problem of severe device corrosion and large amount of salt-containing wastewater caused by sulfur trioxide in the next step of tail gas treatment after incineration.
[0005] In order to achieve the above objectives, the present invention provides the following three technical solutions.
[0006] In a first aspect, the present invention provides a Claus tail gas incineration catalyst, wherein the catalyst uses high-purity silicon dioxide with ultra-low iron impurity content as a carrier to load active components of scandium oxide and chromium oxide;
[0007] Wherein, in the high-purity silicon dioxide with ultra-low iron impurity content, based on the total mass of the high-purity silicon dioxide with ultra-low iron impurity content as 100%, the silicon dioxide content is greater than 99.9%, and the iron oxide content is less than 0.01%;
[0008] The loaded active components do not contain iron oxide.
[0009] The inventor has conducted a lot of research on the existing Claus tail gas incineration catalyst and believes that the substance that catalyzes the chemical reaction of hydrogen sulfide, organic sulfur and elemental sulfur to sulfur dioxide at 300-350°C in the existing Claus tail gas incineration catalyst is mainly chromium oxide, and iron oxide mainly plays a role in improving the dispersibility of chromium oxide on conventional silica gel or silica-alumina carriers; chromium oxide will not catalyze the deep oxidation of sulfur dioxide to sulfur trioxide, but iron oxide can deeply oxidize 2-10% of sulfur dioxide to sulfur trioxide. Based on this, the inventor proposed a Claus tail gas incineration catalyst that uses high-purity and ultra-low iron impurity silica as a carrier to load active components scandium oxide and chromium oxide. In the catalyst, high-purity and ultra-low iron impurity silica is used as a carrier to replace conventional silica gel or silica-alumina materials, eliminating the influence of conventional silica gel or silica-alumina materials on the catalyst due to the high iron oxide impurity content, and using scandium oxide to replace iron oxide, so that chromium oxide can be uniformly dispersed on the high-purity and ultra-low iron impurity silica carrier without catalyzing the deep oxidation of sulfur dioxide to sulfur trioxide. The combination of high-purity silicon dioxide, scandium oxide and chromium oxide with ultra-low iron impurity content achieves efficient catalysis during the Claus tail gas incineration process while avoiding the generation of sulfur trioxide (devices with a detection limit of 1 ppm cannot detect the presence of sulfur trioxide).
[0010] According to a preferred embodiment of the first aspect, based on 100% of the total mass of the catalyst, the amount of scandium oxide is 0.5-0.8%, and the weight content of chromium oxide is 3.0-4.5%.
[0011] According to a preferred embodiment of the first aspect, the high-purity silicon dioxide with ultra-low iron impurity content as a carrier is obtained by tableting high-purity silicon dioxide powder with ultra-low iron impurity content;
[0012] Furthermore, the specific surface area of the high-purity and ultra-low iron impurity silicon dioxide powder is 100-150m 2 / g, average particle size of 0.2-0.5 microns, bulk density of 0.1-0.15g / ml;
[0013] Furthermore, the tableting pressure is 10-30 MPa and the pressing time is 1-2 s.
[0014] Furthermore, the high-purity silicon dioxide powder with ultra-low iron impurity content is a hydrophilic high-purity silicon dioxide powder with ultra-low iron impurity content produced by a gas phase method.
[0015] According to a preferred embodiment of the first aspect, the high-purity silicon dioxide with ultra-low iron impurity content as the carrier is in the form of flakes with a diameter of 8-10 mm and a height of 2-3 mm.
[0016] In a second aspect, the present invention provides a method for preparing the above-mentioned Claus tail gas incineration catalyst, wherein the method comprises:
[0017] High-purity silicon dioxide with ultra-low iron impurity content as a carrier is placed in a mixed solution of scandium salt and chromium salt for impregnation, and then dried and calcined to obtain the catalyst.
[0018] According to a preferred embodiment of the second aspect, the method further comprises a carrier preparation step of preparing a carrier having a specific surface area of 100-150 m 2 / g, an average particle size of 0.2-0.5 microns, a bulk density of 0.1-0.15g / ml, and a high-purity silicon dioxide powder with an ultra-low iron impurity content are mixed with water and then pressed into tablets, and then the tableted product is dried to obtain a sheet of high-purity silicon dioxide with an ultra-low iron impurity content of 8-10mm in diameter and 2-3mm in height as a carrier; wherein the tableting pressure is 10-30MPa and the punching time is 1-2s;
[0019] Further, the mass ratio of high-purity and ultra-low iron impurity content silicon dioxide powder to water is 300-400:100-130;
[0020] Furthermore, the drying temperature is 120-130° C., and the drying time is 2-3 hours.
[0021] According to a preferred embodiment of the second aspect, the scandium salt comprises scandium nitrate and / or scandium sulfate;
[0022] Furthermore, the scandium salt is scandium nitrate.
[0023] According to a preferred embodiment of the second aspect, the chromium salt comprises one or a combination of two or more of chromium nitrate, chromium chloride and chromium sulfate;
[0024] Furthermore, the chromium salt is chromium nitrate.
[0025] According to a preferred embodiment of the second aspect, the drying temperature after impregnation is 100-110°C.
[0026] According to a preferred embodiment of the second aspect, the calcination temperature is 350-400° C. and the calcination time is 2-3 h.
[0027] According to a preferred embodiment of the second aspect, the method comprises:
[0028] Carrier preparation: 300-400 parts by weight of a carrier having a specific surface area of 100-150 m 2 / g, an average particle size of 0.2-0.5 microns, a bulk density of 0.1-0.15g / ml, and a high-purity silicon dioxide powder with ultra-low iron impurity content are mixed with 100-130 parts by weight of water, and then tableted at a molding pressure of 10-30MPa and a punching time of 1-2s to form a sheet with a diameter of 8-10mm and a height of 2-3mm, and then the tableted product is dried at 120-130°C to obtain a carrier;
[0029] Preparation of impregnation solution: Scandium salt (anhydrous scandium nitrate and / or scandium sulfate, purity>98%) and chromium salt (anhydrous chromium nitrate and / or chromium chloride and / or chromium sulfate, purity>99%) are mixed with water to obtain a mixed solution of scandium salt and chromium salt with a scandium salt volume concentration of 83-130 g / L and a chromium salt volume concentration of 470-705 g / L;
[0030] Impregnation: placing the carrier in a mixed solution of scandium salt and chromium salt for impregnation; wherein the amount ratio of the carrier to the mixed solution of scandium salt and chromium salt is 40-50g:50-80ml;
[0031] Drying: Dry the impregnated product at 120-130°C;
[0032] Calcination: The dried product is calcined at 350-400° C. for 2-3 h to obtain the catalyst.
[0033] In a third aspect, the present invention provides the use of the above-mentioned Claus tail gas incineration catalyst as a catalyst in a Claus tail gas incineration process.
[0034] According to a preferred embodiment of the third aspect, in the above application, the Claus tail gas is introduced into an incineration device filled with the above catalyst for incineration.
[0035] According to a preferred embodiment of the third aspect, in the above application, the particle size of the catalyst is 1.5-2 mm.
[0036] According to a preferred embodiment of the third aspect, in the above application, the gas space velocity is 1000-1500h -1 .
[0037] According to a preferred embodiment of the third aspect, in the above application, the incineration temperature is 300-350°C.
[0038] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0039] 1. The existing Claus tail gas catalytic incineration catalyst will catalyze the side reaction of deep oxidation of sulfur dioxide to sulfur trioxide. The volume concentration of sulfur trioxide in the gas after incineration is about 100-200ppm. The catalyst of the present invention can effectively inhibit the formation of sulfur trioxide, and the volume concentration of sulfur trioxide in the gas after incineration is <1ppm.
[0040] 2. The existing Claus tail gas catalytic incineration catalyst has a poor oxidation effect on organic sulfur, and can only ensure that the organic sulfur concentration in the gas after incineration is less than 20ppm. The catalyst of the present invention enhances the organic sulfur oxidation effect, and the organic sulfur concentration in the gas after incineration is less than 5ppm.
[0041] 3. The use of the catalyst provided by the present invention for Claus tail gas catalytic incineration not only satisfies the requirement of sulfur trioxide volume concentration <10ppm proposed by the subsequent tail gas treatment process, but also suppresses the generation of sulfur trioxide, solves the problems of severe corrosion of the device and the generation of a large amount of salt-containing wastewater, and the organic sulfur (COS) concentration is far lower than <20ppm, which reduces the sulfide concentration in the exhaust gas of the device, and has significant environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a flow chart of the catalyst preparation in Example 1. DETAILED DESCRIPTION
[0043] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the content specifically described below is illustrative and non-restrictive, and protection scope of the present invention should not be limited by this. Efforts have been made to ensure the accuracy of numbers (such as amounts, temperatures, etc.), but some errors and deviations should be taken into account.
[0044] Example 1
[0045] This embodiment provides a Claus tail gas incineration catalyst, which is prepared by the following method (process as shown in Figure 1 shown):
[0046] Weigh 383g of high-purity and ultra-low iron impurity silica powder (model OX100 produced by Degussa, Germany, hydrophilic silica produced by gas phase method, with a silica weight percentage of 99.96%, an iron oxide weight percentage of 0.0042%, and a specific surface area of 105m 2 / g, average particle size 0.33 μm, bulk density 0.12 g / ml) were placed in a 5 L beaker, and 125 g of distilled water was added to the 5 L beaker and stirred with a glass rod for 2 min;
[0047] The mixed product was transferred to a rotary tablet press for tableting, and then dried at 120°C for 3 hours to obtain a carrier; the molding was performed using an 8 mm mold, a molding pressure of 16 MPa, and a punching time of 1.2 seconds. The diameter of the formed sheet was 8.1 mm and the height was 2.4 mm;
[0048] Weigh 97 g of anhydrous scandium nitrate (purity 98.5%) and 559 g of anhydrous chromium nitrate (purity 99.2%) into another 5 L beaker, slowly add 500 g of distilled water, slowly stir with a glass rod until completely dissolved, continue to add distilled water until the total volume of the solution is 1 L, and obtain a mixed solution of scandium salt and chromium salt;
[0049] Weigh 42 g of the dried carrier and put it into a 1L beaker; measure 55 ml of a mixed solution of scandium salt and chromium salt and pour it into the above 1L beaker; immerse the carrier in the mixed solution of scandium salt and chromium salt for 2 hours;
[0050] After impregnation, the carrier was filtered out and left to stand for 10 h and then dried at 105 °C for 2 h;
[0051] The dried product was calcined at 380°C for 3h to obtain Claus tail gas incineration catalyst.
[0052] The weight percentage of scandium oxide in the tested catalyst product is 0.66%, and the weight percentage of chromium oxide is 4.05%.
[0053] The Claus tail gas incineration catalyst provided in this embodiment was crushed into particles with a particle size of 1.5-2 mm, and 20 g of the particles were weighed and loaded into a fixed bed reactor of a catalyst activity evaluation device; a gas containing 1.5% by volume of hydrogen sulfide, 0.28% of organic sulfur (COS), 0.05% of elemental sulfur, 0.88% of sulfur dioxide, 3.8% of oxygen, and the balance of nitrogen was introduced and incinerated at 330° C., wherein the gas flow rate was 650 ml / min, the pressure (gauge pressure) was 15 kPa (converted to a catalyst operating space velocity of 1170 h -1 The volume contents of hydrogen sulfide, COS and sulfur trioxide in the reactor outlet gas were analyzed. The results are shown in Table 1. The volume concentration of hydrogen sulfide was 8.5 ppm, COS was 2.6 ppm, and sulfur trioxide could not be detected (the lower limit of analysis detection was 1 ppm).
[0054] Example 2
[0055] This embodiment provides a Claus tail gas incineration catalyst, which is prepared by the following method:
[0056] Weigh 355g of high-purity and ultra-low iron impurity silica powder (model A120 produced by Degussa, Germany, hydrophilic silica produced by gas phase method, with a silica weight percentage of 99.94%, an iron oxide weight percentage of 0.0051%, and a specific surface area of 121m 2 / g, average particle size 0.26 micrometers, bulk density 0.12g / ml) were placed in a 5L beaker, and 130g of distilled water was added to the 5L beaker, and stirred with a glass rod for 3 minutes;
[0057] The mixed product was transferred to a rotary tablet press for tableting, and then dried at 130°C for 3 hours to obtain a carrier; a 10 mm mold was used for the molding, a molding pressure of 19 MPa, and a punching time of 1.8 seconds. The diameter of the molded sheet was 9.9 mm and the height was 2.5 mm;
[0058] Weigh 105 g of anhydrous scandium nitrate (purity 98.5%) and 641 g of anhydrous chromium nitrate (purity 99.2%) into another 5 L beaker, slowly add 500 g of distilled water, slowly stir with a glass rod until completely dissolved, continue to add distilled water until the total volume of the solution is 1 L, and obtain a mixed solution of scandium salt and chromium salt;
[0059] Weigh 48 g of the dried carrier and put it into a 1 L beaker; measure 58 ml of a mixed solution of scandium salt and chromium salt and pour it into the above 1 L beaker; immerse the carrier in the mixed solution of scandium salt and chromium salt for 3 hours;
[0060] After impregnation, the carrier was filtered out and left to stand for 10 h and then dried at 110 °C for 2 h;
[0061] The dried product was calcined at 370°C for 3h to obtain Claus tail gas incineration catalyst.
[0062] The weight percentage of scandium oxide in the tested catalyst product is 0.63%, and the weight percentage of chromium oxide is 3.82%.
[0063] The Claus tail gas incineration catalyst provided in this embodiment was crushed into particles with a particle size of 1.5-2 mm, and 20 g of the particles were weighed and loaded into a fixed bed reactor of a catalyst activity evaluation device; a gas containing 1.7% by volume of hydrogen sulfide, 0.17% of organic sulfur (COS), 0.06% of elemental sulfur, 0.62% of sulfur dioxide, 3.9% of oxygen, and the balance of nitrogen was introduced and incinerated at 340° C., wherein the gas flow rate was 720 ml / min, the pressure (gauge pressure) was 18 kPa (converted to a catalyst operating space velocity of 1340 h -1 The volume contents of hydrogen sulfide, COS and sulfur trioxide in the reactor outlet gas were analyzed. The results are shown in Table 1. The volume concentration of hydrogen sulfide was 8.7 ppm, COS was 3.4 ppm, and sulfur trioxide could not be detected (the lower limit of analysis detection was 1 ppm).
[0064] Example 3
[0065] This embodiment provides a Claus tail gas incineration catalyst, which is prepared by the following method:
[0066] Weigh 327g of high-purity and ultra-low iron impurity silica powder (model A120 produced by Degussa, Germany, hydrophilic silica produced by gas phase method, with a silica weight percentage of 99.94%, an iron oxide weight percentage of 0.0051%, and a specific surface area of 121m 2 / g, average particle size 0.26 micrometers, bulk density 0.12 g / ml) were placed in a 5L beaker, and 124 g of distilled water was added to the 5L beaker and stirred with a glass rod for 1 min;
[0067] The mixed product was transferred to a rotary tablet press for tableting, and then dried at 130°C for 3 hours to obtain a carrier; the molding was performed using an 8 mm mold, a molding pressure of 12 MPa, and a punching time of 2.0 seconds. The diameter of the formed sheet was 8.2 mm and the height was 2.2 mm;
[0068] Weigh 92 g of anhydrous scandium nitrate (purity 98.5%) and 505 g of anhydrous chromium nitrate (purity 99.2%) into another 5 L beaker, slowly add 500 g of distilled water, slowly stir with a glass rod until completely dissolved, continue to add distilled water until the total volume of the solution is 1 L, and obtain a mixed solution of scandium salt and chromium salt;
[0069] Weigh 44 g of the dried carrier and put it into a 1 L beaker; measure 52 ml of a mixed solution of scandium salt and chromium salt and pour it into the above 1 L beaker; immerse the carrier in the mixed solution of scandium salt and chromium salt for 3 hours;
[0070] After impregnation, the carrier was filtered out and left to stand for 10 h and then dried at 110 °C for 2 h;
[0071] The dried product was calcined at 395°C for 3h to obtain Claus tail gas incineration catalyst.
[0072] The weight percentage of scandium oxide in the tested catalyst product is 0.51%, and the weight percentage of chromium oxide is 3.36%.
[0073] The Claus tail gas incineration catalyst provided in this embodiment was crushed into particles with a particle size of 1.5-2 mm, and 20 g of the particles were weighed and loaded into a fixed bed reactor of a catalyst activity evaluation device; a gas containing 0.83% by volume of hydrogen sulfide, 0.09% of organic sulfur (COS), 0.08% of elemental sulfur, 0.83% of sulfur dioxide, 3.1% of oxygen, and the balance of nitrogen was introduced and incinerated at 335° C., wherein the gas flow rate was 800 ml / min, the pressure (gauge pressure) was 12 kPa (converted to a catalyst operating space velocity of 1480 h -1 The volume contents of hydrogen sulfide, COS and sulfur trioxide in the reactor outlet gas were analyzed. The results are shown in Table 1. The volume concentration of hydrogen sulfide was 6.2 ppm, COS was 2.4 ppm, and sulfur trioxide could not be detected (the lower limit of analysis detection was 1 ppm).
[0074] Example 4
[0075] This embodiment provides a Claus tail gas incineration catalyst, which is prepared by the following method:
[0076] Weigh 225 g of scandium sulfate octahydrate (purity 98.5%) and 993 g of chromium chloride hexahydrate (purity 99.1%) into a 5 L beaker, slowly add 925 g of distilled water, slowly stir with a glass rod until completely dissolved, and continue to add distilled water until the total volume of the solution is 2 L to obtain a mixed solution of scandium salt and chromium salt;
[0077] Weigh 48 g of the dried carrier in Example 3 and put it into a 1 L beaker; measure 55 ml of the mixed solution of scandium salt and chromium salt and pour it into the above 1 L beaker; immerse the carrier in the mixed solution of scandium salt and chromium salt for 3 hours;
[0078] After impregnation, the carrier was filtered out and left to stand for 10 h and then dried at 110 °C for 2 h;
[0079] The dried product was calcined at 395°C for 3 hours to obtain Claus tail gas incineration catalyst.
[0080] The weight percentage of scandium oxide in the tested catalyst product is 0.54%, and the weight percentage of chromium oxide is 3.03%.
[0081] The Claus tail gas incineration catalyst provided in this embodiment was crushed into particles with a particle size of 1.5-2 mm, and 20 g of the particles were weighed and loaded into a fixed bed reactor of a catalyst activity evaluation device; a gas containing 0.83% by volume of hydrogen sulfide, 0.09% of organic sulfur (COS), 0.08% of elemental sulfur, 0.83% of sulfur dioxide, 3.1% of oxygen, and the balance of nitrogen was introduced and incinerated at 335° C., wherein the gas flow rate was 800 ml / min, the pressure (gauge pressure) was 12 kPa (converted to a catalyst operating space velocity of 1480 h -1 ). The volume concentration of hydrogen sulfide in the reactor outlet gas was 6.7 ppm, COS was 4.3 ppm, and sulfur trioxide could not be detected (the lower limit of analytical detection was 1 ppm).
[0082] Comparative Example 1
[0083] This comparative example provides a Claus tail gas incineration catalyst
[0084] The difference between the preparation method of the catalyst provided in this comparative example and that in Example 1 is that the carrier is silica gel, the diameter of the formed sheet is 8.5 mm and the height is 3.2 mm, and anhydrous ferric nitrate is used instead of anhydrous scandium nitrate.
[0085] The prepared catalyst has a silicon dioxide content of 92.43% by weight, a chromium oxide content of 3.76% by weight, and an iron oxide content of 2.84% by weight.
[0086] The catalyst provided in this comparative example was crushed into particles with a particle size of 1.5-2 mm, and 20 g of the particles were weighed and loaded into a fixed bed reactor of a catalyst activity evaluation device. A gas containing 1.5% by volume of hydrogen sulfide, 0.28% of organic sulfur (COS), 0.05% of elemental sulfur, 0.88% of sulfur dioxide, 3.8% of oxygen, and the balance of nitrogen was introduced and incinerated at 330°C; wherein, the gas flow rate was 650 ml / min, the gas pressure (gauge pressure) was 15 kPa, and the catalyst operating space velocity was converted to 1265 h -1 The volume contents of hydrogen sulfide, COS and sulfur trioxide in the reactor outlet gas were analyzed. The results are shown in Table 1. The volume concentration of hydrogen sulfide was 8.3 ppm, COS was 17.64 ppm, and sulfur trioxide was 157 ppm.
[0087] Comparative Example 2
[0088] This comparative example provides a Claus tail gas incineration catalyst
[0089] The difference between the preparation method of the catalyst provided in this comparative example and that in Example 1 is that the carrier is silica gel, and the diameter of the formed sheet is 8.5 mm and the height is 3.2 mm. The preparation method of the mixed solution of scandium salt and chromium salt, the carrier impregnation step and the drying time are exactly the same as those in Example 1;
[0090] The weight percentage of scandium oxide in the tested catalyst product is 0.43%, the weight percentage of chromium oxide is 2.66%, and the weight percentage of iron oxide is 0.08%.
[0091] The catalyst provided in this comparative example was crushed into particles with a particle size of 1.5-2 mm, and 20 g of the particles were weighed and loaded into a fixed bed reactor of a catalyst activity evaluation device. A gas containing 1.5% by volume of hydrogen sulfide, 0.28% of organic sulfur (COS), 0.05% of elemental sulfur, 0.88% of sulfur dioxide, 3.8% of oxygen, and the balance of nitrogen was introduced and incinerated at 330°C; wherein, the gas flow rate was 650 ml / min, the gas pressure (gauge pressure) was 15 kPa, and the catalyst operating space velocity was converted to 1265 h -1 The volume contents of hydrogen sulfide, COS and sulfur trioxide in the reactor outlet gas were analyzed. The results are shown in Table 1. The volume concentration of hydrogen sulfide was 7.7 pm, COS was 12.3 ppm, and sulfur trioxide was 85 ppm.
[0092] Comparative Example 3
[0093] This comparative example provides a Claus tail gas incineration catalyst
[0094] The difference between the preparation method of the catalyst provided in this comparative example and that in Example 1 is that anhydrous ferric nitrate is used to replace anhydrous scandium nitrate to prepare the mixed solution. The preparation and molding of the carrier, the carrier impregnation step and the drying time are exactly the same as those in Example 1;
[0095] The weight percentage of chromium oxide in the tested catalyst product is 3.98%, and the weight percentage of iron oxide is 2.43%.
[0096] The catalyst provided in this comparative example was crushed into particles with a particle size of 1.5-2 mm, and 20 g of the particles were weighed and loaded into a fixed bed reactor of a catalyst activity evaluation device. A gas containing 1.5% by volume of hydrogen sulfide, 0.28% of organic sulfur (COS), 0.05% of elemental sulfur, 0.88% of sulfur dioxide, 3.8% of oxygen, and the balance of nitrogen was introduced and incinerated at 330°C; wherein, the gas flow rate was 650 ml / min, the gas pressure (gauge pressure) was 15 kPa, and the catalyst operating space velocity was converted to 1265 h -1 The volume contents of hydrogen sulfide, COS and sulfur trioxide in the reactor outlet gas were analyzed. The results are shown in Table 1. The volume concentration of hydrogen sulfide was 6.4 ppm, COS was 19.3 ppm, and sulfur trioxide was 255 ppm.
[0097] Table 1
[0098]
[0099] As can be seen from Table 1, the catalyst of the present invention can effectively inhibit the formation of sulfur trioxide. The volume concentration of sulfur trioxide in the gas after incineration is <1ppm, and the oxidation effect of organic sulfur is excellent. The concentration of organic sulfur in the gas after incineration is <5ppm, and the environmental protection benefit is significant.
[0100] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A Claus tail gas incineration catalyst, wherein: The catalyst uses high-purity silicon dioxide with ultra-low iron impurity content as a carrier to load the active components scandium oxide and chromium oxide; Wherein, in the high-purity silicon dioxide with ultra-low iron impurity content, based on the total mass of the high-purity silicon dioxide with ultra-low iron impurity content as 100%, the silicon dioxide content is greater than 99.9%, and the iron oxide content is less than 0.01%; The loaded active components do not contain iron oxide.
2. The catalyst according to claim 1, wherein Based on 100% of the total mass of the catalyst, the amount of scandium oxide is 0.5-0.8%, and the weight content of chromium oxide is 3.0-4.5%.
3. The catalyst according to claim 1, wherein The high-purity silicon dioxide with ultra-low iron impurity content as a carrier is obtained by tableting high-purity silicon dioxide powder with ultra-low iron impurity content; Among them, the specific surface area of high-purity and ultra-low iron impurity silica powder is 100-150m 2 / g, average particle size of 0.2-0.5 microns, bulk density of 0.1-0.15g / ml; Among them, the tableting pressure is 10-30MPa and the punching time is 1-2s.
4. The catalyst according to claim 1, wherein The high-purity and ultra-low iron impurity silica used as the carrier is in the form of flakes with a diameter of 8-10 mm and a height of 2-3 mm.
5. The method for preparing the Claus tail gas incineration catalyst according to any one of claims 1 to 4, wherein: The method includes: High-purity silicon dioxide with ultra-low iron impurity content as a carrier is placed in a mixed solution of scandium salt and chromium salt for impregnation, and then dried and calcined to obtain the catalyst.
6. The preparation method according to claim 5, wherein: The preparation method also includes the following steps of preparing a carrier: The specific surface area is 100-150m 2 / g, an average particle size of 0.2-0.5 microns, and a bulk density of 0.1-0.15g / ml of high-purity silicon dioxide powder with ultra-low iron impurity content are mixed with water and pressed into tablets, and then the tableted product is dried to obtain a sheet of high-purity silicon dioxide with ultra-low iron impurity content of 8-10mm in diameter and 2-3mm in height as a carrier; Among them, the tableting pressure is 10-30MPa and the punching time is 1-2s.
7. The preparation method according to claim 6, wherein: The mass ratio of high-purity and ultra-low iron impurity silicon dioxide powder to water is 300-400:100-130.
8. The preparation method according to claim 6, wherein: During the drying process of the tablet-formed product, the drying temperature is 120-130°C and the drying time is 2-3h.
9. The preparation method according to claim 6, wherein: Scandium salts include scandium nitrate and / or scandium sulfate; The chromium salt includes one or a combination of two or more of chromium nitrate, chromium chloride and chromium sulfate.
10. The preparation method according to claim 5, wherein: The drying temperature after impregnation is 100-110°C.
11. The preparation method according to claim 5, wherein: The calcination temperature is 350-400°C and the calcination time is 2-3h.
12. Use of the catalyst according to any one of claims 1 to 4 as a catalyst in a Claus tail gas incineration process.
13. The use according to claim 12, wherein: In the above application, the Claus tail gas is passed into an incineration device filled with the catalyst according to any one of claims 1 to 4 for incineration; Wherein, the particle size of the catalyst is 1.5-2 mm; Among them, the gas space velocity of Claus tail gas is 1000-1500h -1 ; Among them, the incineration temperature is 300-350℃.
Citation Information
Patent Citations
Catalyst for selective oxidation of sulfureted hydrogen into elemental sulfur and reaction process thereof
CN101380582A
Honeycomb catalyst for catalytically incinerating sulfur recovery tail gases and preparation method
CN102039137A
Selective catalytic oxidation catalyst for reducing sulfur pollutants as well as preparation method and application of selective catalytic oxidation catalyst
CN115138371A
Catalyst for catalytic incineration of sulphur bearing gas, its preparation method and application
CN1768928A
Process for removing organic sulphur compounds, and / or sulphur oxides and / or nitrogen oxides from gases
EP0214407A2