Reverse-phase copper-zinc catalyst as well as preparation method and application thereof

Porous copper oxide powder was prepared by solid-phase ball milling and ultrasonic dispersion treatment to form a reverse copper-zinc catalyst. Through cation doping, the problem of low activity of the existing catalyst was solved, and efficient CO2 conversion and methanol selectivity improvement were achieved, which is suitable for Industrial applications.

CN118719072APending Publication Date: 2024-10-01NINGXIA UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410730171.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing commercial copper-zinc-aluminum catalysts have problems with poor methanol selectivity and low carbon dioxide conversion rate during the hydrogenation of CO2 to methanol. This is mainly due to the small metal copper substrate area, resulting in insufficient exposure of the ZnO-Cu interface and low catalytic activity.

Method used

The solid-phase ball milling method is used to prepare porous copper oxide powder with a high specific surface area, and a reverse copper-zinc catalyst is formed through ultrasonic dispersion and reducing atmosphere treatment, combined with a small amount of cation doping such as Mg2+ or Y3+ to improve catalytic activity and selectivity.

Benefits of technology

The CO2 conversion rate and methanol selectivity of the catalyst are significantly improved, and the catalytic activity is improved. The preparation method is simple, the cost is low, and it is suitable for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719072A_ABST
    Figure CN118719072A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of nano materials and heterogeneous catalysis, and particularly relates to a reverse copper-zinc catalyst as well as a preparation method and application thereof. The preparation method comprises the following steps: firstly, carrying out primary ball milling on diluted salt and copper salt, then adding a precipitator for secondary ball milling, then adding water for dissolving, washing, drying and calcining the obtained precipitate to obtain porous CuO powder, finally adding water for ultrasonic dissolution, adding a Zn-containing aqueous solution and an alkali solution for stirring, and then carrying out centrifugal washing, drying and reduction on the precipitate to obtain the porous CuO catalyst. The reverse copper-zinc catalyst is obtained. The specific surface area of CuO powder can be increased in a solid-phase ball milling mode, then Zn < 2 + > is doped, the prepared reverse copper-zinc catalyst is high in catalytic activity, CO2 conversion rate and methanol selectivity, the preparation method is simple, the preparation cost is low, and the reverse copper-zinc catalyst has a good application prospect in the field of preparation of methanol through hydrogenation of carbon dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nano materials and heterogeneous catalysis, and specifically relates to a reverse copper-zinc catalyst and a preparation method and application thereof. Background Art

[0002] Currently used for CO 2 Commercial copper-zinc-aluminum catalysts produced by hydrogenation to methanol industry have always had problems such as poor methanol selectivity and low carbon dioxide conversion rate.

[0003] From the nature of the reaction, CO 2 The selective hydrogenation to methanol reaction is a typical structure-sensitive reaction. The physicochemical properties of the ZnO-Cu interface have an important influence on the CO 2 The reaction pathway of hydrogenation to methanol has an important influence. 0 ,Zn δ+ or Zn 2+ ) and Cu(Cu 0 , Cu δ+ or Cu + The actual chemical state of the ZnO-Cu interface is controversial, but regardless of the nature of the ZnO-Cu interface, it is generally believed that a high ZnO-Cu interface area corresponds to a high methanol space-time yield. Therefore, designing a Cu-Zn catalyst with a rich ZnO-Cu interface is of great significance for the development of active CO 2 Hydrogenation catalysts are of great importance.

[0004] Compared with the traditional metal / oxide configuration (M / MO x , M: metal active site, MO x : metal oxide support), the inverse catalyst with oxide / metal configuration (MO x / M) provides a unique perspective to clarify the role of metal-oxide interfaces. At the same time, due to the fully exposed interface sites and more stable thermodynamically supported metal oxide clusters, compared with the conventional metal / oxide configuration M / MO x Compared with the conventional catalyst, the catalytic performance of the reversed Cu catalyst has been significantly improved. Although the performance of the reversed Cu catalyst has been well optimized, the existing methods for preparing reversed Cu-based catalysts are mainly prepared by simple co-precipitation, impregnation or thermal decomposition. The reversed Cu-based catalysts synthesized by these methods often have a small metal copper substrate area, resulting in only a partial exposure of the ZnO-Cu interface during the actual reaction, resulting in low catalytic activity and poor CO 2 The low conversion rate and methanol selectivity limit the development and application of reverse copper-based catalysts. Summary of the invention

[0005] Based on the above technical background, the main purpose of the present invention is to provide a reverse copper-zinc catalyst and a preparation method and application thereof to overcome the deficiencies in the prior art.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0007] The first aspect of the present invention is to provide a method for preparing a reverse copper-zinc catalyst, the preparation method comprising the following steps:

[0008] Step 1, mixing the diluted salt and the copper salt and performing a first ball milling to obtain a first ball milling mixture;

[0009] Step 2, adding a precipitant to the first ball milling mixture and then performing a second ball milling, adding water to the product after the second ball milling for ultrasonic dissolution, and then stirring with a magnetic force, centrifugally washing and drying the obtained precipitate, and finally calcining at a high temperature to obtain a porous CuO powder;

[0010] Step 3: Add water to the porous CuO powder for ultrasonic dispersion, then add the aqueous solution containing Zn and stir, then slowly add the alkaline solution and continue stirring, centrifuge and wash the obtained precipitate, dry it, and reduce it in a reducing atmosphere to obtain a reverse copper-zinc catalyst.

[0011] Preferably, in step 1, the diluting salt is selected from one or more of sodium chloride, potassium chloride, lithium chloride and cesium chloride; and / or,

[0012] Preferably, the copper salt is selected from one or more of copper chloride, copper nitrate, copper acetate, copper acetylacetonate, copper tartrate, copper citrate, copper sulfate, copper carbonate and basic copper carbonate; and / or,

[0013] Preferably, the molar ratio of the diluent salt to the copper salt is (1-20):1; and / or,

[0014] Preferably, large stainless steel balls with a diameter of 1 to 1.5 cm and small stainless steel balls with a diameter of 0.3 to 0.5 cm are added during the ball milling process; and / or,

[0015] Preferably, the first ball milling time is 0.1 to 2 hours.

[0016] Preferably, in step 2, the precipitant is selected from one or more of sodium hydroxide, potassium hydroxide, potassium carbonate, sodium carbonate and sodium bicarbonate; and / or,

[0017] The molar ratio of the precipitant to the first ball-milling mixture is 1:(5-10).

[0018] Preferably, in step 2, the second ball milling time is 0.1 to 1 h; and / or,

[0019] Add water to the product after the second ball milling and dissolve it by ultrasonic for 3 to 10 minutes, and then stir it magnetically for 10 to 20 minutes; and / or,

[0020] The obtained precipitate is washed by centrifugation for 2 to 5 times, then dried at 70 to 90° C. for 20 to 30 hours, and finally calcined at 250 to 350° C. for 0.5 to 2 hours in an air atmosphere.

[0021] Preferably, in step 3,

[0022] Add water to the porous CuO powder and disperse it ultrasonically for 3 to 10 minutes, then add the Zn-containing aqueous solution and stir for 10 to 20 minutes;

[0023] The aqueous solution containing Zn is selected from one or more of a zinc nitrate solution, a zinc acetate solution and a zinc sulfate solution.

[0024] More preferably, the aqueous solution containing Zn is a zinc nitrate solution;

[0025] The molar ratio of the porous CuO powder to zinc nitrate is 1:(0.1-2).

[0026] Further preferably, in step 3, while adding the zinc nitrate solution, Mg(NO 3 ) 2 Solution or Y(NO 3 ) 3 Solution;

[0027] Preferably, the molar ratio of zinc nitrate to magnesium nitrate is (5-15):1;

[0028] Preferably, the molar ratio of yttrium nitrate to magnesium nitrate is (5-15):1.

[0029] Preferably, in step 3, the alkaline solution is selected from one or more of sodium hydroxide, potassium hydroxide, potassium carbonate, sodium carbonate and sodium bicarbonate; and / or,

[0030] Add an alkaline solution to adjust the pH to 7.0-9.5, and continue stirring for 30-90 minutes; and / or,

[0031] The obtained precipitate was washed by centrifugation 2 to 5 times, then dried at 70 to 90 °C for 20 to 30 h, and finally heated to room temperature. 2 / N 2 Reduce in a reducing atmosphere at 250-350°C for 0.5-2h.

[0032] The second aspect of the present invention is to provide a reverse copper-zinc catalyst prepared by the preparation method of the reverse copper-zinc catalyst described in the first aspect of the present invention.

[0033] The third aspect of the present invention is to provide an application of the reverse copper-zinc catalyst described in the second aspect of the present invention in the field of producing methanol by hydrogenation of carbon dioxide.

[0034] The beneficial effects of the present invention are:

[0035] (1) The present invention first adopts a solid phase ball milling method to prepare a porous copper oxide powder with a high specific surface area. The BET specific surface area of ​​the synthesized copper oxide powder is as high as 120 m 2 / g, while the specific surface area of ​​copper oxide synthesized by traditional sol-gel method, thermal decomposition method and precipitation method is less than 20m 2 On this basis, the obtained copper oxide powder and the aqueous solution containing Zn are mixed and stirred, and then the precipitate is centrifuged, washed, dried, and reduced to obtain a reverse copper-zinc catalyst. The reverse copper-zinc catalyst has high catalytic activity and is effective for CO 2 The conversion rate and methanol selectivity are high.

[0036] (2) The present invention adds a small amount of cation doping to the reverse copper-zinc catalyst, such as a small amount of Mg doping. 2+ or Y 3 + , which can further improve the catalytic activity of the reverse copper-zinc catalyst and further improve the selectivity of the reverse copper-zinc catalyst in the hydrogenation of carbon dioxide to methanol at high temperature.

[0037] (3) The preparation method of the reverse copper-zinc catalyst of the present invention is simple, has low preparation cost, has low requirements on instruments, and can be industrially scaled up, thus opening up new ideas for the development and application of reverse copper-zinc catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 A transmission electron microscope photograph of the porous copper oxide powder prepared in Example 1 is shown;

[0039] Figure 2 A high-resolution transmission electron microscope photograph of the high-performance reverse copper-zinc catalyst with 5 wt.% ZnO-Cu prepared in Example 1 is shown;

[0040] Figure 3 A high-resolution transmission electron micrograph of a high-performance inverse copper-zinc catalyst with 50 wt.% ZnO-Cu prepared in Example 2 is shown;

[0041] Figure 4 A high-resolution transmission electron micrograph of a 100 wt.% ZnO-Cu high-performance inverse copper-zinc catalyst prepared in Example 3 is shown;

[0042] Figure 5 The XRD spectrum of the high performance reverse copper-zinc catalyst with 5 wt.% ZnO-Cu prepared in Example 1 is shown;

[0043] Figure 6 The XRD spectrum of the high performance reverse copper-zinc catalyst with 50 wt.% ZnO-Cu prepared in Example 2 is shown;

[0044] Figure 7 The XRD spectrum of the high performance reverse copper-zinc catalyst with 100 wt.% ZnO-Cu prepared in Example 3 is shown;

[0045] Figure 8 The XRD spectra of the reverse copper-zinc catalysts prepared in Example 2, Example 7 and Example 8 are shown;

[0046] Fig. 9 The carbon dioxide hydrogenation activity diagram of the reverse copper-zinc catalyst prepared in Examples 1-6 is shown;

[0047] Fig.10 The carbon dioxide hydrogenation activity diagrams of the reverse copper-zinc catalysts prepared in Example 2, Example 7, and Example 8 are shown. DETAILED DESCRIPTION

[0048] The present invention will be described in detail below, and the characteristics and advantages of the present invention will become clearer and more distinct with the description.

[0049] The first aspect of the present invention is to provide a method for preparing a reverse copper-zinc catalyst, the preparation method comprising the following steps:

[0050] Step 1, mixing the diluted salt and the copper salt and performing a first ball milling to obtain a first ball milling mixture;

[0051] Step 2, adding a precipitant to the first ball milling mixture and then performing a second ball milling, adding water to the product after the second ball milling for ultrasonic dissolution, and then stirring with a magnetic force, centrifugally washing and drying the obtained precipitate, and finally calcining at a high temperature to obtain a porous CuO powder;

[0052] Step 3: Add water to the porous CuO powder for ultrasonic dispersion, then add the aqueous solution containing Zn and stir, then slowly add the alkaline solution and continue stirring, centrifuge and wash the obtained precipitate, dry it, and reduce it in a reducing atmosphere to obtain a reverse copper-zinc catalyst.

[0053] The above steps are described in detail below.

[0054] In step 1, the diluting salt is selected from one or more of sodium chloride, potassium chloride, lithium chloride and cesium chloride, preferably sodium chloride.

[0055] The copper salt is selected from one or more of copper chloride, copper nitrate, copper acetate, copper acetylacetonate, copper tartrate, copper citrate, copper sulfate, copper carbonate and basic copper carbonate, preferably copper chloride.

[0056] The molar ratio of the diluent salt to the copper salt is (1-20):1, and the preferred molar ratio is (8-9):1.

[0057] The ball milling is carried out in a stainless steel ball mill tank, and 3 to 5 large stainless steel balls with a diameter of 1 to 1.5 cm and 10 to 15 small stainless steel balls with a diameter of 0.3 to 0.5 cm are added during the ball milling process.

[0058] Preferably, 4 large stainless steel balls with a diameter of 1.2 cm and 12 small stainless steel balls with a diameter of 0.4 cm are added during the ball milling process.

[0059] The time of the first ball milling is 0.1 to 2 hours, and preferably the time of the first ball milling is 0.5 hours.

[0060] In step 2, the precipitating agent is selected from one or more of sodium hydroxide, potassium hydroxide, potassium carbonate, sodium carbonate and sodium bicarbonate, preferably sodium hydroxide.

[0061] The molar ratio of the precipitant to the first ball-milling mixture is 1:(5-10), preferably 1:(9-10).

[0062] The second ball milling time is 0.1 to 1 h, and preferably the second ball milling time is 0.5 h.

[0063] Add water to the product after the second ball milling and dissolve it by ultrasonic for 3 to 10 minutes, and then stir it magnetically for 10 to 20 minutes.

[0064] Preferably, water is added to the product after the second ball milling to dissolve it by ultrasonic for 5 minutes, and then magnetically stirred for 15 minutes.

[0065] The obtained precipitate is washed by centrifugation for 2 to 5 times, then dried at 70 to 90° C. for 20 to 30 hours, and finally calcined at 250 to 350° C. for 0.5 to 2 hours in an air atmosphere.

[0066] Preferably, the obtained precipitate is washed by centrifugation for 3 times, then dried at 80° C. for 24 h, and finally calcined at 300° C. for 1 h in an air atmosphere.

[0067] In step 3, water is added to the porous CuO powder for ultrasonic dispersion for 3 to 10 minutes, and then a Zn-containing aqueous solution is added and stirred for 10 to 20 minutes.

[0068] Preferably, water is added to the porous CuO powder and ultrasonically dispersed for 5 minutes, and then the Zn-containing aqueous solution is added and stirred for 15 minutes.

[0069] The Zn-containing aqueous solution is selected from one or more of zinc nitrate solution, zinc acetate solution and zinc sulfate solution, preferably zinc nitrate solution.

[0070] The molar ratio of the porous CuO powder to zinc nitrate is 1:(0.1-2), and preferably, the molar ratio of the porous CuO powder to zinc nitrate is 1:1.

[0071] In the process of carbon dioxide hydrogenation, the high-performance carbon dioxide to methanol reverse copper-zinc catalyst prepared by the present invention is found to have a volcano curve relationship between the time-space yield of methanol and the ZnO loading, that is, when the molar ratio of porous CuO powder to zinc nitrate is 1:1, the reverse copper-zinc catalyst with a ZnO loading of 50wt.% has the highest catalytic activity and the highest methanol selectivity.

[0072] According to a preferred embodiment of the present invention, when adding zinc nitrate solution, Mg(NO 3 ) 2 Solution or Y(NO 3 ) 3 Solution.

[0073] The molar ratio of zinc nitrate to magnesium nitrate is (5-15):1, and the preferred molar ratio is 10:1.

[0074] The molar ratio of yttrium nitrate to magnesium nitrate is (5-15):1, and the preferred molar ratio is 10:1.

[0075] It was found that adding a small amount of Mg to the inverse copper-zinc catalyst 2+ or Y 3+ The selectivity of producing methanol by hydrogenation of carbon dioxide can be further improved.

[0076] The alkaline solution is selected from one or more of sodium hydroxide, potassium hydroxide, potassium carbonate, sodium carbonate and sodium bicarbonate, preferably potassium carbonate.

[0077] Add an alkaline solution to adjust the pH to 7.0-9.5, and continue stirring for 30-90 min, preferably adjust the pH to 8, and continue stirring for 60 min.

[0078] The obtained precipitate was washed by centrifugation 2 to 5 times, then dried at 70 to 90 °C for 20 to 30 h, and finally heated to room temperature. 2 / N 2 Reduce in a reducing atmosphere at 250-350°C for 0.5-2h.

[0079] Preferably, the obtained precipitate is washed by centrifugation 3 times, then dried at 80°C for 24 h, and finally heated to 5 vol.% H 2 / N 2 The samples were reduced at 300 °C in a reducing atmosphere for 1 h.

[0080] The second aspect of the present invention is to provide a reverse copper-zinc catalyst prepared by the preparation method of the reverse copper-zinc catalyst described in the first aspect of the present invention.

[0081] The inverse copper-zinc catalyst has a methanol selectivity of nearly 99.0% at low temperature, and the supported ZnO is doped with cations (such as Mg 2+ or Y 3+ ), which can further improve the catalytic activity of the reverse copper-zinc catalyst and the selectivity of carbon dioxide hydrogenation to methanol at high temperature. The doped reverse copper-zinc catalyst still has 70% methanol selectivity at a high temperature of 260°C.

[0082] The third aspect of the present invention is to provide an application of the reverse copper-zinc catalyst described in the second aspect of the present invention in the field of producing methanol by hydrogenation of carbon dioxide.

[0083] Example

[0084] The present invention is further described below by means of specific examples. These embodiments are only intended to illustrate the present invention but are not intended to limit the scope of the present invention.

[0085] The raw materials used in the embodiments of the present invention are all purchased.

[0086] Example 1

[0087] 1 g NaCl (17.09 mmol) and 2 mmol CuCl 2 The mixture was added to a 50 mL stainless steel ball mill jar containing 4 large stainless steel balls with a diameter of 1.2 cm and 12 small stainless steel balls with a diameter of 0.4 cm. The ball mill jar was sealed and transferred to a three-dimensional high-speed vibration ball mill (MSK-SFM-3) for the first ball milling run of 0.5 h.

[0088] Subsequently, 2 mmol of NaOH solid was added to the above mixture, and ball milling was continued for 0.5 h. The product after the second ball milling was transferred to a round-bottom flask, 50 ml of deionized water was added, and ultrasonic assisted rapid dissolution. After ultrasonication for 5 min, stirring was continued for 15 min under strong magnetic stirring. The obtained precipitate was centrifuged and washed 3 times, dried at 80 ° C for 24 h, and then calcined at 300 ° C in air atmosphere for 1 h to obtain porous CuO powder.

[0089] Weigh 2 mmol of the above CuO powder and add it to the flask, then add 50 ml of deionized water to the flask and disperse it quickly with the help of ultrasound. After 5 minutes of ultrasound, slowly drop 0.4 mL of 0.5 mol / L Zn(NO 3 ) 2 After stirring for 15 minutes, slowly add 0.5 mol / L K2 (CO 3 ) 2 The solution was stirred for 60 min, and the precipitate in the flask was washed by centrifugation for 3 times, dried at 80 °C for 24 h, and finally heated to 5 vol.% H 2 / N 2 The high performance reverse copper-zinc catalyst with 5 wt.% ZnO-Cu was obtained by reduction at 300 °C for 1 h in a reducing atmosphere.

[0090] Figure 1 The transmission electron microscope image of porous CuO powder is shown. Figure 1 It can be seen that the average particle size of the prepared porous CuO powder is about 7.3 nm.

[0091] Example 2

[0092] The inverse copper-zinc catalyst was prepared in a similar manner to Example 1, except that 2 mmol of the above CuO powder was weighed and added to a flask, and then 50 ml of deionized water was added to the flask, and ultrasound was used to assist in its rapid dispersion. After ultrasound for 5 min, 4 mL of 0.5 mol / L Zn(NO 3 ) 2 After stirring for 15 minutes, slowly add 0.5 mol / L K 2 (CO 3 ) 2 The solution was stirred for 60 min, and the precipitate in the flask was washed by centrifugation for 3 times, dried at 80 °C for 24 h, and finally heated to 5 vol.% H 2 / N 2 The catalyst was reduced at 300 °C for 1 h in a reducing atmosphere to obtain a high performance inverse copper-zinc catalyst with 50 wt.% ZnO-Cu.

[0093] Example 3

[0094] The inverse copper-zinc catalyst was prepared in a similar manner to Example 1, except that 2 mmol of the above CuO powder was weighed and added to a flask, and then 50 ml of deionized water was added to the flask, and ultrasound was used to assist in its rapid dispersion. After ultrasound for 5 min, 8 mL of 0.5 mol / L Zn(NO 3 ) 2 After stirring for 15 minutes, slowly add 0.5 mol / L K 2 (CO 3 ) 2The solution was stirred for 60 min, and the precipitate in the flask was washed by centrifugation for 3 times, dried at 80 °C for 24 h, and finally heated to 5 vol.% H 2 / N 2 The catalyst was reduced at 300 °C for 1 h in a reducing atmosphere to obtain a high performance inverse copper-zinc catalyst with 100 wt.% ZnO-Cu.

[0095] Example 4

[0096] The inverse copper-zinc catalyst was prepared in a similar manner to Example 1, except that 2 mmol of the above CuO powder was weighed and added to a flask, and then 50 ml of deionized water was added to the flask, and ultrasound was used to assist in its rapid dispersion. After ultrasound for 5 min, 1.6 mL of 0.5 mol / L Zn(NO 3 ) 2 After stirring for 15 minutes, slowly add 0.5 mol / L K 2 (CO 3 ) 2 The solution was stirred for 60 min, and the precipitate in the flask was washed by centrifugation for 3 times, dried at 80 °C for 24 h, and finally heated to 5 vol.% H 2 / N 2 The catalyst was reduced at 300 °C for 1 h in a reducing atmosphere to obtain a high performance reverse copper-zinc catalyst with 20 wt.% ZnO-Cu.

[0097] Example 5

[0098] The inverse copper-zinc catalyst was prepared in a similar manner to Example 1, except that 2 mmol of the above CuO powder was weighed and added to a flask, and then 50 ml of deionized water was added to the flask, and ultrasound was used to assist in its rapid dispersion. After ultrasound for 5 min, 2.4 mL of 0.5 mol / L Zn(NO 3 ) 2 After stirring for 15 minutes, slowly add 0.5 mol / L K 2 (CO 3 ) 2 The solution was stirred for 60 min, and the precipitate in the flask was washed by centrifugation for 3 times, dried at 80 °C for 24 h, and finally heated to 5 vol.% H 2 / N 2 The catalyst was reduced at 300 °C for 1 h in a reducing atmosphere to obtain a high performance reverse copper-zinc catalyst with 30 wt.% ZnO-Cu.

[0099] Example 6

[0100] The inverse copper-zinc catalyst was prepared in a similar manner to Example 1, except that 2 mmol of the above CuO powder was weighed and added to a flask, and then 50 ml of deionized water was added to the flask, and ultrasound was used to assist in its rapid dispersion. After ultrasound for 5 min, 5.6 mL of 0.5 mol / L Zn(NO 3 ) 2 After stirring for 15 minutes, slowly add 0.5 mol / L K 2 (CO 3 ) 2 The solution was stirred for 60 min, and the precipitate in the flask was washed by centrifugation for 3 times, dried at 80 °C for 24 h, and finally heated to 5 vol.% H 2 / N 2 The catalyst was reduced at 300 °C for 1 h in a reducing atmosphere to obtain a high performance inverse copper-zinc catalyst with 70 wt.% ZnO-Cu.

[0101] Example 7

[0102] 1 g NaCl (17.09 mmol) and 2 mmol CuCl 2 The mixture was added to a 50 mL stainless steel ball mill jar containing 4 large stainless steel balls with a diameter of 1.2 cm and 12 small stainless steel balls with a diameter of 0.4 cm. The ball mill jar was sealed and transferred to a three-dimensional high-speed vibration ball mill (MSK-SFM-3) for the first ball milling run of 0.5 h.

[0103] Subsequently, 2 mmol of NaOH solid was added to the above mixture, and ball milling was continued for 0.5 h. The product after the second ball milling was transferred to a round-bottom flask, 50 ml of deionized water was added, and ultrasonic assisted rapid dissolution. After ultrasonication for 5 min, stirring was continued for 15 min under strong magnetic stirring. The obtained precipitate was centrifuged and washed 3 times, dried at 80 ° C for 24 h, and then calcined at 300 ° C in air atmosphere for 1 h to obtain porous CuO powder.

[0104] Weigh 2 mmol of the above CuO powder into a flask, then add 50 ml of deionized water to the flask and disperse it quickly with the help of ultrasound. After 5 minutes of ultrasound, slowly drop 4 mL of 0.5 mol / L Zn(NO 3 ) 2 and 0.05 mol / L Mg(NO 3 ) 2 After stirring for 15 minutes, slowly add 0.5 mol / L K 2 (CO3 ) 2 The solution was stirred for 60 min, and the precipitate in the flask was washed by centrifugation for 3 times, dried at 80 °C for 24 h, and finally heated to 5 vol.% H 2 / N 2 The high performance reverse copper-zinc catalyst with 50 wt.% Mg-ZnO-Cu was obtained by reduction at 300 °C for 1 h in a reducing atmosphere.

[0105] Example 8

[0106] The inverse copper-zinc catalyst was prepared in a manner similar to that of Example 4, except that 2 mmol of the above CuO powder was weighed in a flask, and then 50 ml of deionized water was added to the flask, and the mixture was rapidly dispersed by ultrasound. After 5 min of ultrasound, 4 ml of 0.5 mol / L Zn(NO 3 ) 2 and 0.05 mol / L Y(NO 3 ) 3 After stirring for 15 minutes, slowly add 0.5 mol / L K 2 (CO 3 ) 2 The solution was stirred for 60 min, and the precipitate in the flask was washed by centrifugation for 3 times, dried at 80 °C for 24 h, and finally heated to 5 vol.% H 2 / N 2 The catalyst was reduced at 300 °C for 1 h in a reducing atmosphere to obtain a high-performance reverse copper-zinc catalyst with 50 wt.% Y-ZnO-Cu.

[0107] Experimental example

[0108] Experimental Example 1 High Resolution Transmission Electron Microscope Test

[0109] The inverse copper-zinc catalysts prepared in Example 1, Example 2 and Example 3 were tested by high-resolution transmission electron microscopy. The test results are as follows: Figure 2 , Figure 3 and Figure 4 shown.

[0110] from Figure 2 , Figure 3 and Figure 4 It can be seen that the inverse copper-zinc catalysts prepared in Example 1, Example 2 and Example 3 have different ZnO dispersions.

[0111] Experimental Example 2 X-ray diffraction test

[0112] The inverse copper-zinc catalysts prepared in Example 1, Example 2 and Example 3 were subjected to XRD tests, and the test results were as follows: Figure 5 , Figure 6 and Figure 7 As shown, the inverse copper-zinc catalysts prepared in Example 2, Example 7 and Example 8 were subjected to XRD test, and the test results are shown in FIG. Figure 8 shown.

[0113] from Figure 5 , Figure 6 and Figure 7 It can be seen that the inverse copper-zinc catalysts prepared in Example 1, Example 2 and Example 3 have higher crystallinity.

[0114] from Figure 8 It can be seen that the inverse copper-zinc catalysts prepared in Example 2, Example 7 and Example 8 have higher crystallinity.

[0115] Experimental Example 3 Carbon dioxide hydrogenation activity test

[0116] The inverse copper-zinc catalysts prepared in Examples 1-6 were tested for carbon dioxide hydrogenation activity. The carbon dioxide hydrogenation to methanol test was carried out in a temperature-controlled microreactor (HDJG-HPCTS, Xiamen Hande Engineering Co., Ltd.). The reactor was equipped with an online gas chromatograph (GC2060, Shanghai Ruimin Instrument Co., Ltd.). The specific test method is as follows: 100 mg of catalyst and a certain amount of silica sand were added to a quartz tube reactor (inner diameter 8 mm). Before the test, the catalyst was heated to 40 ℃ and then heated to 30 ℃. 2 / N 2 Mixed gas (H 2 : 5 vol.%, 30 ml / min) at 300 °C for 2 h. After the reactor was cooled to 170 °C, H 2 / N 2 The mixture is switched to the reactant mixture (CO 2 , H 2 and N 2 The reaction weight hourly space velocity (WHSV) was calculated to be 6,000 ml based on the flow rate of the reactant mixed gas and the catalyst used. -1 g -1 h -1 The product was then analyzed using an online gas chromatograph with a thermal conductivity detector (TCD) and a flame ionization detector (FID). Fig. 9 As shown, the inverse copper-zinc catalysts prepared in Example 2, Example 7, and Example 8 were tested for carbon dioxide hydrogenation activity. The test results are shown in FIG. Fig.10 shown.

[0117] from Fig. 9 and Fig.10 It can be seen that the inverse copper-zinc catalysts prepared in Examples 1-8 have excellent carbon dioxide hydrogenation performance and excellent methanol selectivity at high temperatures. Fig. 9 The reverse copper-zinc catalyst prepared in Example 2 has the highest methanol selectivity at all temperatures, which is better than the reverse copper-zinc catalysts prepared in Example 1 and Examples 3-6. The reverse copper-zinc catalyst prepared in Example 2 has a methanol selectivity of more than 99% at 170°C and a methanol selectivity of more than 55% at a high temperature of 260°C. Fig.10 The methanol selectivity of the inverse copper-zinc catalysts prepared in Examples 7 and 8 at a low temperature of 170°C can reach 100%, and the methanol selectivity at a high temperature of 260°C can still reach 70%, both of which are better than the inverse copper-zinc catalyst prepared in Example 2. This shows that the inverse copper-zinc catalyst prepared by the preparation method of the present invention has excellent carbon dioxide hydrogenation performance and excellent methanol selectivity at high temperatures. At the same time, doping a small amount of Mg into the inverse copper-zinc catalyst 2+ or Y 3+ Its methanol selectivity can be further improved.

[0118] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a reverse copper-zinc catalyst, It is characterized in that The preparation method comprises the following steps: Step 1, mixing the diluted salt and the copper salt and performing a first ball milling to obtain a first ball milling mixture; Step 2, adding a precipitant to the first ball milling mixture and then performing a second ball milling, adding water to the product after the second ball milling for ultrasonic dissolution, and then stirring with a magnetic force, centrifugally washing and drying the obtained precipitate, and finally calcining at a high temperature to obtain a porous CuO powder; Step 3: Add water to the porous CuO powder for ultrasonic dispersion, then add the aqueous solution containing Zn and stir, then slowly add the alkaline solution and continue stirring, centrifuge and wash the obtained precipitate, dry it, and reduce it in a reducing atmosphere to obtain a reverse copper-zinc catalyst.

2. The preparation method according to claim 1, It is characterized in that In step 1, The diluting salt is selected from one or more of sodium chloride, potassium chloride, lithium chloride and cesium chloride; and / or, The copper salt is selected from one or more of copper chloride, copper nitrate, copper acetate, copper acetylacetonate, copper tartrate, copper citrate, copper sulfate, copper carbonate and basic copper carbonate; and / or, The molar ratio of the diluent salt to the copper salt is (1-20):1; and / or, During the ball milling process, large stainless steel balls with a diameter of 1 to 1.5 cm and small stainless steel balls with a diameter of 0.3 to 0.5 cm are added; and / or, The time of the first ball milling is 0.1 to 2 hours.

3. The preparation method according to claim 1, It is characterized in that In step 2, The precipitant is selected from one or more of sodium hydroxide, potassium hydroxide, potassium carbonate, sodium carbonate and sodium bicarbonate; and / or, The molar ratio of the precipitant to the first ball-milling mixture is 1:(5-10).

4. The preparation method according to claim 1, It is characterized in that In step 2, The second ball milling time is 0.1 to 1 h; and / or, Add water to the product after the second ball milling and dissolve it by ultrasonic for 3 to 10 minutes, and then stir it magnetically for 10 to 20 minutes; and / or, The obtained precipitate is washed by centrifugation for 2 to 5 times, then dried at 70 to 90° C. for 20 to 30 hours, and finally calcined at 250 to 350° C. for 0.5 to 2 hours in an air atmosphere.

5. The preparation method according to claim 1, It is characterized in that In step 3, Add water to the porous CuO powder and disperse it ultrasonically for 3 to 10 minutes, then add the Zn-containing aqueous solution and stir for 10 to 20 minutes; The aqueous solution containing Zn is selected from one or more of a zinc nitrate solution, a zinc acetate solution and a zinc sulfate solution.

6. The preparation method according to claim 5, It is characterized in that In step 3, The Zn-containing aqueous solution is a zinc nitrate solution; The molar ratio of the porous CuO powder to zinc nitrate is 1:(0.1-2).

7. The preparation method according to claim 5, It is characterized in that In step 3, When zinc nitrate solution was added, Mg(NO 3 ) 2 Solution or Y(NO 3 ) 3 Solution; The molar ratio of zinc nitrate to magnesium nitrate is (5-15):1; The molar ratio of yttrium nitrate to magnesium nitrate is (5-15):

1.

8. The preparation method according to claim 1, It is characterized in that In step 3, The alkaline solution is selected from one or more of sodium hydroxide, potassium hydroxide, potassium carbonate, sodium carbonate and sodium bicarbonate; and / or, Add an alkaline solution to adjust the pH to 7.0-9.5, and continue stirring for 30-90 minutes; and / or, The obtained precipitate was washed by centrifugation 2 to 5 times, then dried at 70 to 90 °C for 20 to 30 h, and finally heated to room temperature. 2 / N 2 Reduce in a reducing atmosphere at 250-350°C for 0.5-2h.

9. A reverse copper-zinc catalyst prepared by the preparation method of the reverse copper-zinc catalyst according to any one of claims 1 to 8.

10. Use of the reverse copper-zinc catalyst according to claim 9 in the field of producing methanol by hydrogenation of carbon dioxide.

Citation Information

Patent Citations

  • Catalyst used for catalyzing and eliminating toluene in air and preparation method of catalyst

    CN102909031A

  • Mesoporous solid acid catalyst for esterification reaction and preparation method thereof