Modified nickel molecular sieve catalyst as well as preparation method and application thereof

Low-temperature catalytic cracking technology using modified nickel molecular sieve catalysts solves the problems of low catalyst stability and low aromatic hydrocarbon yield in high-temperature treatment of polyolefin waste plastics, achieves efficient and low-cost aromatic hydrocarbon production, and demonstrates the excellent performance of the catalyst Reusable performance.

CN118719129APending Publication Date: 2024-10-01ZHEJIANG UNIV

Patent Information

Application Number
CN202410707931.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing catalytic pyrolysis technology of polyolefin waste plastics, high temperatures lead to low catalyst stability, low aromatic hydrocarbon yield, and high equipment costs, making it difficult to achieve effective low-temperature treatment and high-selectivity conversion to aromatic hydrocarbons.

Method used

Using a modified nickel molecular sieve catalyst, the molecular sieve carrier is calcined and activated and mixed with a nickel salt solution, followed by hydrogen reduction and oxygen-nitrogen mixed gas passivation treatment to prepare a catalyst with high catalytic activity and reusability for low-temperature catalytic cracking. Polyolefin waste plastics to generate aromatics with high selectivity and yield.

Benefits of technology

The low-temperature treatment of polyolefin waste plastics is achieved, the yield and selectivity of aromatic hydrocarbons are improved, the reaction temperature and equipment costs are reduced, the catalyst can be reused, and the process is simple.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004873180650000061
    Figure BDA0004873180650000061
  • Figure BDA0004873180650000071
    Figure BDA0004873180650000071
  • Figure BDA0004873180650000081
    Figure BDA0004873180650000081
Patent Text Reader

Abstract

The invention provides a modified nickel molecular sieve catalyst as well as a preparation method and application thereof. The preparation method comprises the following steps: calcining and activating a molecular sieve carrier, immersing the molecular sieve carrier into a nickel salt solution, stirring, aging, drying, and then reducing and passivating. The preparation method is simple in process, and the nickel metal is low in cost. The synergistic effect between the nickel metal and the molecular sieve carrier in the prepared modified nickel molecular sieve catalyst can obviously improve the performance of the catalyst for preparing the aromatic hydrocarbon by directionally converting the polyolefin waste plastics, and the yield of the aromatic hydrocarbon is improved. The modified nickel molecular sieve catalyst can catalytically treat the polyolefin waste plastics common in life, the polyolefin waste plastics and the modified nickel molecular sieve catalyst are directly mixed in the catalysis process and then placed in a catalytic cracking reactor, the reaction temperature is low (within 300 DEG C), the condition is mild, stirring and reaction solvent are not needed, the process is simple and easy to implement, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waste plastic treatment, and specifically relates to a modified nickel molecular sieve catalyst and a preparation method and application thereof. Background Art

[0002] Waste plastic pollution is becoming increasingly serious and has become an environmental threat that needs to be urgently addressed in modern society. Polyolefins account for the largest portion of waste plastics, but polyolefin waste plastics are more difficult to recycle due to their high chemical inertness, resulting in a recycling rate of less than 10%. Polyolefins are basic hydrocarbons for meeting energy needs. Timely recycling of waste polyolefins and upgrading them to value-added chemicals as much as possible is of great significance to environmental protection and resource recovery.

[0003] Pyrolysis of polyolefin waste plastics is a typical waste plastic resource recovery process and has been a research hotspot in recent years. Through the pyrolysis process, the long-chain hydrocarbons in the waste plastics break at high temperatures to form smaller hydrocarbon molecules, which are further converted into petroleum products or other chemicals through the action of catalysts. This technology can effectively process waste plastics and convert them into growth chemicals instead of simply landfilling or incinerating them. It not only significantly reduces the pollution of waste plastics to the environment, but also reduces greenhouse gas emissions, which is of great significance to environmental protection.

[0004] However, the catalytic pyrolysis technology of polyolefin waste plastics also has some challenges and limitations. The reaction temperature of the waste plastic pyrolysis process is usually above 500°C. The higher reaction temperature increases the energy required for the conversion of waste plastics. At the same time, too high a temperature may make the pyrolysis products unstable, or even cause secondary reactions to generate undesirable products. In addition, high temperatures also have higher requirements on the materials of the reaction equipment, which increases equipment investment and operating costs.

[0005] At the same time, aromatics are a class of hydrocarbon compounds with unique structural characteristics. As the core raw material of the chemical industry, they are widely used in industrial production. If waste plastics can be converted into products such as aromatics, huge economic benefits will be generated. However, with aromatics as the target product, it is still a challenge to improve the selectivity of aromatics while lowering the reaction temperature of waste plastics. The metal loading and carrier structure in the catalyst are important factors affecting the yield of the target product. By selecting a suitable catalyst, the distribution of pyrolysis products can be regulated to improve the selectivity and yield of the target product. Although methods for preparing aromatics by catalytic pyrolysis of waste plastics have emerged in current research, the high reaction temperature and complex secondary reactions result in low catalyst stability and low aromatics yield. Therefore, developing a simple process for preparing aromatics by low-temperature treatment of polyolefin waste plastics is an urgent problem to be solved in related fields. Summary of the invention

[0006] In order to solve the problems existing in the prior art, the present invention provides a modified nickel molecular sieve catalyst and a preparation method and application thereof. The preparation method uses transition metal nickel to modify the molecular sieve catalyst, and the synergistic effect between the metal nickel and the molecular sieve carrier in the obtained catalyst can significantly improve the performance of the catalyst in directional conversion of polyolefin waste plastics to prepare aromatic hydrocarbons, and improve the yield of preparing aromatic hydrocarbons from polyolefin waste plastics. The preparation method has a simple process, high catalytic activity and is reusable, and can effectively realize the high-value utilization of polyolefin waste plastics.

[0007] A method for preparing a modified nickel molecular sieve catalyst comprises the following steps:

[0008] (1) placing the molecular sieve carrier in a muffle furnace for calcination and activation, then immersing it in a nickel salt solution, mixing it evenly, aging it, and drying it to obtain an intermediate product;

[0009] (2) The intermediate product is placed in a tubular furnace and sequentially subjected to hydrogen reduction and nitrogen and oxygen mixed gas passivation to obtain a modified nickel molecular sieve catalyst.

[0010] In the above step (1):

[0011] Preferably, the molecular sieve carrier is one or more of ZSM-5, HY, β, SAPO-34, and MOR. More preferably, it is one of ZSM-5 and HY. More preferably, the molecular sieve carrier is ZSM-5, wherein the molar ratio of Si / Al is (100-150):1. More preferably, it is (120-140):1. Specifically, it is preferably 130:1.

[0012] Preferably, the mass ratio of the molecular sieve carrier to the nickel salt is 1:(0.1-1), more preferably 1:(0.2-0.6), and even more preferably 1:(0.2-0.3).

[0013] Preferably, the calcination temperature of the molecular sieve carrier is 400-600°C, and the calcination time is 2-6 hours. More preferably, the calcination temperature of the molecular sieve carrier is 450-550°C, and the calcination time is 3-5 hours. More preferably, the calcination temperature of the molecular sieve carrier is 500°C, and the calcination time is 4 hours.

[0014] Preferably, the nickel salt solution is prepared by dissolving nickel nitrate hexahydrate in deionized water, wherein the concentration of nickel nitrate hexahydrate is 10 to 80 g / L. Specifically, nickel nitrate hexahydrate is placed in deionized water and magnetically stirred for 30 to 90 minutes to obtain the nickel salt solution.

[0015] More preferably, the concentration of nickel nitrate hexahydrate in the nickel salt solution is 15 to 40 g / L, and even more preferably 20 to 30 g / L.

[0016] More preferably, the magnetic stirring time is 50 to 70 minutes, and even more preferably 60 minutes.

[0017] Preferably, the activated molecular sieve carrier is immersed in the nickel salt solution and mixed by magnetic stirring for 10 to 50 minutes, wherein the stirring speed is 200 to 400 rpm. More preferably, the magnetic stirring is performed for 20 to 40 minutes for mixing, wherein the stirring speed is 250 to 350 rpm. More preferably, the magnetic stirring is performed for 30 minutes for mixing, wherein the stirring speed is 300 rpm.

[0018] Preferably, the aging temperature is 50-70°C, and the aging time is 2-4 hours. More preferably, the aging temperature is 60-70°C, and the aging time is 2.5-3.5 hours. More preferably, the aging temperature is 67°C, and the aging time is 3 hours.

[0019] Preferably, the drying temperature is 100-150°C, and the drying time is 10-20 hours. More preferably, the drying temperature is 110-130°C, and the drying time is 12-18 hours. Even more preferably, the drying temperature is 120°C, and the drying time is 15 hours.

[0020] In the above step (2):

[0021] Preferably, the temperature of hydrogen reduction is 300-500°C, and the time is 2-5 hours. More preferably, the temperature of hydrogen reduction is 400-500°C, and the time is 2-4 hours. More preferably, the temperature of hydrogen reduction is 450°C, and the time is 3 hours.

[0022] Preferably, the hydrogen flow rate is 50 to 200 mL / min, more preferably 80 to 120 mL / min, and even more preferably 100 mL / min.

[0023] Preferably, in the mixed gas, the volume ratio of nitrogen to oxygen is 98:2, and the flow rate of the mixed gas is 20 to 70 mL / min. More preferably, the flow rate of the mixed gas is 40 to 60 mL / min. Even more preferably, the flow rate of the mixed gas is 50 mL / min.

[0024] Preferably, the passivation is carried out at room temperature for 20 to 40 minutes, and more preferably, the passivation time is 30 minutes.

[0025] As a specific preference, the intermediate product is placed in a tubular furnace, hydrogen is introduced to carry out a reduction reaction, and after the reduction reaction is completed, a mixed gas of nitrogen and oxygen is introduced to carry out a passivation reaction to obtain a modified nickel molecular sieve catalyst.

[0026] A modified nickel molecular sieve catalyst is prepared by any of the above-mentioned methods for preparing the modified nickel molecular sieve catalyst.

[0027] A low-temperature treatment method for polyolefin waste plastics, wherein the polyolefin waste plastics and a catalyst are uniformly mixed and then placed in a catalytic cracking reactor for catalytic reaction, and after the reaction is completed, condensation and centrifugal separation are performed to obtain a liquid product rich in aromatics;

[0028] The catalyst is the modified nickel molecular sieve catalyst.

[0029] Preferably, the mass ratio of the catalyst to the polyolefin waste plastic is 1:(1-10), more preferably 1:(5-10), and even more preferably 1:8.

[0030] Preferably, the catalytic reaction temperature is 260-300°C, and the reaction time is 0.5-24h. More preferably, the catalytic reaction temperature is 270-290°C, and the reaction time is 0.5-6h. More preferably, the catalytic reaction temperature is 280°C, and the reaction time is 0.5-2h. More preferably, the reaction time is 1h.

[0031] Preferably, the catalytic reaction is carried out in a nitrogen atmosphere with a nitrogen pressure of 1 to 4 MPa, more preferably 2 to 3 MPa, and even more preferably 2 MPa.

[0032] Preferably, the polyolefin waste plastic is one or both of low-density polyethylene (LDPE) and high-density polyethylene (HDPE).

[0033] Under the action of modified nickel molecular sieve catalyst, polyolefin waste plastics are catalytically cracked, and the products are condensed after the reaction. The non-condensable gases (C1-C5 hydrocarbons) are collected by air bags. The condensed liquid products (hydrocarbons above C5) are separated from the solid products and the catalyst after the reaction by centrifugation to obtain liquid products rich in aromatics.

[0034] The catalyst after the reaction is calcined at high temperature and regenerated in step (2) before being reused. The calcination temperature is 400-600°C and the calcination time is 2-6 hours. Preferably, the calcination temperature is 500°C and the calcination time is 4 hours.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] The preparation method of the modified nickel molecular sieve catalyst of the present invention comprises the following steps: first calcining and activating the molecular sieve carrier, immersing the molecular sieve carrier in a nickel salt solution, stirring, aging, drying, and then performing reduction and passivation treatment. The preparation method has a simple process and low nickel metal cost. The synergistic effect between the nickel metal and the molecular sieve carrier in the prepared modified nickel molecular sieve catalyst can significantly improve the performance of the catalyst in directional conversion of polyolefin waste plastics to prepare aromatic hydrocarbons, and improve the yield of aromatic hydrocarbons. The modified nickel molecular sieve catalyst can catalytically treat common polyolefin waste plastics in life, and the catalytic process directly mixes the polyolefin waste plastics with the modified nickel molecular sieve catalyst and places them in a catalytic cracking reactor for the reaction, the reaction temperature is low (within 300°C), the conditions are mild, and no stirring and reaction solvent are required, the process is simple and easy, and the cost is low. DETAILED DESCRIPTION

[0037] In the following embodiments:

[0038] The melt index of low-density polyethylene (LDPE) is 25 g / 10 min (190 ° C / 2.16 kg);

[0039] The melt index of high-density polyethylene (HDPE) is 6 to 9 g / 10 min (190°C / 2.16 kg);

[0040] ZSM-5 (silicon-aluminum ratio of 38, 130, 300) and HY were purchased from Tianjin Nanhua Catalyst Co., Ltd. (NKC).

[0041] Example 1

[0042] 0g, 0.125g, 0.25g, 0.5g, 0.75g of nickel nitrate hexahydrate were added to 10ml of deionized water and magnetically stirred for 60min; 1g of ZSM-5 molecular sieve with a Si / Al molar ratio of 130:1 was calcined at 500℃ for 4h in a muffle furnace, and then added to nickel nitrate hexahydrate solution and magnetically stirred for 30min at a speed of 300rpm, and then aged at 67℃ for 3h, and then dried at 120℃ for 15h. The dried catalyst was reduced with hydrogen in a tubular furnace at a reduction temperature of 450℃, a reduction time of 3h, and a hydrogen flow rate of 100ml / min. After the reduction, the catalyst was passivated at room temperature in a tubular furnace. The passivation atmosphere was a mixed gas of 98% nitrogen and 2% oxygen. The passivation gas flow rate was 50 ml / min and the passivation time was 30 min. After the passivation, five different modified nickel molecular sieve catalysts were obtained and were respectively recorded as 1#, 2#, 3#, 4# and 5# modified catalysts.

[0043] 1.6 g of low-density polyethylene (LDPE) was added as the waste plastic raw material for the reaction into a catalytic cracking reactor, and 0.2 g of the modified catalyst (1#, 2#, 3#, 4#, 5#) prepared above was added. After mixing evenly, the mixture was reacted at 280°C for 60 min under a nitrogen atmosphere (partial pressure of 2 MPa).

[0044] Analysis of reaction products of waste plastics catalyzed by different catalysts:

[0045] After the reaction, the product was condensed, and the non-condensable gas product was collected by using an air bag. The condensed liquid product was extracted by 5 ml of dichloromethane solution and separated from the solid product and catalyst by centrifugation. The specific components of the liquid product were analyzed by liquid chromatography, and the selectivity of aromatics therein was determined by normalization. The solid product and catalyst after centrifugation were dried in an oven at 60°C for 12 hours and then weighed to obtain the mass of the solid product.

[0046] Before the reaction starts, the initial total mass of the waste plastics and catalyst added to the catalytic cracking reactor is recorded as m1; after the reaction is completed, the total mass of the catalytic cracking reactor and its internal reactants and catalyst is recorded as m2, and the mass of the gas products (including condensable gas products and non-condensable gas products) is m1-m2; the mass of the liquid product is the mass of the waste plastics minus the mass of the gas products and the solid products.

[0047] Wherein, waste plastic conversion rate = (initial waste plastic mass - solid product mass after reaction) * 100% / initial waste plastic mass;

[0048] Liquid product yield = mass of liquid product * 100% / initial waste plastic mass;

[0049] Aromatic hydrocarbon yield = mass of aromatic hydrocarbons in liquid phase product * 100% / mass of initial waste plastic.

[0050] The analytical calculation results of the reaction products are shown in Table 1:

[0051] Table 1 Analysis results of waste plastic products catalyzed by molecular sieves with different nickel loadings

[0052]

[0053] It can be seen from Table 1 that when the nickel-modified ZSM-5 catalyst (2~5#) catalyzes waste plastics, the waste plastic conversion rate, liquid phase product yield and aromatic hydrocarbon yield are significantly better than the waste plastic conversion rate, liquid phase product yield and aromatic hydrocarbon yield when pure ZSM-5 is used as a catalyst to catalyze waste plastics. And when the mass ratio of nickel salt (nickel nitrate hexahydrate) to ZSM-5 is 0.25:1 (3# modified catalyst), the waste plastic conversion rate, liquid phase product yield and aromatic hydrocarbon yield are all optimal.

[0054] Example 2

[0055] 0.25g of nickel nitrate hexahydrate was added to 10ml of deionized water and magnetically stirred for 60min; 1g of ZSM-5 molecular sieve with a molar ratio of Si / Al of 130:1 was calcined at 500℃ for 4h in a muffle furnace, and after calcination, it was added to the nickel nitrate hexahydrate solution and magnetically stirred for 30min at a speed of 300rpm, and then aged at 67℃ for 3h, and then dried at 120℃ for 15h. The dried catalyst was hydrogen reduced in a tubular furnace, the reduction temperature was 450℃, the reduction time was 3h, and the hydrogen flow rate was 100ml / min. The catalyst after reduction was passivated at room temperature in a tubular furnace, the passivation atmosphere was a mixed gas composed of 98% nitrogen and 2% oxygen, the passivation gas flow rate was 50ml / min, and the passivation time was 30min. After passivation, the modified nickel molecular sieve catalyst was obtained.

[0056] Four portions of 1.6 g of low-density polyethylene (LDPE) were taken as waste plastic raw materials for the reaction and added into four catalytic cracking reactors respectively, and 0.2 g of the prepared modified catalyst was added respectively. After mixing evenly, the mixture was reacted at 260°C, 270°C, 280°C and 300°C for 60 min respectively under a nitrogen atmosphere (partial pressure of 2 MPa).

[0057] The products at different catalytic reaction temperatures were analyzed using the analysis process of the reaction products in Example 1. The results are shown in Table 2.

[0058] Table 2 Analysis results of waste plastic products catalyzed by modified nickel molecular sieve catalyst at different catalytic reaction temperatures

[0059]

[0060] It can be seen from Table 2 that with the gradual increase of the catalytic reaction temperature, the conversion rate of waste plastics, the yield of liquid products and the yield of aromatics are significantly improved. However, when the reaction temperature reaches 280°C, the conversion rate of waste plastics, the yield of liquid products and the yield of aromatics are basically unchanged when the temperature is further increased, and the increase in reaction temperature increases energy consumption. Therefore, 280°C is selected as the optimal catalytic reaction temperature.

[0061] Example 3

[0062] 0.25g of nickel nitrate hexahydrate was added to 10ml of deionized water and magnetically stirred for 60min; 1g of ZSM-5 molecular sieve (the molar ratio of Si / Al was 38:1, 130:1 and 300:1 respectively) was calcined at 500℃ in a muffle furnace for 4h, and then added to the nickel nitrate hexahydrate solution and magnetically stirred for 30min at a speed of 300rpm, and then aged at 67℃ for 3h, and then dried at 120℃ for 15h. The dried catalyst was hydrogen reduced in a tubular furnace at a reduction temperature of 450℃, a reduction time of 3h, and a hydrogen flow rate of 100ml / min. The catalyst after reduction was passivated at room temperature in a tubular furnace, and the passivation atmosphere was a mixed gas composed of 98% nitrogen and 2% oxygen, the passivation gas flow rate was 50ml / min, and the passivation time was 30min. After passivation, three different modified nickel molecular sieve catalysts were obtained, and they were respectively recorded as 6#, 7#, and 8# modified catalysts.

[0063] 1.6 g of low-density polyethylene (LDPE) was added as the waste plastic raw material for the reaction into a catalytic cracking reactor, and 0.2 g of the prepared modified catalyst (6#, 7#, 8#) was added. After mixing evenly, the mixture was reacted at 280°C for 60 min under a nitrogen atmosphere (partial pressure of 2 MPa).

[0064] The products at different catalytic reaction temperatures were analyzed using the analysis process of the reaction products in Example 1. The results are shown in Table 3.

[0065] Table 3 Analysis results of waste plastic products catalyzed by modified catalysts of ZSN-5 carrier with different silicon-aluminum ratios

[0066]

[0067] It can be seen from Table 3 that when the modified catalysts (8#, 6#) prepared with the silicon-aluminum ratio of the ZSN-5 carrier being too large (300) or too small (38) are used to catalyze the decomposition of waste plastics, the waste plastic conversion rate, liquid product yield and aromatics yield are significantly worse than those of the modified catalyst 7# prepared when the silicon-aluminum ratio is 130; it can be seen that when the silicon-aluminum ratio is 130, the prepared modified catalyst has the optimal waste plastic conversion rate, liquid product yield and aromatics yield when catalyzing the decomposition of waste plastics.

[0068] Example 4

[0069] 0.25g of nickel nitrate hexahydrate was added to 10ml of deionized water and magnetically stirred for 60min; 1g of HY molecular sieve was calcined at 500℃ in a muffle furnace for 4h, and after calcination, it was added to the nickel nitrate hexahydrate solution and magnetically stirred for 30min at a speed of 300rpm, and then aged at 67℃ for 3h, and then dried at 120℃ for 15h. The dried catalyst was reduced with hydrogen in a tubular furnace, the reduction temperature was 450℃, the reduction time was 3h, and the hydrogen flow rate was 100ml / min. The catalyst after reduction was passivated at room temperature in a tubular furnace, the passivation atmosphere was a mixed gas composed of 98% nitrogen and 2% oxygen, the passivation gas flow rate was 50ml / min, and the passivation time was 30min. After passivation, the modified nickel molecular sieve catalyst (5Ni / HY) was obtained.

[0070] 1.6 g of low-density polyethylene (LDPE) was added as the waste plastic raw material to the catalytic cracking reactor, and 0.2 g of the modified catalyst (5Ni / HY) prepared above was added. After mixing evenly, the mixture was reacted at 280° C. for 60 min under a nitrogen atmosphere (partial pressure of 2 MPa).

[0071] The reaction products were analyzed using the analysis process of the reaction products in Example 1, wherein the waste plastic conversion rate, liquid product yield, and aromatics yield were 76.25%, 34.38%, and 18.22%, respectively.

[0072] Example 5

[0073] 0.25g of nickel nitrate hexahydrate was added to 10ml of deionized water and magnetically stirred for 60min; 1g of ZSM-5 molecular sieve with a molar ratio of Si / Al of 130:1 was calcined at 500℃ for 4h in a muffle furnace, and after calcination, it was added to the nickel nitrate hexahydrate solution and magnetically stirred for 30min at a speed of 300rpm, and then aged at 67℃ for 3h, and then dried at 120℃ for 15h. The dried catalyst was reduced with hydrogen in a tube furnace, the reduction temperature was 450℃, the reduction time was 3h, and the hydrogen flow rate was 100ml / min. The catalyst after reduction was passivated at room temperature in a tube furnace, the passivation atmosphere was a mixed gas composed of 98% nitrogen and 2% oxygen, the passivation gas flow rate was 50ml / min, and the passivation time was 30min. After passivation, a modified nickel molecular sieve catalyst (5Ni / ZSM-5(130)) was obtained.

[0074] 1.6 g of high-density polyethylene (HDPE) was taken as the waste plastic raw material for the reaction and added into the catalytic cracking reactor, and 0.2 g of the prepared modified catalyst (5Ni / ZSM-5(130)) was added. After mixing evenly, the mixture was reacted at 280°C for 60 min under a nitrogen atmosphere (partial pressure of 2 MPa).

[0075] The reaction products were analyzed using the analysis process of the reaction products in Example 1, wherein the waste plastic conversion rate, liquid product yield, and aromatics yield were 91.25%, 64.38%, and 30.12%, respectively.

[0076] Modified catalyst reusability performance test:

[0077] Catalyst preparation

[0078] 0.25g of nickel nitrate hexahydrate was added to 10ml of deionized water and magnetically stirred for 60min; 1g of ZSM-5 molecular sieve with a molar ratio of Si / Al of 130:1 was calcined at 500℃ for 4h in a muffle furnace, and after calcination, it was added to the nickel nitrate hexahydrate solution and magnetically stirred for 30min at a speed of 300rpm, and then aged at 67℃ for 3h, and then dried at 120℃ for 15h. The dried catalyst was reduced with hydrogen in a tubular furnace, the reduction temperature was 450℃, the reduction time was 3h, and the hydrogen flow rate was 100ml / min. The catalyst after reduction was passivated at room temperature in a tubular furnace, the passivation atmosphere was a mixed gas composed of 98% nitrogen and 2% oxygen, the passivation gas flow rate was 50ml / min, and the passivation time was 30min. After passivation, a modified nickel molecular sieve catalyst (catalyst R0) was obtained.

[0079] Catalytic reaction of waste plastics

[0080] 1.6 g of low-density polyethylene (LDPE) was added as the waste plastic raw material to the catalytic cracking reactor, and 0.2 g of the prepared modified catalyst (5Ni / ZSM-5(130)) was added. After mixing evenly, the mixture was reacted at 280°C for 60 min under a nitrogen atmosphere (partial pressure of 2 MPa).

[0081] After the reaction is completed, the reaction product is analyzed with reference to the analysis process of the reaction product in Example 1; then the solid product is calcined at 500° C. in a muffle furnace for 4 h to obtain the used catalyst, which is subjected to hydrogen reduction (reduction temperature is 450° C., reduction time is 3 h, hydrogen flow rate is 100 ml / min) and passivation at room temperature (passivation gas is a mixed gas composed of 98% nitrogen and 2% oxygen, passivation gas flow rate is 50 ml / min, passivation time is 30 min) to obtain the 5Ni / ZSM-5 (130) catalyst after the first use, which is recorded as catalyst R1. Then, according to the above-mentioned waste plastic catalytic reaction process, the waste plastic is catalyzed by catalyst R1, and the reaction product is analyzed by the analysis process of the reaction product in Example 1; the above operation is repeated to obtain the analysis results of the reaction products of the waste plastic catalyzed by catalysts R2 and R3 after the second and third uses, respectively, and the results are shown in Table 4.

[0082] Table 4 Analysis results of waste plastic products catalyzed by catalysts with different reuse times

[0083]

[0084] It can be seen from Table 4 that after being reused three times, the waste plastic conversion rate, liquid phase product yield and aromatic hydrocarbon yield of the catalytic decomposition of waste plastics by the modified catalyst still have high waste plastic conversion rate, liquid phase product yield and aromatic hydrocarbon yield. Compared with the newly prepared catalyst R0, only the liquid phase product yield is slightly decreased, while the waste plastic conversion rate and aromatic hydrocarbon yield are basically unchanged; This shows that the modified nickel molecular sieve catalyst prepared by the present invention has excellent reusability.

Claims

1. A method for preparing a modified nickel molecular sieve catalyst, characterized in that: The following steps are involved: (1) placing the molecular sieve carrier in a muffle furnace for calcination and activation, then immersing it in a nickel salt solution, mixing it evenly, aging it, and drying it to obtain an intermediate product; (2) The intermediate product is placed in a tubular furnace and sequentially subjected to hydrogen reduction and nitrogen and oxygen mixed gas passivation to obtain a modified nickel molecular sieve catalyst.

2. The method for preparing a modified nickel molecular sieve catalyst according to claim 1, characterized in that: The molecular sieve carrier is one or more of ZSM-5, HY, β, SAPO-34, and MOR; The mass ratio of the molecular sieve carrier to the nickel salt is 1:(0.1-1).

3. The method for preparing the modified nickel molecular sieve catalyst according to claim 1, characterized in that: The calcination temperature of the molecular sieve carrier is 400-600° C., and the calcination time is 2-6 hours.

4. The method for preparing the modified nickel molecular sieve catalyst according to claim 1, characterized in that: The nickel salt solution is prepared by dissolving nickel nitrate hexahydrate in deionized water, wherein the concentration of nickel nitrate hexahydrate is 10-80 g / L.

5. The method for preparing the modified nickel molecular sieve catalyst according to claim 1, characterized in that: The aging temperature is 50-70°C and the aging time is 2-4h; The drying temperature is 100-150°C and the drying time is 10-20 hours.

6. The method for preparing a modified nickel molecular sieve catalyst according to claim 1, characterized in that: The temperature of hydrogen reduction is 300-500°C and the time is 2-5h; The hydrogen flow rate is 50-200 mL / min.

7. The method for preparing a modified nickel molecular sieve catalyst according to claim 1, characterized in that: In the mixed gas, the volume ratio of nitrogen to oxygen is 98:2, and the flow rate of the mixed gas is 20~ 70mL / min; Passivation at room temperature, passivation time is 20 to 40 minutes.

8. A modified nickel molecular sieve catalyst, characterized in that: The modified nickel molecular sieve catalyst is prepared by the preparation method of any one of claims 1 to 7.

9. A low temperature treatment method for polyolefin waste plastics, characterized in that: The polyolefin waste plastic and the catalyst are uniformly mixed and placed in a catalytic cracking reactor for catalytic reaction. After the reaction is completed, the mixture is condensed and centrifuged to obtain a liquid product rich in aromatics. The catalyst is the modified nickel molecular sieve catalyst described in claim 8.

10. The low temperature treatment method for polyolefin waste plastics according to claim 9, characterized in that: The mass ratio of the catalyst to the polyolefin waste plastic is 1:(1-10); The catalytic reaction temperature is 260-300°C, and the reaction time is 0.5-24h; The catalytic reaction is carried out in a nitrogen atmosphere with a nitrogen pressure of 1-4 MPa.

Citation Information

Patent Citations

  • Composite catalyst for catalytic pyrolysis preparation of aromatic hydrocarbon and preparation method of composite catalyst

    CN103920526A

  • Method for preparing aromatic hydrocarbon and hydrogen-rich fuel gas through catalytic thermal conversion of polyolefin waste plastics

    CN110819372A

  • Method for depolymerizing lignin to phenol by using bifunctional catalyst through one-step method

    CN111217679A

  • Process for converting waste plastic into liquid gases, fuels, and waxes by catalytic cracking

    US20180371327A1

Cited By