Catalyst for epoxidation of bicyclic diene compound and preparation method and application thereof
By using a peroxypolytungstate quaternary ammonium salt catalyst in combination with a carrier, the rate and selectivity of the epoxidation reaction of bicyclic diene compounds are improved, solving the problems of low conversion rate and poor selectivity in the existing technology, and achieving efficient Aliphatic diepoxy compounds are produced and reduce production costs.
Patent Information
- Application Number
- CN202410756479.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-12
AI Technical Summary
In the prior art, the conversion rate and selectivity of aliphatic diepoxy compounds produced by epoxidation of bicyclic diene compounds are low, resulting in high production costs and poor product performance.
Peroxypolytungstate quaternary ammonium salts are used as catalysts, including A3[PW4O24], A2[SeW2O14], A3[AsW4O24] and A3[(OH)SiW3O18] and other types of peroxypolytungstate quaternary ammonium salts, combined with carriers such as Diatomaceous earth, zeolite, activated carbon and silica gel are used in the epoxidation reaction of bicyclic diene compounds to improve the reaction rate, conversion rate and selectivity.
The reaction rate, conversion rate and selectivity of the epoxidation of bicyclic diene compounds to produce aliphatic diepoxy compounds are significantly improved. The conversion rate can reach more than 95% and the selectivity can reach more than 99.8%. The catalyst is easy to recycle and reduces the cost. production costs.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of catalytic chemistry, and in particular to a catalyst for epoxidation of bicyclic diene compounds and a preparation method and application thereof. Background Art
[0002] Aliphatic diepoxides are a type of epoxy resin developed by Union Carbide Corporation of the United States. Compared with bisphenol A epoxy resins, they have good thermal stability, high weather resistance, and excellent electrical insulation properties. Therefore, aliphatic diepoxides are widely used in coatings, packaging, electronics, automobiles and other fields, and there is a large demand for them in the world.
[0003] Aliphatic diepoxides prepared by epoxidation of bicyclic diene compounds have good properties. Currently, the industry mostly adopts the organic peroxyacid method to epoxidize bicyclic diene compounds to prepare aliphatic diepoxides, but it has disadvantages such as low conversion rate and poor selectivity.
[0004] Based on this, there is a need to improve the conversion rate and selectivity of epoxidation of bicyclic diene compounds to prepare aliphatic diepoxides. Summary of the invention
[0005] The present application provides a catalyst for the epoxidation of bicyclic diene compounds, a preparation method and an application thereof, aiming to improve the reaction rate, conversion rate and selectivity of the epoxidation of bicyclic diene compounds to produce aliphatic diepoxide compounds.
[0006] In a first aspect, the present application provides a catalyst for the epoxidation of a bicyclic diene compound, the catalyst comprising a quaternary ammonium peroxypolytungstate salt, the quaternary ammonium peroxypolytungstate salt being selected from A3[PW4O 24 ]、A2[SeW2O 14 ]、A3[AsW4O 24 ]、A3[(OH)SiW3O 18 ] and A2[SW2O 14 ] one or more of them,
[0007] Here, A is an organic quaternary ammonium salt cation having 8 to 24 carbon atoms.
[0008] According to the present application, a catalyst including a quaternary ammonium peroxide polytungstate is provided, which can be used for the epoxidation of bicyclic diene compounds to produce aliphatic diepoxides, has high catalytic activity, can obtain aliphatic diepoxides with high specificity and selectivity, and can significantly improve the reaction rate, conversion rate and selectivity of the epoxidation of bicyclic diene compounds to produce aliphatic diepoxides, the conversion rate can reach more than 95%, and the selectivity can reach more than 99.8%; in addition, the catalyst is easy to recover and can be reused, thereby saving production costs.
[0009] In some embodiments of the present application, A is an organic quaternary ammonium salt cation having 16 to 21 carbon atoms.
[0010] In some embodiments of the present application, A is [C 18 H 37 N(CH3)3] + or [C 16 H 36 N] + .
[0011] In some embodiments of the present application, the peroxypolytungstate quaternary ammonium salt is selected from [C 18 H 37 N(CH3)3]3[PW4O 24 ]、[C 18 H 37 N(CH3)3]2[SeW2O 14 ] 、[C 18 H 37 N(CH3)3]3[AsW4O 24 ] 、 [C 18 H 37 N(CH3)3]3[(OH)SiW3O 18 ] and [C 16 H 36 N]2[SW2O 14 ] one or more of the following.
[0012] In some embodiments of the present application, the catalyst further comprises a carrier, and the peroxypolytungstate quaternary ammonium salt is loaded on the carrier;
[0013] Optionally, the carrier is selected from one or more of metal oxides, diatomaceous earth, zeolite, activated carbon and silica gel.
[0014] In a second aspect, the present application provides a use of the catalyst according to any embodiment of the first aspect in the preparation of aliphatic diepoxides.
[0015] According to the present application, the use of the catalyst described in any embodiment of the first aspect for preparing aliphatic diepoxides has a high reaction rate, conversion rate and selectivity, and recycling the catalyst can reduce production costs.
[0016] In a third aspect, the present application provides a method for preparing 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, comprising the following steps:
[0017] In the presence of a catalytic amount of the catalyst according to any embodiment of the first aspect, 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester and an oxidant are subjected to epoxidation reaction in an organic solvent to obtain 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate.
[0018] According to the present application, the catalyst described in any embodiment of the first aspect is used to catalyze the epoxidation of 3-cyclohexenecarboxylic acid-3'-cyclohexene methyl ester to produce 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate. It can be understood that the method for preparing 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate has the beneficial effects of the first aspect, that is, it has a higher reaction rate, conversion rate and selectivity, and recycling the catalyst can reduce production costs.
[0019] In some embodiments of the present application, the following steps are specifically included:
[0020] S1: dissolving and dispersing 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester and the catalyst according to any embodiment of the first aspect in an organic solvent to obtain a mixed solution;
[0021] S2: at a preset reaction temperature, an oxidant is added dropwise to the mixed solution to cause 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to undergo epoxidation reaction to obtain 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate.
[0022] In some embodiments of the present application, the mass ratio of the 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to the catalyst is 1:0.01 to 0.5.
[0023] In some embodiments of the present application, the molar ratio of the 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to the oxidant is 1:1-5.
[0024] In some embodiments of the present application, the organic solvent is selected from one or more of ethyl acetate, ethylene dichloride, tert-butanol, 1,4-dioxane, and acetonitrile; and / or the oxidant is hydrogen peroxide and / or peracetic acid.
[0025] In some embodiments of the present application, the step S1 further includes dispersing a dehydrating agent in an organic solvent.
[0026] In some embodiments of the present application, in step S2, the preset reaction temperature is 20-70°C. DETAILED DESCRIPTION
[0027] The various embodiments or implementation schemes in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments.
[0028] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the implementation or examples are included in at least one implementation or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same implementation or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more implementations or examples in a suitable manner.
[0029] In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present application, "room temperature" has a meaning well known in the art, generally referring to a temperature of "15°C to 35°C", unless otherwise clearly and specifically defined.
[0030] As described in the background art above, currently, bicyclic diene compounds are mostly used as raw materials in the industry to synthesize aliphatic diepoxides through an organic peroxyacid method, but this method has disadvantages such as low conversion rate and poor selectivity.
[0031] Based on this, the use of catalysts to efficiently catalyze the epoxidation reaction of bicyclic diene compounds is considered to be an effective way to improve the reaction rate, conversion rate and selectivity. Therefore, the inventors have found through a large number of experiments that the use of catalysts containing a specific type of quaternary ammonium peroxypolytungstate can effectively improve the reaction rate, conversion rate and selectivity of the epoxidation of bicyclic diene compounds to produce aliphatic diepoxides.
[0032] It should be noted that, unless otherwise specified, the conversion rate described in the context of this application refers to the conversion rate of the bicyclic diene compound, which can be calculated by the following formula: conversion rate = m / (n*M), wherein m represents the mass of the actual product, n is the amount of the bicyclic diene compound in the raw material, and M is the molar mass of the bicyclic diene compound; the maximum conversion rate is 100%.
[0033] Unless otherwise specified, the selectivity described in the context of this application refers to the selectivity of the epoxidation reaction of the bicyclic diene compound, which can be obtained by calculating the mass fraction of the target aliphatic diepoxide compound in the actual product, and the highest selectivity is 100%. Since the bicyclic diene compound may generate other by-products (such as monoepoxides generated by incomplete epoxidation or ring-opening of epoxides, etc.) during the process of epoxidation of the bicyclic diene compound to produce the target aliphatic diepoxide compound, the actual product generally contains a certain amount of by-products, and the actual product can be qualitatively and quantitatively analyzed by gas chromatography and gas chromatography-mass spectrometry to calculate the mass fraction of the target aliphatic diepoxide compound in the actual product, which is the selectivity of the epoxidation reaction of the bicyclic diene compound.
[0034] The catalyst for epoxidation of bicyclic diene compounds and its application provided by the present application are described in detail below.
[0035] In a first aspect, the present application provides a catalyst for the epoxidation of a bicyclic diene compound, the catalyst comprising a quaternary ammonium peroxypolytungstate salt, the quaternary ammonium peroxypolytungstate salt being selected from A3[PW4O 24 ]、A2[SeW2O 14 ]、A3[AsW4O 24 ]、A3[(OH)SiW3O 18 ] and A2[SW2O 14 ] one or more of them,
[0036] Here, A is an organic quaternary ammonium salt cation having 8 to 24 carbon atoms.
[0037] According to the present application, the inventors have found through a large number of experiments that a specific type of peroxy polytungstate quaternary ammonium salt has a high catalytic activity for the epoxidation reaction of bicyclic diene compounds. In the peroxy polytungstate quaternary ammonium salt, the type of peroxy polytungstate anion and the type of organic quaternary ammonium salt cation have a certain influence on the catalytic activity of the peroxy polytungstate quaternary ammonium salt. Specifically, the inventors found that the peroxy polytungstate anion is [PW4O 24 ] 3- 、[SeW2O 14 ] 2- 、[AsW4O 24 ] 3- 、[(OH)SiW3O 18 ] 3- or [SW2O 14 ] 2-, and when the carbon number of the organic quaternary ammonium salt cation is 8 to 24, the peroxypolytungstate quaternary ammonium salt has extremely high catalytic activity for the epoxidation of bicyclic diene compounds. For example, the carbon number of the organic quaternary ammonium salt can be 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24.
[0038] Therefore, when the catalyst containing the above-mentioned type of peroxy polytungstate quaternary ammonium salt is used for the epoxidation of bicyclic diene compounds to produce aliphatic diepoxide compounds, it has the following beneficial effects due to its good catalytic activity:
[0039] (1) It can effectively increase the epoxidation reaction rate and improve production efficiency; in addition, a lower reaction temperature can be used, thereby improving safety and saving production costs.
[0040] (2) It is possible to use an oxidant with relatively stable properties and slightly weak oxidizing power to epoxidize the bicyclic diene compound. For example, low-concentration hydrogen peroxide can be used as an oxidant. It is stable in nature and green and environmentally friendly, and can effectively avoid the use of organic peroxides (such as organic peroxyacids) in traditional processes. On the one hand, organic peroxyacids are prone to explosion and will also produce a large amount of acidic waste liquid, causing corrosion of the reaction equipment. In addition, under acidic conditions, the target product aliphatic diepoxy compounds are prone to acidic ring opening to generate by-products such as aliphatic monoepoxy compounds. At the same time, the by-products are difficult to separate from the target product, resulting in a decrease in the selectivity of the reaction; in addition, in order to avoid the influence of acidic waste liquid, a large amount of inorganic compounds need to be added to the system, which will produce a large amount of saline wastewater, polluting the environment and increasing production costs. Therefore, the use of the above catalyst can avoid the use of organic peroxides, thereby effectively overcoming the above problems.
[0041] (3) It can effectively improve the conversion rate and selectivity of the reaction system. Experiments have shown that under appropriate reaction conditions, the conversion rate and selectivity of the epoxidation of bicyclic diene compounds to produce 2, aliphatic diepoxide compounds can reach more than 95% and more than 99.8%, respectively, which can effectively reduce production costs.
[0042] (4) The above catalyst is easy to recover in the reaction system and has good catalytic stability, and can be recycled multiple times, thereby further reducing production costs.
[0043] In some embodiments of the present application, A is an organic quaternary ammonium salt cation having 16 to 21 carbon atoms.
[0044] In some of the above embodiments, as described above, the number of carbon atoms in the organic quaternary ammonium salt cation of peroxypolytungstate quaternary ammonium salt has a certain influence on its catalytic activity. Through a large number of experiments, it is found that under the same conditions, when the number of carbon atoms in the organic quaternary ammonium salt cation is between 16 and 21, the catalytic activity of peroxypolytungstate quaternary ammonium salt is better.
[0045] In some embodiments of the present application, A is [C 18 H 37 N(CH3)3] + or [C 16 H 36 N] + .
[0046] In some of the above embodiments, the inventors further found through a large number of experiments that the catalytic activity of the quaternary ammonium peroxypolytungstate is not only related to the number of C atoms in the organic quaternary ammonium salt cation, but also to the specific structure of the organic quaternary ammonium salt cation. Under the same conditions, when the organic quaternary ammonium salt cation is [C 18 H 37 N(CH3)3] + or [C 16 H 36 N] + When the catalytic activity of quaternary ammonium peroxypolytungstate is better.
[0047] In some embodiments of the present application, the quaternary ammonium peroxypolytungstate salt is selected from [C 18 H 37 N(CH3)3]3[PW4O 24 ] 、[C 18 H 37 N(CH3)3]2[SeW2O 14 ] 、[C 18 H 37 N(CH3)3]3[AsW4O 24 ] 、 [C 18 H 37 N(CH3)3]3[(OH)SiW3O 18 ] and [C 16 H 36 N]2[SW2O 14 ] one or more of the following.
[0048] In some of the above embodiments, several quaternary ammonium peroxide polytungstate salts with high catalytic activity are specifically listed. When the catalyst containing the above quaternary ammonium peroxide polytungstate salt is used for the epoxidation of bicyclic olefin compounds to produce 2,3-epoxypinane, it has a high reaction rate, conversion rate and selectivity.
[0049] In some embodiments of the present application, the catalyst further comprises a carrier, and the quaternary ammonium peroxypolytungstate salt is loaded on the carrier;
[0050] Optionally, the carrier is selected from one or more of diatomaceous earth, zeolite, activated carbon and silica gel.
[0051] In some of the above embodiments, the catalyst may further include a carrier, and the peroxy polytungstate quaternary ammonium salt is loaded on the carrier. It is understandable that the peroxy polytungstate quaternary ammonium salt can be directly added to the reaction system as a catalyst for use, and further, it can also be loaded on a carrier. When added to the reaction system as a catalyst, the carrier can serve as the skeleton of the peroxy polytungstate quaternary ammonium salt, which can be stably dispersed, thereby increasing its catalytic activity and catalytic stability. In addition, loading it on a carrier is also more convenient for recycling, thereby reducing production costs.
[0052] Furthermore, the carrier can be selected from one or more of diatomaceous earth, zeolite, activated carbon and silica gel. It is understood that the carrier can stably load the peroxypolytungstate quaternary ammonium salt and does not react with the raw materials and products in the reaction system. Those skilled in the art can make a selection according to actual conditions.
[0053] In some embodiments of the present application, A3[PW4O 24 ] can be prepared by the following method:
[0054] Concentrated hydrochloric acid is added to sodium tungstate, and then hydrogen peroxide is added to react, and then phosphoric acid is added to react to obtain a mixed solution; a soluble quaternary ammonium salt containing A is added to the mixed solution to obtain A3[PW4O 24 The A3[PW4O 24 ] has a higher yield.
[0055] In some embodiments of the present application, A2[SeW2O 14 ] can be prepared by the following method:
[0056] After hydrogen peroxide is added to tungstic acid for reaction, selenic acid is added for reaction to obtain a mixed solution; a soluble quaternary ammonium salt containing A is added to the mixed solution to obtain A2[SeW2O 14 The A2[SeW2O 14 ] has a higher yield.
[0057] In some embodiments of the present application, A3[AsW4O 24 ] can be prepared by the following method:
[0058] Concentrated hydrochloric acid is added to sodium tungstate, and then hydrogen peroxide is added to react, and then disodium hydrogen arsenate is added to react to obtain a mixed solution; a soluble quaternary ammonium salt containing A is added to the mixed solution to obtain A3[AsW4O 24]. The A3[AsW4O 24 ] has a higher yield.
[0059] In some embodiments of the present application, A3[(OH)SiW3O 18 ] can be prepared by the following method:
[0060] To K8[γ-SiW 10 O 36 ] is added with hydrogen peroxide to obtain a mixed solution; a soluble quaternary ammonium salt containing A is added to the mixed solution to obtain A3[(OH)SiW3O 18 ]. A3[(OH)SiW3O 18 ] has a higher yield.
[0061] In some embodiments of the present application, A2[SW2O 14 ] can be prepared by the following method:
[0062] After adding hydrogen peroxide to tungstic acid for reaction, sulfuric acid is added for reaction to obtain a mixed solution; a soluble quaternary ammonium salt containing A is added to the mixed solution to obtain A2[SW2O 14 ]. The A2[SW2O 14 ] has a higher yield.
[0063] It is understandable that A3[PW4O 24 ]、A2[SeW2O 14 ]、A3[AsW4O 24 ]、A3[(OH)SiW3O 18 ] and A2[SW2O 14 ] including but not limited to being prepared by the above method.
[0064] In some embodiments of the present application, the bicyclic diene compound is 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester or dicyclopentadiene.
[0065] In a second aspect, the present application provides a use of the catalyst according to any embodiment of the first aspect in the preparation of aliphatic diepoxides.
[0066] According to the present application, the use of the catalyst described in any embodiment of the first aspect for preparing aliphatic diepoxides has a high reaction rate, conversion rate and selectivity, and recycling the catalyst can reduce production costs.
[0067] In some embodiments of the present application, the catalyst described in any embodiment of the first aspect can be used to catalyze the preparation of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate from 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester.
[0068] In some embodiments of the present application, the catalyst described in any embodiment of the first aspect can be used to catalyze the preparation of dicyclopentadiene dioxide from dicyclopentadiene.
[0069] In a second aspect, the present application provides a method for preparing 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, comprising the following steps:
[0070] In the presence of a catalytic amount of the catalyst according to any embodiment of the first aspect, 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester and an oxidant are subjected to epoxidation reaction in an organic solvent to obtain 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate.
[0071] According to the present application, the catalyst described in any embodiment of the first aspect is used to catalyze the epoxidation of 3-cyclohexenecarboxylic acid-3'-cyclohexene methyl ester to produce 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate. It can be understood that the method for preparing 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate has the beneficial effects of the first aspect, that is, it has a higher reaction rate, conversion rate and selectivity, and recycling the catalyst can reduce production costs.
[0072] In some embodiments of the present application, the method specifically comprises the following steps:
[0073] S1: dissolving and dispersing 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester and the catalyst according to any embodiment of the first aspect in an organic solvent to obtain a mixed solution;
[0074] S2: at a preset reaction temperature, an oxidant is added dropwise to the mixed solution to cause 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to undergo epoxidation reaction to obtain 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate.
[0075] In some of the above embodiments, the steps of preparing 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexyl carboxylate are specifically defined, in which 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester and the catalyst according to any embodiment of the first aspect are dissolved and dispersed in an organic solvent in step S1, and the oxidant is not directly mixed, and in step S2, 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester is subjected to epoxidation reaction by dripping the oxidant. The advantage of this method is that a large amount of oxidant can be avoided from accumulating in the reaction system, thereby avoiding potential safety hazards; the dripping of the oxidant can also improve the conversion rate and selectivity of the reaction, saving production costs.
[0076] It is worth mentioning that the use of the catalyst according to any embodiment of the first aspect has a higher catalytic activity. Therefore, despite the use of the method of dripping the oxidant, the system can still be guaranteed to have a faster reaction rate, which is also a beneficial effect brought about by the use of the above catalyst.
[0077] In some embodiments of the present application, the mass ratio of 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to the catalyst is 1:0.01 to 0.5. For example, the mass ratio of 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to the catalyst can be 1:0.01, 1:0.02, 1:0.05, 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5 or within the range of any of the above values.
[0078] In some of the above embodiments, the mass ratio of 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to the catalyst is specifically defined. Since the above catalyst has a high catalytic activity, a small amount of catalyst can effectively improve the reaction rate, conversion rate and selectivity of the reaction system. Too high a catalyst content will lead to increased production costs. Therefore, the mass ratio of 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to the catalyst can be controlled in the range of 1:0.01 to 0.5.
[0079] In some embodiments of the present application, the molar ratio of 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to the oxidant is 1:1 to 5. For example, the molar ratio of 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to the oxidant is 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5 or any range thereof.
[0080] In some of the above embodiments, the molar ratio of 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to the oxidant is specifically defined. In order to improve the conversion rate of 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester, the oxidant can be appropriately excessive in the reaction system. However, if the content of the oxidant is too much, it may lead to an increase in the by-products of the reaction. At the same time, the excess oxidant may also cause certain safety hazards. Therefore, the molar ratio of 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to the oxidant can be controlled in the range of 1:1 to 5.
[0081] In some embodiments of the present application, the organic solvent is selected from one or more of ethyl acetate, ethylene dichloride, tert-butanol, 1,4-dioxane, and acetonitrile; and / or the oxidant is hydrogen peroxide and / or peracetic acid.
[0082] In some of the above embodiments, several commonly used organic solvents are specifically listed, and the epoxidation reaction of 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester is carried out in an organic solvent. It is understandable that it is miscible with 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester and does not react with the components in the reaction system. Those skilled in the art can choose according to actual needs. As an example, in some embodiments, 1,4-dioxane is used as an organic solvent.
[0083] The types of oxidants are also specifically listed. Hydrogen peroxide and peracetic acid are commonly used oxidants in the epoxidation reaction of 3-cyclohexenecarboxylic acid-3'-cyclohexene methyl ester. Since the above catalyst has good reactivity, hydrogen peroxide with weaker oxidizing property can be used as an oxidant. In some embodiments, the oxidant is hydrogen peroxide with a mass concentration of 15% to 35%. As an example, hydrogen peroxide with a mass concentration of 27.5% is used as the oxidant.
[0084] In some embodiments of the present application, the step S1 further includes dispersing a dehydrating agent in an organic solvent.
[0085] In some of the above embodiments, the reaction system may further include a dehydrating agent. Since both 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester and 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate contain ester groups and undergo hydrolysis reactions, the dehydrating agent can combine with the water in hydrogen peroxide and the water generated by hydrogen peroxide reduction, thereby reducing the hydrolysis of 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester and 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, thereby further improving the conversion rate and selectivity of the present method.
[0086] In some embodiments, the dehydrating agent may include but is not limited to acetic anhydride and anhydrous sodium sulfate. It is understandable that those skilled in the art may also select a dehydrating agent known in the art according to the above reaction system.
[0087] In some embodiments of the present application, the preset reaction temperature is 20-70° C. For example, the preset reaction temperature can be 20° C., 25° C., 30° C., 35° C., 40° C., 45° C., 50° C., 55° C., 60° C., 65° C., 70° C. or any range thereof.
[0088] In some of the above embodiments, the reaction temperature of the epoxidation reaction of 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester is specifically defined. It is understandable that too high or too low a temperature will affect the reaction time, conversion rate and selectivity. The inventors have found through a large number of experiments that under the conditions of using the above catalyst, when the preset reaction temperature is 20 to 70° C., the conversion rate and selectivity are higher. As an example, the preset reaction temperature is 60° C.
[0089] In some embodiments of the present application, the time for adding the oxidant dropwise is 1 to 5 hours.
[0090] In some of the above embodiments, the time for dropping the oxidant is specifically defined. It can be understood that the time for dropping the oxidant has a certain relationship with the preset reaction temperature. The higher the preset reaction temperature, the time for dropping the oxidant should be reduced accordingly. The lower the preset reaction temperature, the time for dropping the oxidant should be increased accordingly. Experiments have found that when the preset reaction temperature is 20 to 70°C, the time for dropping the oxidant can be controlled at 1 to 5 hours. As an example, the time for dropping the oxidant is 3 hours.
[0091] In some embodiments of the present application, step S2 also includes, after the epoxidation reaction of 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester, cooling to room temperature, collecting the organic phase by separation, extracting the aqueous phase with ethyl acetate, filtering to recover the catalyst, collecting the ethyl acetate phase by separation again, mixing the organic phase and the ethyl acetate phase and rotary evaporating to obtain 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate.
[0092] Example
[0093] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0094] Example 1
[0095] [C 18 H 37 N(CH3)3]3[PW4O 24 Preparation of ]:
[0096] Add 66g (0.2mol) of Na2WO4·2H2O to a 2500mL flask with a stirrer, a thermometer and a condenser, dissolve it with 400mL of deionized water, and after the solution is clarified, add 40g (200mmol) of concentrated HCl to form a light yellow precipitate immediately. Then add 170g of 30% H2O2 to form a peroxypolytungstate solution. Cool to room temperature, add 5.76g (50mmol) of 85% phosphoric acid, stir and react at room temperature for 1h, add 200mL of tert-butanol solution containing 52.2g of octadecyltrimethylammonium chloride (150mmol), stir the solution at room temperature for 30min, collect the white precipitate by filtration, and then wash it with excess deionized water and ether. Drain the precipitate. Wash the crude product with excess deionized water and anhydrous ethanol, and vacuum dry overnight to obtain [C18 H 37 N(CH3)3]3[PW4O 24 ]100.5g, yield 96.3%.
[0097] Example 2
[0098] Preparation of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate:
[0099] Take a clean 2500mL beaker and weigh [C 18 H 37 N(CH3)3]3[PW4O 24 ]6.26g (3mmol), 4g (28mmol) disodium hydrogen phosphate were placed in a beaker, 500mL solvent 1,4-dioxane and 330g (1.5mol) 3-cyclohexenecarboxylic acid-3'-cyclohexene methyl ester were added to the beaker, the system was stirred at 60°C for 15min, and then 185g of 27.5% hydrogen peroxide (1.5mol) was added dropwise to the solution to react for 3h. After the reaction was completed, the system was cooled to room temperature, the organic phase was separated and collected, the aqueous phase was extracted with ethyl acetate, the catalyst was collected by filtration, the ethyl acetate phase was separated and collected again, the organic phase and the ethyl acetate phase were mixed and evaporated to obtain 334g of product, with a conversion rate of 95.1%.
[0100] Example 3
[0101] [C 18 H 37 N(CH3)3]2[SeW2O 14 Preparation of ]:
[0102] Add 50.0g (0.2mol) H2WO4 and 700mL 27.5% H2O2 to a 2500mL three-necked flask, stir on a 60℃ water bath until a colorless clear solution is obtained, filter while hot, cool to room temperature, and then add 4 times 80% H2SeO4 (4.2mL, 56mmol). After stirring and reacting at room temperature for 1h, add 200mL tert-butanol solution containing 69.6g octadecyltrimethylammonium chloride (200mmol), stir the solution at room temperature for 30min, collect the white precipitate by filtration, and then wash with excess deionized water and ether. Drain the precipitate. Wash the crude product with excess deionized water and anhydrous ethanol, and vacuum dry overnight to obtain [C 18 H 37 N(CH3)3]2[SeW2O 14 ]122.3g, yield 94.2%.
[0103] Example 4
[0104] Preparation of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate:
[0105] Take a clean 2500mL beaker and weigh [C 18 H 37 N(CH3)3]2[SeW2O 14 ]3.98g (3mmol), 4g (28mmol) disodium hydrogen phosphate were placed in a beaker, 500mL solvent 1,4-dioxane and 238mL (1.5mol) 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester were added to the beaker, the system was stirred at 60°C for 15min, and then 185g of 27.5% hydrogen peroxide (1.5mol) was added dropwise to the solution, and the reaction was continued for 3h. After the reaction was completed, the system was cooled to room temperature, the organic phase was separated and collected, the aqueous phase was extracted with ethyl acetate, the catalyst was collected by filtration, the ethyl acetate phase was separated and collected again, the organic phase and the ethyl acetate phase were mixed and evaporated, and 223g of the product was obtained, and the conversion rate was 97.4%.
[0106] Example 5
[0107] [C 18 H 37 N(CH3)3]3[AsW4O 24 Preparation of ]:
[0108] Add 66g (0.2mol) of Na2WO4·2H2O to a 2500mL flask with a stirrer, a thermometer and a condenser, dissolve it with 400mL of deionized water, and after the solution is clarified, add 40g (200mmol) of concentrated HC1, and a light yellow precipitate is immediately generated. Then, add 170g of 30% H2O2 to generate a peroxypolytungstate solution, cool to room temperature, and then add 4 times Na2H[AsO4]·7H2O aqueous solution (40mL, 15.6g, 50mmol). After stirring and reacting at room temperature for 1h, add 200mL of tert-butanol solution containing 52.2g of octadecyltrimethylammonium chloride (100mmol), stir the solution at room temperature for 30min, collect the white precipitate by filtration, and then wash it with excess deionized water and ether. Drain the precipitate. Wash the crude product with excess deionized water and anhydrous ethanol, and vacuum dry overnight to obtain the catalyst [C 18 H 37 N(CH3)3]3[AsW4O 24 ]98.6g, yield 92.5%.
[0109] Example 6
[0110] Preparation of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate:
[0111] Take a clean 2500mL beaker and weigh [C 18 H 37 N(CH3)3]3[AsW4O 24 ]6.4g (3mmol), 4g (28mmol) disodium hydrogen phosphate were placed in a beaker, 500mL solvent 1,4-dioxane and 238ml (1.5mol) 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester were added to the beaker, the system was stirred at 60°C for 15min, and then 185g of 27.5% hydrogen peroxide (1.5mol) was added dropwise to the solution, and the reaction was continued for 3h. After the reaction was completed, the system was cooled to room temperature, the organic phase was separated and collected, the aqueous phase was extracted with ethyl acetate, the catalyst was collected by filtration, the ethyl acetate phase was separated and collected again, the organic phase and the ethyl acetate phase were mixed and evaporated, and 219g of the product was obtained, and the conversion rate was 95.9%.
[0112] Example 7
[0113] [C 18 H 37 N(CH3)3]3[(OH)SiW3O 18 Preparation of ]:
[0114] K8[γ-SiW 10 O 36 ]·12H2O (25 g, 8.5 mmol), dissolved in 480 mL 30% H2O2, after the solution is clarified, the solution is stirred at room temperature for 4 h. Octadecyltrimethylammonium chloride (29.6 g, 85 mmol) is dissolved in 200 mL tert-butyl alcohol, and the mixed solution is vigorously stirred at 45 ° C for 4 h. A white flocculent suspension appears, which is filtered, and the white precipitate is collected by filtration, and then washed with excess deionized water and ether. The precipitate is drained. The crude product is washed with excess deionized water and anhydrous ethanol, and vacuum dried overnight to obtain [C 18 H 37 N(CH3)3]3[(OH)SiW3O 18 ]49.6g, yield 96.1%.
[0115] Example 8
[0116] Preparation of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate:
[0117] Take a clean 2500mL beaker and weigh [C 18 H 37 N(CH3)3]3[(OH)SiW3O 18]5.5g (3mmol), 4g (28mmol) disodium hydrogen phosphate were placed in a beaker, 500mL solvent 1,4-dioxane and 238mL (1.5mol) 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester were added to the beaker, the system was stirred at 60°C for 15min, and then 185g of 27.5% hydrogen peroxide (1.5mol) was added dropwise to the solution, and the reaction was continued for 3h. After the reaction was completed, the system was cooled to room temperature, the organic phase was separated and collected, the aqueous phase was extracted with ethyl acetate, the catalyst was collected by filtration, the ethyl acetate phase was separated and collected again, the organic phase and the ethyl acetate phase were mixed and evaporated, and 215.3g of the product was obtained, and the conversion rate was 94.3%.
[0118] Example 9
[0119] [C 16 H 36 N]2[SW2O 14 Preparation of ]:
[0120] Add 50.0g (0.2mol) H2WO4 and 700mL 27.5% H2O2 to a 2500mL three-necked flask, stir on a 60℃ water bath until a colorless clear solution is obtained, filter while hot, cool to room temperature, and then add 2mol / L H2SO4 aqueous solution (8mL, 70mmol). After stirring and reacting at room temperature for 1h, add 200mL tert-butanol solution containing tetrabutylammonium hydrogen sulfate (67.9g, 200mmol), stir the solution at room temperature for 30min, collect the light yellow precipitate by filtration, and then wash with excess deionized water and ether. Drain the precipitate. Wash the crude product with excess deionized water and anhydrous ethanol, and vacuum dry overnight to obtain [C 16 H 36 N]2[SW2O 14 ]98.6g, yield 88.9%.
[0121] Example 10
[0122] Preparation of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate:
[0123] Take a clean 2500mL beaker and weigh [C 18 H 37 N(CH3)3]3[(OH)SiW3O 18]3.33g (3mmol), 4g (28mmol) disodium hydrogen phosphate were placed in a beaker, 500mL solvent 1,4-dioxane and 238mL (1.5mol) 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester were added to the beaker, the system was stirred at 60°C for 15min, and then 185g of 27.5% hydrogen peroxide (1.5mol) was added dropwise to the solution, and the reaction was continued for 3h. After the reaction was completed, the system was cooled to room temperature, the organic phase was separated and collected, the aqueous phase was extracted with ethyl acetate, the catalyst was collected by filtration, the ethyl acetate phase was separated and collected again, the organic phase and the ethyl acetate phase were mixed and evaporated, and 221.9g of the product was obtained, and the conversion rate was 97.2%.
[0124] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A catalyst for the epoxidation of a bicyclic diene compound, characterized in that: The catalyst comprises a quaternary ammonium peroxide polytungstate salt, wherein the quaternary ammonium peroxide polytungstate salt is selected from A3[PW4 24 ]、A2[SeW2O 14 ]、A3[AsW4O 24 ]、A3[(OH)SiW3O 18 ] and A2[SW2O 14 ] one or more of them, Here, A is an organic quaternary ammonium salt cation having 8 to 24 carbon atoms.
2. The catalyst according to claim 1, characterized in that A is an organic quaternary ammonium salt cation having 16 to 21 carbon atoms; Optionally, the A is [C 18 H 37 N(CH3)3] + or [C 16 H 36 N] + ; Optionally, the peroxypolytungstate quaternary ammonium salt is selected from [C 18 H 37 N(CH3)3]3[PW4O 24 ]、[C 18 H 37 N(CH3)3]2[SeW2O 14 ]、[C 18 H 37 N(CH3)3]3[AsW4O 24 ]、[C 18 H 37 N(CH3)3]3[(OH)SiW3O 18 ] and [C 16 H 36 N]2[SW2O 14 ] one or more; Optionally, the catalyst further comprises a carrier, and the peroxypolytungstate quaternary ammonium salt is loaded on the carrier; Optionally, the carrier is selected from one or more of metal oxides, diatomaceous earth, zeolite, activated carbon and silica gel.
3. Use of the catalyst according to claim 1 or 2 in the preparation of aliphatic diepoxides.
4. A method for preparing 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, characterized in that: The following steps are involved: In the presence of a catalytic amount of the catalyst according to claim 1 or 2, 3-cyclohexenecarboxylic acid-3'-cyclohexenylmethyl ester and an oxidant are subjected to epoxidation reaction in an organic solvent to obtain 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate.
5. The method according to claim 4, characterized in that The specific steps include: S1: dissolving and dispersing 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester and the catalyst according to claim 1 or 2 in an organic solvent to obtain a mixed solution; S2: at a preset reaction temperature, an oxidant is added dropwise to the mixed solution to cause 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to undergo epoxidation reaction to obtain 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate.
6. The method according to claim 4 or 5, characterized in that: The mass ratio of the 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to the catalyst is 1:0.01-0.
5.
7. The method according to claim 4 or 5, characterized in that: The molar ratio of the 3-cyclohexenecarboxylic acid-3'-cyclohexenemethyl ester to the oxidant is 1:1-5.
8. The method according to claim 4 or 5, characterized in that: The organic solvent is selected from one or more of ethyl acetate, ethylene dichloride, tert-butyl alcohol, 1,4-dioxane, and acetonitrile; and / or The oxidant is hydrogen peroxide and / or peracetic acid.
9. The method according to claim 5, characterized in that The step S1 also includes dispersing a dehydrating agent in an organic solvent.
10. The method according to claim 5, characterized in that In the step S2, the preset reaction temperature is 20-70°C.
Citation Information
Patent Citations
Catalytic preparation method of dicyclopentadiene dioxide by quaternary ammonium heteropoly phosphato tungstate
CN101704824A
Ultra-deep oxidation desulphurization catalyst
CN102380423A
Nitrogen-containing heterocyclic compound and method for producing same
CN102844302A
Phase-transfer catalytic synthesis method of 3, 4-epoxy cyclohexyl methyl-3', 4'-epoxy cyclohexyl formate
CN113880790A
Method for producing substituted amino-6-methylpyridine-n-oxide derivative
IN201748027279A