G-C3N4 / ZnIn2S4 hollow tubular flower-shaped photocatalyst with photocatalytic performance as well as preparation method and application of g-C3N4 / ZnIn2S4 hollow tubular flower-shaped photocatalyst
By combining g-C3N4 with ZnIn2S4 hollow tubes, a nanotube structure with improved photocatalytic properties was prepared, which solved the problem of poor photoelectron transmission performance of pure g-C3N4 and achieved efficient CO2 reduction and pollutant degradation, and the catalyst Easy to recycle.
Patent Information
- Application Number
- CN202410751767.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-01
AI Technical Summary
The practical application of pure graphite-carbon nitride (g-C3N4) in photocatalysis is limited by its poor photoelectron transmission performance and high photogenerated charge recombination rate, resulting in its poor performance in pollutant degradation and CO2 reduction.
By combining with ZnIn2S4 hollow tubes, g-C3N4/ZnIn2S4 hollow tube flower-shaped photocatalysts were prepared. Urea and melamine were used as raw materials, calcined in a muffle furnace and reacted at high temperature, and then centrifuged and washed in deionized water. and drying, forming nanotube structures with improved photocatalytic properties.
The catalyst shows excellent CO2 reduction performance under visible light irradiation, with a CO production rate as high as 204.63 μmol/g, and can effectively degrade antibiotics and dyes, with a degradation performance of 98% to 92%, and has a stable structure and is easy to recycle.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photocatalysis, and in particular relates to a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance, a preparation method and an application thereof. Background Art
[0003] Photocatalysis has been applied to environmental pollutant treatment and energy conversion, and has attracted great attention in recent decades. In 1972, the discovery of semiconductor photocatalytic processes under solar irradiation opened up a promising method for water pollution treatment. After decades of scientific research, the technology of photocatalytic degradation of water pollutants has flourished. Some studies have also shown that photocatalytic reduction of carbon dioxide (CO2) is a promising solution for reducing atmospheric carbon dioxide to form hydrocarbon fuels to alleviate energy shortages, and the photocatalyst is recyclable and will not cause secondary pollution. Therefore, photocatalytic technology has received widespread attention. Graphite-carbon nitride (g-C3N4), as a photocatalytic material with broad application prospects, has attracted widespread attention from researchers around the world for its suitable band structure, non-toxicity, low cost, and good stability. The conduction band edge of g-C3N4 is -1.13 eV compared with NHE, which is negative enough to provide strong redox reaction ability, and it has aroused great interest due to its large specific surface area, strong adsorption capacity and unique photoelectric properties. Therefore, g-C3N4 is an ideal catalyst for pollutant degradation and CO2 reduction. However, the practical application of pure g-C3N4 in photocatalysis is severely limited by its poor photoelectron transport performance and high photogenerated charge recombination rate. Therefore, modifying pure g-C3N4 to make it a good photocatalyst has become a research focus. Summary of the invention
[0004] The purpose of the embodiments of the present invention is to provide a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance and a preparation method and application thereof, aiming to solve the problems existing in the prior art pointed out in the background technology.
[0005] The embodiment of the present invention is implemented as follows: a method for preparing a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance comprises the following steps: urea and melamine are evenly mixed, calcined in a muffle furnace and then dispersed in deionized water, TAA, ZnCl2, and InCl3 are added in sequence, the product obtained after high-temperature reaction is centrifuged, washed, and dried to obtain a g-C3N4 / ZnIn2S4 hollow tube flower-shaped catalyst.
[0006] As another preferred embodiment of the present invention, the mass ratio of urea to melamine is (100-1200): (20-100). The mass ratio of TAA, ZnCl2, and InCl3 is (150-450): (100-450): (200-600). The mass of g-C3N4 is (50-300).
[0007] As another preferred embodiment of the present invention, when preparing the g-C3N4 sample, urea and melamine are placed in a muffle furnace, heated to 300 ~ 600 ° C at a heating rate of 5 ° C / min, and calcined in air at this temperature for 2 ~ 6h.
[0008] As another preferred embodiment of the present invention, during the drying process, the substrate is placed in a vacuum drying oven at 50-70° C. for 10-18 h, and during the washing operation, deionized water and ethanol are used for washing.
[0009] As another preferred embodiment of the present invention, when the sample is dispersed in deionized water, the deionized water is 100 mL, and the pH is adjusted to 1-4.
[0010] As another preferred embodiment of the present invention, the oil bath reaction temperature is 60-100° C., and the reaction time is 1-4 h.
[0011] As another preferred embodiment of the present invention, the zinc chloride is anhydrous zinc chloride, and the indium chloride is anhydrous indium chloride.
[0012] Another object of an embodiment of the present invention is to provide a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance prepared by the above method.
[0013] As another preferred embodiment of the present invention, the length of the g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst is 3 μm to 6 μm.
[0014] As another preferred embodiment of the present invention, the g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst is a nanotube with stable structure and good dispersion performance. Under the irradiation of visible light, it has good CO2 reduction performance and can also degrade antibiotics and dyes.
[0015] The g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst of the present invention has the characteristics of stable structure, good dispersibility and large specific surface area, which is conducive to separating and transmitting photogenerated electrons between interfaces and inhibiting the recombination of photogenerated electron-hole pairs; the preparation method of the present invention is simple and low in cost, and the prepared g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst has excellent performance of photocatalytic reduction of CO2 to produce CO under the irradiation of visible light, and the yield of CO is as high as 204.63 μmol / g within 2 h of illumination. It can also effectively degrade antibiotics such as norfloxacin (NFX), oxytetracycline (OTC), levofloxacin hydrochloride (LEF), dye reactive red 2 (RR2), methyl orange (MO), etc., and the degradation performance reaches 98% to 92% within 60 minutes. In addition, the g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst of the present invention is also easy to recycle and easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 is the XRD spectrum of g-C3N4 / ZnIn2S4 nanotube catalyst; Figure 2 is the CO yield diagram of g-C3N4 / ZnIn2S4 nanotube catalyst; Figure 3 It is a bar graph of the degradation performance of g-C3N4 / ZnIn2S4 nanotube catalyst; Figure 4 It is the degradation performance cycle diagram of g-C3N4 / ZnIn2S4 nanotube catalyst; Figure 5 This is the SEM image of g-C3N4 / ZnIn2S4 nanotube catalyst. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0018] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments. Example
[0019] This embodiment provides a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance, and a preparation method thereof, comprising the following steps: (1) Weigh 10 g urea and 1 g melamine in an agate mortar, grind thoroughly, transfer to a large crucible and place in a muffle furnace for high-temperature calcination at 600 °C, heating rate 5 °C / min, and keep warm for 4 h. After cooling to room temperature, a light yellow solid powder is obtained, which is ground again to obtain a hollow tubular g-C3N4 sample.
[0020] (2) Take 100 mg of hollow tubular g-C3N4 and disperse it evenly in 100 mL of deionized water, adjust the pH value to 2.0, and add 300 mg of TAA, 270 mg of ZnCl2 and 440 mg of InCl3 in sequence after continuous stirring. After continued stirring, transfer it to a round-bottom flask and react it in an oil bath at 75 °C for 1.5 h, and stir continuously during this period. The obtained product was centrifuged, washed with deionized water and ethanol, and vacuum dried at 70 °C for 10 h to obtain a g-C3N4 / ZnIn2S4 hollow tubular flower-shaped composite sample. Example
[0021] This embodiment provides a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance, and a preparation method thereof, comprising the following steps: (1) Weigh 5 g of urea and 0.5 g of melamine in an agate mortar, grind thoroughly, transfer to a large crucible and place in a muffle furnace for high-temperature calcination at 500 °C, heating rate 5 °C / min, and keep warm for 3 h. After cooling to room temperature, a light yellow solid powder is obtained, which is ground again to obtain a hollow tubular g-C3N4 sample.
[0022] (2) Take 200 mg of hollow tubular g-C3N4 and evenly disperse it in 100 mL of deionized water, adjust the pH value to 1, and add 150 mg of TAA, 135 mg of ZnCl2 and 220 mg of InCl3 in sequence after continuous stirring. After continued stirring, transfer it to a round-bottom flask and react it in an oil bath at 90 °C for 1.5 h, and stir continuously during this period. The obtained product was centrifuged, washed with deionized water and ethanol, and vacuum dried at 50 °C for 17 h to obtain a g-C3N4 / ZnIn2S4 hollow tubular flower-shaped composite sample. Example
[0023] This embodiment provides a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance, and a preparation method thereof, comprising the following steps: (1) Weigh 7 g urea and 0.5 g melamine into an agate mortar, grind thoroughly, transfer to a large crucible and place in a muffle furnace for high-temperature calcination at 300 °C, heating rate 5 °C / min, and keep warm for 6 h. After cooling to room temperature, a light yellow solid powder is obtained, which is ground again to obtain a hollow tubular g-C3N4 sample.
[0024] (2) Take 175 mg of hollow tubular g-C3N4 and disperse it evenly in 100 mL of deionized water, adjust the pH value to 2.5, and add 200 mg TAA, 180 mg ZnCl2 and 300 mg InCl3 in sequence after continuous stirring. After continued stirring, transfer it to a round-bottom flask and react it in an oil bath at 60 °C for 2.5 h, and stir continuously during this period. The obtained product was centrifuged, washed with deionized water and ethanol, and vacuum dried at 55 °C for 15 h to obtain a g-C3N4 / ZnIn2S4 hollow tubular flower-shaped composite sample. Example
[0025] This embodiment provides a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance, and a preparation method thereof, comprising the following steps: (1) Weigh 10 g urea and 1 g melamine into an agate mortar, grind thoroughly, transfer to a large crucible and place in a muffle furnace for high-temperature calcination at 400 °C, heating rate 5 °C / min, and keep warm for 5 h. After cooling to room temperature, a light yellow solid powder is obtained, which is ground again to obtain a hollow tubular g-C3N4 sample.
[0026] (2) Take 150 mg of hollow tubular g-C3N4 and disperse it evenly in 100 mL of deionized water, adjust the pH value to 4, add 350 mg of TAA, 320 mg of ZnCl2 and 510 mg of InCl3 in sequence after continuous stirring, continue stirring, transfer to a round-bottom flask and react in an oil bath at 100 °C for 1 h, and stir continuously during this period. The obtained product was centrifuged, washed with deionized water and ethanol, and vacuum dried at 65 °C for 11 h to obtain a g-C3N4 / ZnIn2S4 hollow tubular flower-shaped composite sample. Example
[0027] This embodiment provides a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance, and a preparation method thereof, comprising the following steps: (1) Weigh 9 g urea and 0.4 g melamine in an agate mortar, grind thoroughly, transfer to a large crucible and place in a muffle furnace for high-temperature calcination at 350 °C, heating rate 5 °C / min, and keep warm for 6 h. After cooling to room temperature, a light yellow solid powder is obtained, which is ground again to obtain a hollow tubular g-C3N4 sample.
[0028] (2) Take 180 mg of hollow tubular g-C3N4 and disperse it evenly in 100 mL of deionized water, adjust the pH value to 3.5, and add 250 mg of TAA, 220 mg of ZnCl2 and 370 mg of InCl3 in sequence after continuous stirring. After continued stirring, transfer it to a round-bottom flask and react it in an oil bath at 75 °C for 2.5 h, and stir it continuously during this period. The obtained product was centrifuged, washed with deionized water and ethanol, and vacuum dried at 70 °C for 16 h to obtain a g-C3N4 / ZnIn2S4 hollow tubular flower-shaped composite sample. Example
[0029] This embodiment provides a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance, and a preparation method thereof, comprising the following steps: (1) Weigh 4 g urea and 0.7 g melamine in an agate mortar, grind thoroughly, transfer to a large crucible and place in a muffle furnace for high-temperature calcination at 600 °C, heating rate 5 °C / min, and keep warm for 2 h. After cooling to room temperature, a light yellow solid powder is obtained, which is ground again to obtain a hollow tubular g-C3N4 sample.
[0030] (2) Take 200 mg of hollow tubular g-C3N4 and evenly disperse it in 100 mL of deionized water, adjust the pH value to 3.0, and add 350 mg of TAA, 310 mg of ZnCl2 and 500 mg of InCl3 in sequence after continuous stirring. After continued stirring, transfer it to a round-bottom flask and react it in an oil bath at 100 °C for 1.5 h, and stir continuously during this period. The obtained product was centrifuged, washed with deionized water and ethanol, and vacuum dried at 55 °C for 10 h to obtain a g-C3N4 / ZnIn2S4 hollow tubular flower-shaped composite sample. Example
[0031] This embodiment provides a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance, and a preparation method thereof, comprising the following steps: (1) Weigh 8 g of urea and 0.8 g of melamine into an agate mortar, grind thoroughly, transfer to a large crucible and place in a muffle furnace for high-temperature calcination at 500 °C, heating rate 5 °C / min, and keep warm for 3.5 h. After cooling to room temperature, a light yellow solid powder is obtained, which is ground again to obtain a hollow tubular g-C3N4 sample.
[0032] (2) Take 80 mg of hollow tubular g-C3N4 and disperse it evenly in 100 mL of deionized water, adjust the pH value to 1.5, and add 250 mg of TAA, 225 mg of ZnCl2, and 370 mg of InCl3 in sequence after continuous stirring. After continued stirring, transfer to a round-bottom flask and react in an oil bath at 60 °C for 3.5 h, and stir continuously during this period. The obtained product was centrifuged, washed with deionized water and ethanol, and vacuum dried at 60 °C for 14 h to obtain a g-C3N4 / ZnIn2S4 hollow tubular flower-shaped composite sample. Example
[0033] This embodiment provides a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance, and a preparation method thereof, comprising the following steps: (1) Weigh 1 g urea and 0.2 g melamine in an agate mortar, grind thoroughly, transfer to a large crucible and place in a muffle furnace for high-temperature calcination at 300 °C, heating rate 5 °C / min, and keep warm for 4.5 h. After cooling to room temperature, a light yellow solid powder is obtained, which is ground again to obtain a hollow tubular g-C3N4 sample.
[0034] (2) Take 240 mg of hollow tubular g-C3N4 and disperse it evenly in 100 mL of deionized water, adjust the pH value to 3.5, and add 200 mg of TAA, 180 mg of ZnCl2 and 300 mg of InCl3 in sequence after continuous stirring. After continued stirring, transfer it to a round-bottom flask and react it in an oil bath at 95 °C for 2.5 h, and stir continuously during this period. The obtained product was centrifuged, washed with deionized water and ethanol, and vacuum dried at 55 °C for 17 h to obtain a g-C3N4 / ZnIn2S4 hollow tubular flower-shaped composite sample. Example
[0035] This embodiment provides a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance, and a preparation method thereof, comprising the following steps: (1) Weigh 3.5 g urea and 0.3 g melamine in an agate mortar, grind thoroughly, transfer to a large crucible and place in a muffle furnace for high-temperature calcination at 450 °C, heating rate 5 °C / min, and keep warm for 4.5 h. After cooling to room temperature, a light yellow solid powder is obtained, which is ground again to obtain a hollow tubular g-C3N4 sample.
[0036] (2) Take 50 mg of hollow tubular g-C3N4 and disperse it evenly in 100 mL of deionized water, adjust the pH value to 4.0, and add 260 mg of TAA, 230 mg of ZnCl2 and 380 mg of InCl3 in sequence after continuous stirring. After continued stirring, transfer it to a round-bottom flask and react it in an oil bath at 95 °C for 2.5 h, and stir it continuously during this period. The obtained product was centrifuged, washed with deionized water and ethanol, and vacuum dried at 60 °C for 12 h to obtain a g-C3N4 / ZnIn2S4 hollow tubular flower-shaped composite sample. Example
[0037] This embodiment provides a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance, and a preparation method thereof, comprising the following steps: (1) Weigh 5 g of urea and 0.6 g of melamine in an agate mortar, grind thoroughly for 1 h, transfer to a large crucible and place in a muffle furnace for high-temperature calcination at 500 °C, heating rate 5 °C / min, and keep warm for 4 h. After cooling to room temperature, a light yellow solid powder is obtained, which is ground again to obtain a hollow tubular g-C3N4 sample.
[0038] (2) Take 260 mg of hollow tubular g-C3N4 and disperse it evenly in 100 mL of deionized water, adjust the pH value to 1.5, and add 300 mg of TAA, 270 mg of ZnCl2 and 440 mg of InCl3 in sequence after continuous stirring. After continued stirring, transfer it to a round-bottom flask and react it in an oil bath at 80 °C for 2 h, and stir it continuously during this period. The obtained product was centrifuged, washed with deionized water and ethanol, and vacuum dried at 70 °C for 10 h to obtain a g-C3N4 / ZnIn2S4 hollow tubular flower-shaped composite sample. Figure 1 It can be seen that the prepared g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst was successfully synthesized, has good crystallinity, and no other impurities appear.
[0039] Figure 2 It can be seen that the yield of CO produced by the photocatalytic reduction of CO2 by the prepared g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst is 204.63 μmol / g.
[0040] Figure 3 It can be seen that the prepared g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst can effectively degrade NFX, OTC, LEF, RR2, and MO pollutants in water, with a degradation rate of 98%~92%.
[0041] Figure 4 It can be seen that the prepared g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst can still have good degradation performance and good stability after four cycles.
[0042] Figure 5 It can be seen that the morphology of the prepared g-C3N4 / ZnIn2S4 is a hollow tube flower.
[0043] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst, characterized in that: The method comprises the following steps: urea and melamine are uniformly mixed, calcined in a muffle furnace and then dispersed in deionized water, thioacetamide (TAA), zinc chloride (ZnCl2) and indium chloride (InCl3) are added in sequence, the product obtained after oil bath reaction is centrifuged, washed and dried to obtain a g-C3N4 / ZnIn2S4 hollow tube flower-shaped catalyst.
2. The method for preparing the g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance according to claim 1, characterized in that: The mass ratio of urea and melamine is (100-1200): (20-100). The mass ratio of TAA, ZnCl2, and InCl3 is (150-450): (100-450): (200-600). The mass of g-C3N4 is (50-300).
3. The method for preparing the g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance according to claim 1, characterized in that: When preparing g-C3N4 samples, urea and melamine were placed in a muffle furnace, heated to 300 ~ 600 °C at a heating rate of 5 °C / min, and calcined in air at this temperature for 2 ~ 6 h.
4. The method for preparing the g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance according to claim 1, characterized in that: During the drying process, the sample is placed in a vacuum drying oven at 50 to 70°C for 10 to 18 hours, and during the washing operation, deionized water and ethanol are used for washing.
5. The method for preparing the g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance according to claim 1, characterized in that: When the sample is dispersed in deionized water, the deionized water is 100 mL, and the pH is adjusted to 1-4.
6. The method for preparing the g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance according to claim 1, characterized in that: The oil bath reaction temperature is 60-100°C, and the reaction time is 1-4 h.
7. The method for preparing the g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance according to claim 1, characterized in that: The zinc chloride used is anhydrous zinc chloride, and the indium chloride used is anhydrous indium chloride.
8. A g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance prepared by the method according to any one of claims 1 to 7.
9. The g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance according to claim 8, characterized in that: The length of the g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst is 3 μm to 6 μm.
10. Use of the g-C3N4 / ZnIn2S4 hollow tube flower-shaped photocatalyst with photocatalytic performance as claimed in claim 8 or 9 in reducing CO2 and degrading antibiotics and dyes.
Citation Information
Patent Citations
Preparation method and application of sulfur-indium-zinc / graphite-phase carbon nitride graded hollow heterojunction
CN112221532A
Fish scale tubular carbon nitride composite heterojunction photocatalyst as well as preparation method and application thereof
CN112916035A
Ball-flower-shaped sulfur indium zinc / carbon nitride heterojunction photocatalyst and preparation method and application thereof
CN116726973A
Preparation and application of CdS / g-C3N4 nanotube catalyst with photocatalytic performance
CN117772256A
Cited By
Photocatalyst for degrading tetracycline and preparation method thereof
CN116809079A