Parylene coating for metal substrate surface and preparation method and application thereof
By using silicone or polyolefin skeleton coupling agent between the Perrylin layer and the metal substrate, the problem of difficult appearance and adhesion in the prior art is solved, and the high adhesion and corrosion-free Perry is achieved. Forest coating, suitable for protection of metal substrates.
Patent Information
- Application Number
- CN202411217165.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-02
AI Technical Summary
The existing coupling agents used between metal substrates and the parelin layer are difficult to meet the needs of appearance and adhesion at the same time and often lead to the generation of corrosive marks.
Using a coupling agent with a silicone polymer or polyolefin backbone, through which chemical bonds are formed between the parelin layer and the metal substrate, the molecular weight and mass ratio of the coupling agent are controlled to improve the adhesion of the parelin layer. And inhibit the generation of corrosion marks.
It achieves high adhesion and good appearance of the Perrelin coating on the surface of the metal substrate, while significantly inhibiting the generation of corrosive marks and meeting the protection needs of industrial applications.
Smart Images

Figure CN118719510B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of parylene materials, and in particular relates to a parylene coating for a metal substrate surface and a preparation method and application thereof. Background Art
[0002] Parylene can be divided into N-type, C-type, D-type, HT-type and other types according to different molecular structures. Parylene layer can provide various properties, such as protection performance, lubrication performance, barrier performance, insulation and withstand voltage performance. Parylene layer deposition usually adopts the process of vapor deposition, and the Parylene layer itself has a very strong water vapor barrier efficiency.
[0003] Parylene layer can be used as a protective layer for metal substrates. However, since parylene (polyparaxylene) itself is relatively symmetrical (with weak polarity), the adhesive force generated during the transformation from gas to solid is like liquid wax turning into solid wax. It has a little adhesive force, but the adhesive strength is difficult to be used for industrialization. In order to give full play to the protective effect of the parylene layer, it is necessary to improve the adhesion of the parylene layer on the metal substrate. Coupling agents can be used to improve the adhesion of the parylene layer on the metal substrate.
[0004] In order to bond with metals, coupling agents with carboxyl groups, phosphate groups, acrylates, and amine nitrogen can be used. However, when these substances are bonded with metals, they will cause a certain degree of corrosion to the metal itself, leaving corrosive marks on the metal surface, similar to water stains, etc., and the appearance of the parylene coating is difficult to meet customer needs.
[0005] Although the existing coupling agents such as A174 used for parylene coating can basically meet the appearance requirements of parylene coating, their adhesion to metal is relatively low.
[0006] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention
[0007] The purpose of the present invention is to overcome the defect that the existing coupling agent used between the metal substrate and the parylene layer is difficult to meet the requirements of appearance and adhesion at the same time, and to provide a parylene coating for the surface of a metal substrate and a preparation method and application thereof. The parylene coating has high adhesion on the surface of the metal substrate and can meet the requirements for appearance.
[0008] In order to achieve the above-mentioned object, in a first aspect, the present invention provides a parylene coating for a metal substrate surface, the parylene coating comprising a parylene layer and a coupling agent, the coupling agent being present between the parylene layer and the substrate to be plated, the coupling agent being chemically bonded to the parylene layer and the substrate to be plated, respectively, the mass of the coupling agent being 0.5%-13% of the mass of the parylene layer; the substrate to be plated is a metal substrate; the coupling agent has the following general formula: AMB;
[0009] Among them, A is selected from , , or ;
[0010] B is selected from a group containing a carboxyl group or ;
[0011] M is an organosilicon polymer skeleton or a polyolefin skeleton;
[0012] * indicates a connection key;
[0013] When the M is a silicone polymer skeleton, the molecular weight of the coupling agent is 750-2200; when the M is a polyolefin skeleton, the molecular weight of the coupling agent is 190-550.
[0014] In some preferred embodiments, the M is an organosilicon polymer backbone.
[0015] Preferably, the general formula of the organosilicon polymer skeleton is , where * represents the connecting key, a=1~7, b=1~4, c=0~3, d=0~18.
[0016] In some preferred embodiments, M is or , where * represents the connection key, n 1 =1~18, n=1~9.
[0017] In some preferred embodiments, the coupling agent is a carboxyl-organosilicon-vinyl coupling agent, a phosphoric acid-organosilicon-methacrylate coupling agent, a carboxymethyl-organosilicon-vinyl coupling agent, or a carboxymethyl-organosilicon-methacrylate coupling agent.
[0018] In some preferred embodiments, the mass of the coupling agent is 0.5%-10% of the mass of the parylene layer.
[0019] In a second aspect, the present invention provides a method for preparing a parylene coating, which is used to prepare the parylene coating described in the first aspect, and the preparation method sequentially comprises a first step or a second step, depositing a parylene layer;
[0020] The first step is to immerse the substrate to be plated in an organic solution containing a coupling agent and then dry it;
[0021] The second step is to put the coupling agent into the atomization chamber, volatilize the coupling agent in a vacuum heating environment, and make the volatilized coupling agent react on the surface of the substrate to be plated.
[0022] In some preferred embodiments, the preparation method comprises the first step and depositing a parylene layer in sequence.
[0023] Preferably, the coupling agent-containing organic solution is obtained by dissolving the coupling agent in an organic solvent, and the mass concentration of the coupling agent in the coupling agent-containing organic solution is 0.8wt%-6wt%;
[0024] and / or,
[0025] The soaking time is 10 min-180 min, and the drying conditions include: the drying temperature is 40° C.-80° C., and the time is 1 h-3 h.
[0026] In a third aspect, the present invention provides use of the parylene coating described in the first aspect or the parylene coating prepared by the preparation method of the parylene coating described in the second aspect in surface protection of a substrate to be plated, wherein the substrate to be plated is a metal substrate.
[0027] In the parylene coating of the present invention, a coupling agent exists between the parylene layer and the substrate to be plated, one end of the coupling agent has a carboxyl group or a phosphate group, which can enable the coupling agent to establish a good interaction with the metal, and one end has an allyl group, a vinyl group, a methacrylate group, an acrylate group, etc., which can establish a good interaction with the parylene layer, and an organic silicon polymer skeleton or a polyolefin skeleton is between the two end caps. The structures other than the carboxyl group in the organic silicon polymer skeleton or the polyolefin skeleton and the carboxyl group can play a role in diluting the concentration of the carboxyl or phosphate metal action end to a certain extent. When it is an organic silicon polymer, the molecular weight of the coupling agent is 750-2200, and when the skeleton is a polyolefin skeleton, the molecular weight of the coupling agent is 190-550, the mass of the metal active end such as the carboxyl group or the phosphate group relative to the mass of the coupling agent is within a certain range, and the mass of the coupling agent is 0.5%-13% of the mass of the parylene layer, which can simultaneously meet the requirements of the parylene coating on appearance and adhesion, and can significantly inhibit the generation of corrosive marks. When the parylene coating of the present invention is used for metal substrate protection, it can simultaneously meet the requirements of appearance and adhesion.
[0028] The parylene coating prepared by the preparation method of the present invention can meet the requirements of appearance and adhesion at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0030] Figure 1 The photograph is of a stainless steel substrate having the Parylene coating of Example 2 on its surface, which was stored at room temperature of 25° C. and humidity of 50% for one week after being taken out of the oven. DETAILED DESCRIPTION
[0031] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0032] The inventors of the present invention have found through research that the existing coupling agent used between the metal substrate and the parylene layer is difficult to simultaneously meet the requirements of the parylene coating for appearance and adhesion.
[0033] In this regard, in a first aspect, the present invention provides a parylene coating for a metal substrate surface, the parylene coating comprising a parylene layer and a coupling agent, the coupling agent being present between the parylene layer and the substrate to be plated, the coupling agent being chemically bonded to the parylene layer and the substrate to be plated, respectively, the mass of the coupling agent being 0.5%-13% of the mass of the parylene layer; the substrate to be plated is a metal substrate; the coupling agent has the following general formula: AMB;
[0034] Among them, A is selected from , , or ;
[0035] B is selected from a group containing a carboxyl group or ;
[0036] M is an organosilicon polymer skeleton or a polyolefin skeleton;
[0037] * indicates a connection key;
[0038] When the M is a silicone polymer skeleton, the molecular weight of the coupling agent is 750-2200; when the M is a polyolefin skeleton, the molecular weight of the coupling agent is 190-550.
[0039] The parylene coating of the present invention comprises a parylene layer, wherein a coupling agent exists between the parylene layer and the metal substrate, wherein the general formula of the coupling agent is AMB, wherein A is selected from an allyl group, a vinyl group, a methacrylate group, and an acrylate group, and the coupling agent can establish a good interaction force with the parylene layer through the free radical reaction between the A end and the parylene layer, wherein B is selected from a group containing a carboxyl group or a phosphate group, and the coupling agent can establish a good interaction force with the metal substrate through the interaction between the B end and the metal end, and M is an organic silicon polymer skeleton or a polyolefin skeleton, and the structures other than the carboxyl group in the organic silicon polymer skeleton or the polyolefin skeleton and the carboxyl group can play To a certain extent, the concentration of the carboxyl or phosphate metal active ends is diluted. On this basis, by controlling the following two aspects, the parylene coating can meet the requirements of appearance and adhesion at the same time, and significantly inhibit the generation of corrosive marks. The first aspect is that when the skeleton is a silicone polymer, the molecular weight of the coupling agent is 750-2200, and when the skeleton is a polyolefin skeleton, the molecular weight of the coupling agent is 190-550. The mass of the metal active ends such as carboxyl or phosphate groups relative to the mass of the coupling agent is within a certain range. The second aspect is that the mass of the coupling agent is 0.5%-13% of the mass of the parylene layer.
[0040] The inventors have found that if the molecular weight of the coupling agent is less than the above range, there will be a problem of imprinting, and if the molecular weight is greater than the above range, there will be a problem of too low bonding between the coupling agent and the parylene layer or the metal substrate. If the relative content of the coupling agent and the parylene layer is less than the above range or greater than the above range, there will be a problem of too low bonding between the parylene layer and the metal substrate. If the relative content of the coupling agent and the parylene layer is greater than the above range, there will be a problem of too low barrier performance of the overall parylene coating.
[0041] In some preferred embodiments of the present invention, M is an organosilicon polymer skeleton. In this preferred embodiment, M is an organosilicon polymer skeleton, and the organosilicon polymer skeleton has structural adjustability. The temperature resistance of the parylene coating can be adjusted by adjusting the structure of the organosilicon skeleton. When the organosilicon skeleton with a Q-type structure is used in conjunction with the C material or the F material, the temperature resistance can be increased. The original C material can only withstand a temperature of about 130 degrees. When used in conjunction, the temperature resistance can be increased to about 250 degrees, which is more conducive to the parylene layer to exert its protective performance at a higher temperature.
[0042] Further preferably, the general formula of the organosilicon polymer skeleton is , where * represents a connecting bond, a=1~7, b=1~4, c=0~3, d=0~18. In this preferred embodiment, the organic silicon polymer skeleton of the above general formula is adopted, where a=1~7, b=1~4, c=0~3, d=0~18, which is more conducive to balancing the appearance and adhesion of the parylene coating and matching the temperature resistance of various types of parylene layers, wherein in the general formula of the organic silicon polymer skeleton, all the groups directly connected to silicon are methyl groups. In this preferred embodiment, there are two * in the organic silicon polymer skeleton, which are connected to the A end and the B end respectively, and the present invention does not limit the specific connection positions of the A end and the B end.
[0043] In some preferred embodiments of the present invention, M is or , where * represents the connection key, n 1 = 1-18, n = 1~9. In this preferred embodiment, since there is no hydrolyzable group, when the parylene coating is prepared by the immersion method, the life of the prepared immersion solution is longer, which can reach two months. M is When n 1 =1-18, M is When n=1~9, it is more conducive to balancing the appearance and adhesion of the parylene coating.
[0044] In some preferred embodiments of the present invention, the coupling agent is a carboxyl-organic silicon-vinyl coupling agent, a phosphoric acid-organic silicon-methacrylate coupling agent, a carboxymethyl-organic silicon-vinyl coupling agent, or a carboxymethyl-organic silicon-methacrylate coupling agent. The preferred coupling agent is more conducive to improving the adhesion of the parylene layer on the metal substrate.
[0045] In some preferred embodiments of the present invention, the mass of the coupling agent is 0.5%-10% of the mass of the parylene layer. Under this preferred embodiment, when M is a silicone polymer skeleton and the molecular weight of the coupling agent is 750-2200, or when M is a polyolefin skeleton and the molecular weight of the coupling agent is 190-550, the mass of the coupling agent is 0.5%-10% of the mass of the parylene layer, which is more conducive to balancing the appearance and adhesion of the parylene coating.
[0046] The coupling agent of the present invention is applicable to any type of parylene layer, for example, C-type, N-type, F-type or HT-type parylene layer, etc., all of which can be used in the present invention.
[0047] In a second aspect, the present invention provides a method for preparing a parylene coating, which is used to prepare the parylene coating described in the first aspect, and the preparation method sequentially comprises a first step or a second step, depositing a parylene layer;
[0048] The first step is to immerse the substrate to be plated in an organic solution containing a coupling agent and then dry it;
[0049] The second step is to put the coupling agent into the atomization chamber, volatilize the coupling agent in a vacuum heating environment, and make the volatilized coupling agent react on the surface of the substrate to be plated.
[0050] The coupling agent of the present invention is applicable to a wide range of preparation processes, and can be applied to an immersion method, an atomization method, and the like.
[0051] In some preferred embodiments, the preparation method includes the first step and the deposition of a parylene layer in sequence. The coupling agent of the present invention contains an organosilicon polymer skeleton or a polyolefin skeleton. When the skeleton is an organosilicon polymer, the molecular weight of the coupling agent is 750-2200, and when the skeleton is a polyolefin skeleton, the molecular weight of the coupling agent is 190-550. The preparation of the parylene coating by the immersion method including the first step is more conducive to improving the uniformity of the coupling agent distribution, improving and uniformizing the adhesion of the parylene layer to the substrate to be plated, and exerting the insulation withstand voltage, lubrication and protection of the parylene layer.
[0052] In some preferred embodiments of the present invention, the organic solution containing the coupling agent is obtained by dissolving the coupling agent in an organic solvent.
[0053] The organic solvent may be, for example, at least one of isopropanol, ethanol, toluene, acetone, and butanone.
[0054] Preferably, the mass concentration of the coupling agent in the organic solution containing the coupling agent is 0.8wt%-6wt%, preferably 1wt%-4wt%. Under this preferred embodiment, it is more conducive to improving the uniformity of the coupling agent distribution, improving and uniformizing the adhesion of the parylene layer to the substrate to be plated, and balancing the appearance and adhesion of the parylene coating.
[0055] In the second aspect, the soaking time is shorter if the substrate has no pores, and longer if the substrate has many pores. In some preferred embodiments of the present invention, the soaking time is 10 min to 180 min.
[0056] Preferably, the drying conditions include: a drying temperature of 40° C.-80° C. and a drying time of 1 h-3 h.
[0057] In the second aspect, the deposition amount ratio of the parylene layer to the coupling agent layer can be adjusted within a suitable range by controlling the feeding amounts of the coupling agent and parylene.
[0058] In the second aspect of the present invention, the process of CVD deposition of the parylene layer can be carried out with reference to the prior art. For example, the deposition of the parylene layer is generally divided into three temperature zones: the first temperature zone is called the evaporation zone, and the temperature is generally controlled at 130°C-180°C; the second temperature zone is called the cracking zone, and the temperature is controlled at 680°C-730°C; the third temperature zone is called the deposition zone, and the temperature is controlled at 20°C-30°C. The deposition rate in the deposition zone is 0.6-2.4 μm / hour.
[0059] In a third aspect, the present invention provides use of the parylene coating described in the first aspect or the parylene coating prepared by the preparation method of the parylene coating described in the second aspect in surface protection of a substrate to be plated, wherein the substrate to be plated is a metal substrate.
[0060] In some preferred embodiments of the present invention, the metal is stainless steel, aluminum alloy, etc.
[0061] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0062] Example 1
[0063] The coupling agent is a carboxyl-organic silicon-vinyl coupling agent. The preparation method of the coupling agent is as follows: 50 g of triethoxysilyl valeric acid (synthesized by the synthesis method in "Stable carboxylic acid derivatized alkoxy silanes", Chem. Commun., 2015, 51, 2339-2341), 39.4 g of tetraethyl orthosilicate (Sinopharm Chemical Reagent Co., Ltd.), 92.1 g of hexamethyldisiloxane (Sinopharm Chemical Reagent Co., Ltd.), 36 g of vinyl triethoxysilane (Sinopharm Chemical Reagent Co., Ltd.), 4 g of acetic acid (Sinopharm Chemical Reagent Co., Ltd.), 45 g of deionized water and 200 g of isopropanol (Sinopharm Chemical Reagent Co., Ltd.) are added into a three-necked flask, and after stirring for 6 hours at 25°C, the solvent is removed by rotary evaporation, the hydrolyzate is dissolved in toluene, and after washing three times with deionized water, it is dried and spin-dried to obtain a carboxyl-organic silicon-vinyl (CaSiVi) coupling agent. The molecular weight of the coupling agent is 780, and the general formula of the silicone skeleton in the coupling agent is , where * represents the connecting key; a=1, b=2, c=0, d=6.
[0064] The preparation method of the parylene coating is as follows:
[0065] The coupling agent was dissolved in isopropanol to prepare a 1.5wt% soaking solution, and the stainless steel substrate was soaked in the soaking solution for 0.5h, and then dried at 65°C for 1h to obtain a plated device, and then the plated device was placed in a furnace for evaporation at 25°C for 20 hours, and then the parylene layer was deposited by CVD. The mass of the coupling agent is 5% of the mass of the parylene layer. Among them, parylene was purchased from Suzhou Yaco Technology Co., Ltd., and the type was C; the stainless steel sheet was purchased from Dongguan Baiside Plastic Co., Ltd., and the test piece size was 25.4×112.5×2mm. The length and width of the parylene layer were the same as the substrate, which were 25.4mm and 112.5mm respectively. The average thickness of the parylene layer was 10μm. The CVD deposition of the parylene layer included three stages. The first stage was the evaporation stage, with a temperature of 150°C and a vacuum degree of 30-60Pa. The second stage was the thermal decomposition stage, with a temperature of 700°C and a vacuum degree of 13-33Pa. The third stage was the deposition stage, with a temperature of 25°C, a vacuum degree of 1-3Pa, and a deposition rate of 1μm / hour.
[0066] Example 2
[0067] Refer to Example 1, except that the coupling agent is a phosphoric acid-organic silicon-methacrylate coupling agent. The coupling agent is prepared by adding 50 g of polydimethylsiloxane phosphate (KSG-370, Shin-Etsu Chemical Co., Ltd.), 31.5 g of tetraethyl orthosilicate (Sinopharm Group Chemical Reagent Co., Ltd.), 73.7 g of hexamethyldisiloxane (Sinopharm Group Chemical Reagent Co., Ltd.), 37.6 g of 3-(methacryloyloxy)propyltrimethoxysilane (Sinopharm Group Chemical Reagent Co., Ltd.), 4 g of acetic acid (Sinopharm Group Chemical Reagent Co., Ltd.), 36 g of deionized water and 200 g of isopropanol (Sinopharm Group Chemical Reagent Co., Ltd.) into a three-necked flask, stirring for 6 hours at 25°C, and then removing the solvent by rotary evaporation, dissolving the hydrolyzate in toluene, washing three times with deionized water, drying, and spin drying to obtain a phosphoric acid-organic silicon-methacrylate (PSiMe) coupling agent. The general formula of the coupling agent silicone skeleton is the same as that of the coupling agent silicone skeleton in Example 1, wherein a=1, b=2, c=0, d=6, and the molecular weight of the coupling agent is 945. The mass of the coupling agent is 5% of the mass of the parylene layer. The average thickness of the parylene layer is 10 μm.
[0068] Example 3
[0069] Refer to Example 1, except that the coupling agent is a carboxyl-silicone-vinyl coupling agent. The preparation method of the coupling agent is as follows: 50 g of triethoxysilyl valeric acid (synthesized by the synthesis method of "Stable carboxylic acid derivatized alkoxy silanes", Chem. Commun., 2015, 51, 2339-2341), 78.8 g of tetraethyl orthosilicate (Sinopharm Chemical Reagent Co., Ltd.), 122.8 g of hexamethyldisiloxane (Sinopharm Chemical Reagent Co., Ltd.), 36 g of vinyl triethoxysilane (Sinopharm Chemical Reagent Co., Ltd.), 10 g of acetic acid (Sinopharm Chemical Reagent Co., Ltd.), 60 g of deionized water and 767 g of isopropanol (Sinopharm Chemical Reagent Co., Ltd.) are added into a three-necked flask, and after stirring for 6 hours at 25° C., the solvent is removed by rotary evaporation, the hydrolyzate is dissolved in toluene, washed three times with deionized water, dried, and spin-dried to obtain a carboxyl-silicon-vinyl (CaSiVi) coupling agent. The general formula of the coupling agent silicone skeleton is the same as that of the coupling agent silicone skeleton in Example 1, wherein a=2, b=3, c=0, d=8, and the molecular weight of the coupling agent is 1018. The mass of the coupling agent is 5% of the mass of the parylene layer. The average thickness of the parylene layer is 10 μm.
[0070] Example 4
[0071] Referring to Example 1, the difference is that the coupling agent is a carboxyl-organic silicon-acrylate coupling agent, and the coupling agent is prepared by adding 50 g of triethoxysilyl valeric acid (synthesized by the synthesis method of "Stable carboxylic acid derivatized alkoxy silanes", Chem. Commun., 2015, 51, 2339-2341), 39.4 g of tetraethyl orthosilicate (Sinopharm Chemical Reagent Co., Ltd.), 92.1 g of hexamethyldisiloxane (Sinopharm Chemical Reagent Co., Ltd.), 47 g of 3-methacryloxypropyltrimethoxysilane (Sinopharm Chemical Reagent Co., Ltd.), 10 g of acetic acid (Sinopharm Chemical Reagent Co., Ltd.), 40 g of deionized water and 618 g of isopropanol (Sinopharm Chemical Reagent Co., Ltd.) into a three-necked flask. After stirring for 6 hours at 25°C, the solvent was removed by rotary evaporation, and the hydrolyzate was dissolved in toluene, washed three times with deionized water, dried, and spin-dried to obtain a carboxyl-organic silicon-acrylate (CaSiAcrylate) coupling agent. The general formula of the coupling agent silicone skeleton is the same as the general formula of the coupling agent silicone skeleton in Example 1, wherein a=1, b=2, c=0, d=6, and the molecular weight of the coupling agent is 865. The mass of the coupling agent is 5% of the mass of the parylene layer. The average thickness of the parylene layer is 10 μm.
[0072] Example 5
[0073] Refer to Example 1, except that the coupling agent is a carboxyl-organic silicon-allyl coupling agent. The preparation method of the coupling agent is as follows: 50 g of triethoxysilyl valeric acid (synthesized by the synthesis method of "Stable carboxylic acid derivatized alkoxy silanes", Chem. Commun., 2015, 51, 2339-2341), 39.4 g of tetraethyl orthosilicate (Sinopharm Chemical Reagent Co., Ltd.), 92.1 g of hexamethyldisiloxane (Sinopharm Chemical Reagent Co., Ltd.), 38.6 g of allyl triethoxysilane (Sinopharm Chemical Reagent Co., Ltd.), 10 g of acetic acid (Sinopharm Chemical Reagent Co., Ltd.), 35 g of deionized water and 560 g of isopropanol (Sinopharm Chemical Reagent Co., Ltd.) are added into a three-necked flask, and after stirring for 6 hours at 25° C., the solvent is removed by rotary evaporation, and the hydrolyzate is dissolved in toluene, washed three times with deionized water, dried, and spin-dried to obtain a carboxyl-organosilicon-allyl (CaSiAllyl) coupling agent. The general formula of the coupling agent silicone skeleton is the same as that of the coupling agent silicone skeleton in Example 1, wherein a=1, b=2, c=0, d=6, and the molecular weight of the coupling agent is 793. The mass of the coupling agent is 5% of the mass of the parylene layer. The average thickness of the parylene layer is 10 μm.
[0074] Example 6
[0075] Referring to Example 1, the difference is that the amount of coupling agent is different, specifically, the concentration of the soaking solution is 15wt%. The mass of the coupling agent is 12.5% of the mass of the parylene layer. The average thickness of the parylene layer is 10μm.
[0076] Example 7
[0077] Referring to Example 1, the difference is that the coupling agent is a carboxyl-silicone-vinyl coupling agent, and the coupling agent is prepared by adding dimethylethoxysilane valeric acid (using "Stable carboxylic acidderivatized alkoxy silanes", Chem. Commun., 2015, 51, 2339-2341) into a three-necked flask. The mixture was stirred at 25°C for 6 hours, and then the solvent was removed by rotary evaporation. The hydrolyzate was dissolved in toluene, washed with deionized water three times, dried, and spin-dried to obtain a carboxyl-organic silicon-vinyl (CaSiVi) coupling agent. The general formula of the coupling agent organosilicon skeleton was the same as that of the coupling agent organosilicon skeleton in Example 1. The coupling agent organosilicon skeleton had a=0, b=0, c=7, d=2, and a molecular weight of 779. The mass of the coupling agent was 5% of the mass of the parylene layer. The average thickness of the parylene layer was 10 μm.
[0078] Example 8
[0079] Referring to Example 1, the difference is that the coupling agent is (Guangzhou Jingde Chemical Materials Co., Ltd., PM-1510SP), the organic skeleton is a polyolefin skeleton, n 1 =8, the molecular weight of the coupling agent is 280, the mass of the coupling agent is 5% of the mass of the parylene layer, and the average thickness of the parylene layer is 10 μm.
[0080] Example 9
[0081] The method of Example 8 is followed, except that n 1 =10, the molecular weight of the coupling agent is 308, the mass of the coupling agent is 5% of the mass of the parylene layer, the coupling agent is purchased from Guangzhou Jingde Chemical Materials Co., Ltd., and the product number is PM1520EC. The average thickness of the parylene layer is 10μm.
[0082] Comparative Example 1
[0083] The method of Example 1 was followed, except that the coupling agent was (Guangzhou Jingde Chemical Materials Co., Ltd., PM-2010SP), the organic skeleton is a polyether skeleton, the molecular weight of the coupling agent is 328, the mass of the coupling agent is 10% of the mass of the parylene layer, the concentration of the immersion liquid is 3.5%. The average thickness of the parylene layer is 10μm.
[0084] Comparative Example 2
[0085] The method was carried out in accordance with Example 1, except that the amount of the coupling agent was different, specifically, the concentration of the soaking solution was 30wt%, and the mass of the coupling agent was 60% of the mass of the parylene layer. The average thickness of the parylene layer was 10μm.
[0086] Comparative Example 3
[0087] The method is carried out in accordance with Example 1, except that the coupling agent is a carboxyl-silicone-vinyl coupling agent, and the coupling agent is prepared by adding dimethylethoxysilane valeric acid (using "Stable carboxylic acid derivatized alkoxy silanes", Chem. Commun., 2015, 51, 2339-2341) into a three-necked flask. The mixture was stirred at 25°C for 6 hours, and then the solvent was removed by rotary evaporation. The hydrolyzate was dissolved in toluene, washed with deionized water three times, dried, and spin-dried to obtain a carboxyl-organic silicon-vinyl (CaSiVi) coupling agent. The general formula of the coupling agent organosilicon skeleton was the same as that of the coupling agent organosilicon skeleton in Example 1. The coupling agent organosilicon skeleton had a=0, b=1, c=1, d=3, and a molecular weight of 482. The mass of the coupling agent was 5% of the mass of the parylene layer. The average thickness of the parylene layer was 10 μm.
[0088] Comparative Example 4
[0089] The method of Example 1 was followed, except that the coupling agent was (Guangzhou Jingde Chemical Materials Co., Ltd., PM-1560EC), the organic skeleton is polymerized tetrahydrofuran, the molecular weight of the coupling agent is 296, and the mass of the coupling agent is 5% of the mass of the parylene layer. The average thickness of the parylene layer is 10μm.
[0090] Comparative Example 5
[0091] The method of Example 1 was used, except that the coupling agent was prepared by adding 50 g of triethoxysilyl valeric acid (synthesized by the synthesis method of "Stable carboxylic acid derivatized alkoxy silanes", Chem. Commun., 2015, 51, 2339-2341), 39.4 g of tetraethyl orthosilicate (Sinopharm Chemical Reagent Co., Ltd.), 92.1 g of hexamethyldisiloxane (Sinopharm Chemical Reagent Co., Ltd.), 33.7 g of methyltriethoxysilane (Sinopharm Chemical Reagent Co., Ltd.), 8 g of acetic acid (Sinopharm Chemical Reagent Co., Ltd.), 35 g of deionized water and 583 g of isopropanol (Sinopharm Chemical Reagent Co., Ltd.) into a three-necked flask, stirring for 6 hours at 25° C., and then removing the solvent by rotary evaporation. The hydrolyzate was dissolved in toluene, washed three times with deionized water, dried, and spin-dried to obtain a carboxyl-silicon-methyl end-capping (CaSiMethyl) coupling agent. The coupling agent is , the molecular weight of the coupling agent is 767. The mass of the coupling agent is 5% of the mass of the parylene layer. The average thickness of the parylene layer is 10 μm.
[0092] Comparative Example 6
[0093] The method of Example 1 is referred to, except that the coupling agent is prepared by adding 50 g of n-hexyltriethoxysilane (Sinopharm Chemical Reagent Co., Ltd.), 42.0 g of tetraethyl orthosilicate (Sinopharm Chemical Reagent Co., Ltd.), 98.2 g of hexamethyldisiloxane (Sinopharm Chemical Reagent Co., Ltd.), 41.2 g of allyltriethoxysilane (Sinopharm Chemical Reagent Co., Ltd.), 8 g of acetic acid (Sinopharm Chemical Reagent Co., Ltd.), 35 g of deionized water and 625 g of isopropanol (Sinopharm Chemical Reagent Co., Ltd.) into a three-necked flask, stirring for 6 hours at 25°C, and then removing the solvent by rotary evaporation, dissolving the hydrolyzate in toluene, washing it three times with deionized water, drying it, and spinning it to obtain an alkyl-organosilicon-allyl (AlkylSiAllyl) coupling agent. The coupling agent is The molecular weight of the coupling agent is 777, and the mass of the coupling agent is 5% of the mass of the parylene layer. The average thickness of the parylene layer is 10 μm.
[0094] Test Case
[0095] The parylene coating obtained in the above-mentioned embodiment and comparative example was subjected to various performance tests shown in Table 1, and the results are shown in Table 1. Among them, the bonding strength was tested according to the ASTM D3359 hundred-grid test method, and the bonding strength grades are shown in Table 1. The higher the grade number, the stronger the bonding strength. The hundred-grid test method includes: marking the coating surface according to the standard, and then adhering it with a specific tape to see whether the coating can be adhered by the tape to judge the bonding strength of the coating. And because the atmosphere at different heights in the CVD furnace may be different, the present invention divides the furnace into 5 different heights when the parylene layer is deposited by CVD, and stainless steel sheets are placed at different heights. Five groups of grade data are obtained by testing, and the bonding strength data are represented by range and point values. For example, if the five groups of grade data are 5B, 5B, 4B, 4B, 5B, the final data measured is 4B~5B, and if the five groups of grade data are 5B, 5B, 5B, 5B, 5B, the final data measured is 5B.
[0096] Among them, the bonding strength 2 hours out of the oven is obtained by storing it at room temperature 25°C and humidity 50% for 2 hours and then testing it according to the above standards.
[0097] The bonding strength at 150℃ for 2h refers to the bonding strength measured according to the above standard after being baked for 3 days and aged in a drying oven at 150℃ for 2h.
[0098] The appearance is the appearance of the parylene coating on the surface of the stainless steel substrate after being stored for one week at room temperature 25°C and humidity 50%.
[0099] The coatings in Comparative Examples 5 and 6 have no binding force and cannot be used for surface protection of metal substrates. The surface of the stainless steel substrate has the parylene coating of Example 2, and the photographs taken after being stored at room temperature 25°C and humidity 50% for one week after being taken out of the oven refer to Figure 1 .
[0100] Table 1
[0101]
[0102] Comparing Examples 4 and 5 with Examples 1-3, the coupling agents are carboxyl-organic silicon-vinyl coupling agents and phosphoric acid-organic silicon-methacrylate coupling agents, which are more conducive to improving the bonding strength between the parylene layer and the substrate, and the bonding strength does not decrease after aging at 150 degrees Celsius for 2 hours. Comparing Examples 1 and 6, the coupling agent is 0.5%-10% of the mass of the parylene layer, which is more conducive to maintaining high bonding strength after aging at a higher temperature of 150 degrees Celsius. Comparing Examples 1 and 7, the general formula of the silicone polymer skeleton is a=1~7, b=1~4, c=0~3, d=0~18, which is more conducive to improving the bonding strength between the parylene layer and the substrate, and the bonding strength does not decrease after aging at 150 degrees Celsius for 2 hours. Comparing Examples 1, 8 and 9, the skeleton is a silicone skeleton, which is more conducive to improving the bonding strength between the parylene layer and the substrate, and the bonding strength does not decrease after aging at 150 degrees Celsius for 2 hours.
[0103] Comparing Comparative Examples 1 and 4 with the embodiment, M is an organic silicon polymer skeleton or a polyolefin skeleton, which can improve the bonding strength between the parylene layer and the substrate, and the bonding strength does not decrease after aging at 150 degrees Celsius for 2 hours. Comparing Comparative Example 2 with the embodiment, the mass of the coupling agent is 0.5%-13% of the mass of the parylene layer, which can improve the bonding strength between the parylene layer and the substrate, and the bonding strength does not decrease after aging at 150 degrees Celsius for 2 hours. Comparing Comparative Example 3 with the embodiment, when M is an organic silicon polymer skeleton, the molecular weight of the coupling agent is 750-2200, which can prevent the generation of imprints. Comparing Comparative Examples 5 and 6 with the embodiment, the coupling agent has both an A end and a B end, which can improve the bonding strength between the parylene layer and the substrate.
[0104] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A parylene coating for a metal substrate surface, characterized in that: The parylene coating comprises a parylene layer and a coupling agent, wherein the coupling agent exists between the parylene layer and the substrate to be plated, and the coupling agent is chemically bonded to the parylene layer and the substrate to be plated, respectively, and the mass of the coupling agent is 0.5%-13% of the mass of the parylene layer; the substrate to be plated is a metal substrate; the coupling agent has the following general formula: AMB; Among them, A is selected from , , or ; B is selected from a group containing a carboxyl group or ; M is an organosilicon polymer skeleton or a polyolefin skeleton; * indicates a connection key; When the M is a silicone polymer skeleton, the molecular weight of the coupling agent is 750-2200; when the M is a polyolefin skeleton, the molecular weight of the coupling agent is 190-550.
2. The parylene coating according to claim 1, characterized in that: The general formula of the organosilicon polymer skeleton is , where * represents the connecting key, a=1~7, b=1~4, c=0~3, d=0~18.
3. The parylene coating according to claim 1, characterized in that: The M is or , where * represents the connecting key, n1=1~18, n=1~9.
4. The parylene coating according to claim 1, characterized in that: The coupling agent is a carboxyl-organic silicon-vinyl coupling agent, a phosphoric acid-organic silicon-methacrylate coupling agent, a carboxymethyl-organic silicon-vinyl coupling agent, and a carboxymethyl-organic silicon-methacrylate coupling agent.
5. The parylene coating according to claim 1, characterized in that: The mass of the coupling agent is 0.5%-10% of the mass of the parylene layer.
6. A method for preparing a parylene coating, characterized in that: It is used to prepare the parylene coating as described in any one of claims 1 to 5, and the preparation method sequentially comprises the first step or the second step, and depositing the parylene layer; The first step is to immerse the substrate to be plated in an organic solution containing a coupling agent and then dry it; The second step is to put the coupling agent into the atomization chamber, volatilize the coupling agent in a vacuum heating environment, and make the volatilized coupling agent react on the surface of the substrate to be plated.
7. The preparation method according to claim 6, characterized in that: The coupling agent-containing organic solution is obtained by dissolving the coupling agent in an organic solvent, wherein the mass concentration of the coupling agent in the coupling agent-containing organic solution is 0.8wt%-6wt%; and / or, The soaking time is 10 min-180 min, and the drying conditions include: the drying temperature is 40° C.-80° C., and the time is 1 h-3 h.
8. Use of the parylene coating according to any one of claims 1 to 5 or the parylene coating prepared by the method for preparing the parylene coating according to claim 6 or 7 in surface protection of a substrate to be plated, wherein the substrate to be plated is a metal substrate.
Citation Information
Patent Citations
Parylene protective coating and preparation method and application thereof
CN106905813A
Parylene coating as well as preparation method and application thereof
CN115569823A
Ink-jet head and the preparation method thereof, and a coating layer and the preparation method thereof
US20030052949A1
Composite coating, preparation method and device
WO2024131538A1