Fullerol / silver nanocluster composite material with nonlinear optical property as well as preparation method and application of fullerol / silver nanocluster composite material

Through supramolecular co-assembly technology, hydroxylated fullerol and Ag6-nanoclusters are formed into spherical assemblies, which solves the problems of fullerene solubility and nonlinear optical properties, and realizes fullerol/silver nanocluster composites. The efficient dispersion and nonlinear optical performance are improved, making it suitable for laser protection.

CN118720128APending Publication Date: 2024-10-01SHANDONG UNIV +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410761751.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing fullerenes and their derivatives have low solubility in water, which limits their application scope. At the same time, their nonlinear optical properties are reduced due to the introduction of oxygen-containing functional groups, and they lack the composite optical limiting of fullerenes and metal nanoclusters. Materials research.

Method used

Through a supramolecular co-assembly method, hydroxylated fullerol (C60-OH) and Ag6-nanoclusters (Ag6-NCs) were formed into a spherical assembly through hydrogen bonding interactions, and a fullerol/silver nanocluster composite was prepared. materials that break solubility limitations and improve nonlinear optical properties.

Benefits of technology

The good dispersion and nonlinear optical properties of the fullerol/silver nanocluster composite material in methylene chloride have been achieved, and its nonlinear optical properties have been significantly improved, making it suitable for use as optical limiting materials in the field of laser protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004891278790000011
    Figure HDA0004891278790000011
  • Figure HDA0004891278790000012
    Figure HDA0004891278790000012
  • Figure HDA0004891278790000013
    Figure HDA0004891278790000013
Patent Text Reader

Abstract

The invention relates to a fullerol / silver nanocluster composite material with nonlinear optical properties and a preparation method and application thereof. A supramolecular assembly method is utilized, a mixed aqueous solution of fullerol and Ag6-NCs is mixed with NMP, no template is needed, and the NMP induces hydroxyl on the surface of fullerol and carboxyl of an Ag6-NCs ligand to be co-assembled through hydrogen bond interaction to form a spherical assembly; and then centrifuging, washing and freeze-drying to obtain the fullerol / silver nanocluster composite material. The fullerol / silver nanocluster composite material synthesized by the method is good in dispersity and can be uniformly dispersed in a PMMA (polymethyl methacrylate) film, and the obtained fullerol / silver nanocluster / PMMA film is high in transparency, shows excellent anti-saturation absorption property and has great potential application value in the field of laser protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a fullerol / silver nanocluster composite material with nonlinear optical properties and a preparation method and application thereof, belonging to the field of new optical limiting materials. Background Art

[0002] In modern life, the widespread use of high-energy lasers brings convenience to people's lives, but also poses great safety hazards. High-energy lasers have the advantages of fast speed, high intensity, and low production cost, and have become a popular modern warfare weapon studied by various countries. In addition to causing damage to human eyes, causing dizziness or even blindness, laser weapons can also be used to destroy optical sensors and large weapons such as missiles, which are very destructive. As a material that can effectively limit high-intensity input light in an ultra-short time, nonlinear optical limiting materials have a wide limiting band, fast response speed, high linear transparency and low linear transmittance, which can effectively reduce the harm and losses that may be caused by strong lasers, and effectively counter the threat of frequency-sensitive and short pulses.

[0003] There are many types of optical limiting materials, such as fullerene (C 60 ), graphene (GO), inorganic semiconductor nanomaterials, metal nanoclusters (NCs), and various composite materials have been studied as optical limiting materials. For example, Gao et al. combined silver nanoparticles with C 60 The composite material C 60 tpy-Ag, its chloroform solution has good optical confinement performance, and as the concentration of silver nanoparticles increases, the optical limiting threshold will decrease (Y.Gao, et al.Opt.Commun.2003,223,103-108). Patent document CN117282657 A (application number: 202310999444.X) discloses a method for regulating the nonlinear optical properties of reduced graphene oxide by Au@CdS and rGO-Au@CdS composite materials. The Au@CdS core-shell structure grows evenly on the surface of reduced graphene oxide, and the core-shell structure is tightly connected to the reduced graphene oxide. The rGO-Au@CdS composite material was successfully synthesized by the solvothermal method. The nonlinear absorption of the composite material shows the characteristics of transition from saturated absorption to reverse saturation, and it becomes more obvious with the increase of light intensity. As the size of the Au@CdS composite structure increases, the intensity of the reverse saturation absorption is also improved.

[0004] Most fullerenes and their derivatives have anti-saturation absorption characteristics and fast response time, which makes them have great potential application value in optical devices. However, the solubility of fullerene in water is very low, which greatly limits its application scope. The emergence of water-soluble fullerene derivatives (hydroxylated fullerene, i.e., fullerol, etc.) breaks the limitation of its solubility and greatly broadens its application scope in biomedicine and other fields. However, due to the introduction of oxygen-containing functional groups, the large π conjugated structure of fullerene is destroyed, resulting in its nonlinear optical properties and optical limiting effect being lower than that of the original fullerene (X. Zhang, et al. J. Opt. 2015, 17, 015501).

[0005] Some metal NCs also have nonlinear optical limiting capabilities. For example, it has been reported that the favorable synergy between organic ligand modification and cluster core fine-tuning leads to enhanced third-order nonlinear optical response of copper (I) sulfide clusters (Y. Cheng, et al. Cryst. Growth Des. 2023, 23, 5421-5427). However, there are currently no literature reports on composite optical limiting materials of fullerenes and their derivatives with metal NCs. Summary of the invention

[0006] In view of the shortcomings of the prior art, in order to further enrich the composite optical limiting materials of fullerene and its derivatives, break the limitation of fullerene solubility and the limitation of low nonlinear optical signals of metal nanoclusters and fullerols, the present invention provides a fullerol / silver nanocluster composite material with nonlinear optical properties, and its preparation method and application.

[0007] The fullerol / silver nanocluster composite material of the present invention has both excellent solubility and dispersibility and nonlinear optical properties, can be uniformly dispersed in a dichloromethane solution of PMMA, and can be used as an optical limiting material in laser protection.

[0008] Terminology Note:

[0009] Ag6-NCs: It is an atomically precise hexanuclear silver nanocluster with 2-mercaptonicotinic acid (H2mna) as its ligand. Under certain conditions, π-π interactions, charge transfer from ligand to metal, charge transfer from ligand to metal-metal, and metal-metal interactions can occur between the ligands. After assembling Ag6-NCs, they have certain luminescence properties.

[0010] C 60 -OH: It is a polyhydroxy fullerene derivative with 18-24 hydroxyl groups and a molecular formula of C 60 (OH) 18.2 (ONa) 3.86 6.6H2O, abbreviated as C 60 -OH.

[0011] C 60 -OH / Ag6-NCs / NMP / H2O: The fullerol / silver nanocluster composite material prepared by the present invention is composed of Ag6-NCs and C 60 -OH is obtained by supramolecular co-assembly through hydrogen bonding interactions.

[0012] Ag6-NCs / NMP / H2O: The silver nanocluster assembly prepared by the present invention is obtained by supramolecular self-assembly of Ag6-NCs through hydrogen bonding interaction.

[0013] Polymethyl methacrylate is referred to as PMMA.

[0014] The technical solution of the present invention is as follows:

[0015] A fullerol / silver nanocluster composite material with nonlinear optical properties. The composite material is a small spherical assembly formed by co-assembly of hydroxyl groups on the surface of fullerol and carboxyl groups of silver nanocluster ligands through hydrogen bond interaction.

[0016] Preferably according to the present invention, the silver nanoclusters are Ag6-NCs.

[0017] According to the preferred embodiment of the present invention, the fullerol is C 60 -OH, C 60 -OH is a hydroxylated fullerene derivative, i.e. fullerene C 60 The surface is modified with 18-24 hydroxyl groups. 60 -OH is carried out according to the prior art (see S. Zhou, et al. Chem. Eur. J. 2018, 24, 16609-16619).

[0018] The preparation method of the fullerol / silver nanocluster composite material having nonlinear optical properties comprises the following steps:

[0019] Ag6-NCs powder is added to a fullerol aqueous solution, and vortexed to mix evenly to obtain an Ag6-NCs / fullerol mixed aqueous solution; N-methylpyrrolidone (NMP) is added to the Ag6-NCs / fullerol mixed aqueous solution to obtain a mixed solution, which is vortexed to allow sufficient reaction, and then allowed to stand, centrifuged, washed, and freeze-dried to obtain a fullerol / silver nanocluster composite material.

[0020] According to the preferred embodiment of the present invention, the fullerol is C 60 -OH.

[0021] Preferably according to the present invention, the concentration of fullerol in the Ag6-NCs / fullerol mixed aqueous solution is 5-20 mg / mL.

[0022] Most preferably, the concentration of fullerol in the Ag6-NCs / fullerol mixed aqueous solution is 10 mg / mL.

[0023] Preferably according to the present invention, the amount of Ag6-NCs contained in the Ag6-NCs / fullerol mixed aqueous solution is 3-8 mmol.

[0024] Most preferably, the amount of Ag6-NCs contained in the Ag6-NCs / fullerol mixed aqueous solution is 5 mmol.

[0025] Preferably according to the present invention, the volume ratio of the Ag6-NCs / fullerol mixed aqueous solution to NMP is (1-3): (7-9).

[0026] Most preferably, the volume ratio of the Ag6-NCs / fullerol mixed aqueous solution to NMP is 1:9.

[0027] Preferably according to the present invention, the concentration of fullerenol in the mixed solution is 0.5-2 mg / mL.

[0028] Most preferably, the concentration of fullerenol in the mixed solution is 1 mg / mL.

[0029] Preferably according to the present invention, the concentration of Ag6-NCs in the mixed solution is 3-8 mmol / mL.

[0030] Most preferably, the concentration of Ag6-NCs in the mixed solution is 5 mmol / mL.

[0031] Preferably according to the present invention, after the Ag6-NCs powder is added to the fullerol aqueous solution, the powder is vortexed at room temperature for 1-5 minutes; after the NMP is added, the powder is vortexed at room temperature for 1-2 minutes.

[0032] Preferably according to the present invention, the standing time is 2-3 days.

[0033] Preferably according to the present invention, the centrifugal speed is 7000-9000 r / min, and the centrifugal time is 5-10 min.

[0034] Most preferably, the centrifugal speed is 8000 r / min and the centrifugal time is 8 min.

[0035] Preferably according to the present invention, the washing is performed at room temperature using a mixed solvent of water and NMP in a volume ratio of 1:9.

[0036] Preferably according to the present invention, the centrifugation and washing steps are repeated 2-3 times.

[0037] According to the preferred embodiment of the present invention, the freeze-drying temperature is -50 to -70°C and the freeze-drying time is 2 to 3 days. After freeze-drying, the fullerol / silver nanocluster composite material is obtained.

[0038] A fullerol / silver nanocluster / PMMA film with nonlinear optical properties is prepared by using the fullerol / silver nanocluster composite material with nonlinear optical properties.

[0039] The preparation method of fullerol / silver nanocluster / PMMA film with nonlinear optical properties comprises the following steps:

[0040] Dissolve polymethyl methacrylate (PMMA) in dichloromethane, and perform ultrasonic treatment to obtain a dichloromethane solution of PMMA; disperse the fullerol / silver nanocluster composite material in the dichloromethane solution of PMMA, mix evenly, and homogenize to obtain a dispersion; transfer the obtained dispersion to a watch glass, and let it stand at room temperature to form a film, thereby obtaining a fullerol / silver nanocluster / PMMA film.

[0041] Preferably according to the present invention, the mass ratio of PMMA to the volume ratio of dichloromethane is 30-50 mg:1 mL.

[0042] Preferably according to the present invention, the relative molecular mass of the polymethyl methacrylate (PMMA) is 300,000-400,000.

[0043] Most preferably, the relative molecular mass of the polymethyl methacrylate (PMMA) is 350,000.

[0044] According to the preferred embodiment of the present invention, the ultrasonic treatment time is 2-15 min.

[0045] Preferably according to the present invention, the mass ratio of the fullerol / silver nanocluster composite material to PMMA is 1:150-250.

[0046] Further preferably, the mass ratio of the fullerol / silver nanocluster composite material to PMMA is 1:180-220.

[0047] Most preferably, the mass ratio of the fullerol / silver nanocluster composite material to PMMA is 1:200.

[0048] Preferably, according to the present invention, the homogenization is to homogenize the mixture of the fullerol / silver nanocluster composite material and the dichloromethane solution of PMMA through a homogenizer at room temperature for 3-5 minutes at a homogenization speed of 80-110 r / min.

[0049] Preferably according to the present invention, the film forming time is 10-24h.

[0050] Preferably according to the present invention, the thickness of the obtained fullerol / silver nanocluster / PMMA film is 21.5-98.6 μm; the content of the fullerol / silver nanocluster composite material in the fullerol / silver nanocluster / PMMA film is 0.2-1%.

[0051] The present invention also provides an application of fullerol / silver nanocluster / PMMA film with nonlinear optical properties, which is used as a light limiting material for laser protection.

[0052] The technical features and beneficial effects of the present invention are as follows:

[0053] 1. The present invention utilizes a supramolecular assembly method to mix a mixed aqueous solution of fullerol and Ag6-NCs with NMP, without any template, and NMP induces the hydroxyl groups on the surface of fullerol and the carboxyl groups of the Ag6-NCs ligands to co-assemble to form a spherical assembly through hydrogen bonding interaction; then centrifugation, washing, and freeze-drying are performed to obtain a fullerol / silver nanocluster composite material. The fullerol / silver nanocluster composite materials synthesized by the present invention all exhibit nonlinear optical properties of anti-saturation absorption; wherein the Ag6-NCs and fullerol are co-assembled through hydrogen bonding interaction, which is conducive to expanding the π electron delocalization system and greatly improving the nonlinear optical performance.

[0054] 2. The present invention mixes a mixed aqueous solution of fullerol and Ag6-NCs with NMP to assemble a fullerol / silver nanocluster composite material, which has greatly improved nonlinear optical properties and optical limiting properties compared with fullerol and silver nanoclusters.

[0055] 3. The fullerene alcohol / silver nanocluster composite material prepared by the method of the present invention has good dispersibility in dichloromethane and is an organic-inorganic hybrid optical limiting material with excellent dispersibility. It breaks the limitation of fullerene solubility and the limitation of low nonlinear optical signals of metal nanoclusters and fullerene alcohol, and exhibits excellent anti-saturation absorption properties, so that its nonlinear optical performance test is not limited to the solution state.

[0056] 4. The fullerol / silver nanocluster / PMMA film with nonlinear optical properties of the present invention has high transparency and has great potential application value in the field of laser protection.

[0057] 5. The polymethyl methacrylate used in the present invention has specificity, and the nonlinear optical signal of the PMMA film formed by it is basically zero, which will not affect the test signal. It is worth noting that in the process of preparing the PMMA film, since the dichloromethane solution of PMMA is relatively volatile, after adding the fullerol / silver nanocluster composite material and mixing it evenly, it needs to be quickly transferred to a watch glass and allowed to stand to form a film. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1Schematic diagram of the preparation of the fullerol / silver nanoclusters / PMMA film of the present invention.

[0059] Figure 2 These are micrographs of the fullerol / silver nanocluster composite material prepared in Example 1, wherein (a) is a SEM photograph and (b) is a TEM photograph.

[0060] Figure 3 C 60 -OH, Ag6-NCs, Ag6-NCs assembly Ag6-NCs / NMP / H2O and fullerol / silver nanocluster composite material C prepared in Example 1 60 Infrared spectrum of -OH / Ag6-NCs / NMP / H2O (a) and local enlarged image (b).

[0061] Figure 4 Photos and film thicknesses of the fullerol / silver nanocluster / PMMA film prepared in Example 1, the fullerol / PMMA film prepared in Comparative Example 1, the silver nanocluster / PMMA film prepared in Comparative Example 2, and the silver nanocluster assembly / PMMA film prepared in Comparative Example 3.

[0062] Figure 5 These are graphs showing the nonlinear reverse saturation absorption optical properties of the fullerol / silver nanoclusters / PMMA films prepared in Examples 1 to 5.

[0063] Figure 6 These are nonlinear reverse saturation absorption optical performance graphs of the fullerol / PMMA film, silver nanocluster / PMMA film, and silver nanocluster assembly / PMMA film prepared in Example 1 and Comparative Examples 1 to 3.

[0064] Figure 7 Comparison of the optical limiting curves of the fullerol / silver nanocluster / PMMA films prepared in Examples 1 to 5, and the fullerol / PMMA films, silver nanocluster / PMMA films and silver nanocluster assembly / PMMA films prepared in Comparative Examples 1 to 3 at a laser energy of 1 μJ.

[0065] Figure 8 The nonlinear absorption coefficient β and the optical limiting threshold F of the fullerol / silver nanocluster / PMMA film prepared in Example 1, and the fullerol / PMMA film, silver nanocluster / PMMA film and silver nanocluster assembly / PMMA film prepared in Comparative Examples 1 to 3 are ol . DETAILED DESCRIPTION

[0066] In order to better understand the present invention, the present invention is further described below in conjunction with specific embodiments and drawings, but is not limited thereto.

[0067] Unless otherwise specified, the experimental methods used in the examples are conventional methods.

[0068] Unless otherwise specified, the materials and reagents used in the examples can be obtained from commercial sources.

[0069] The fullerene alcohol used in the examples is C 60 (OH) 18.2 (ONa) 3.86 6.6H2O, referred to as C 60 -OH, prepared according to the literature "S.Zhou, H.Li, et al.Chem.Eur.J.2018,24,16609-16619";

[0070] The specific process is as follows: 360 mg of fullerene C 60 Dissolve in 225mL of toluene (1.6mg / mL), then add 9mL of 1g / mL sodium hydroxide aqueous solution, 1mL of 30% hydrogen peroxide aqueous solution, 2mL of 40% phase transfer catalyst tetrabutylammonium hydroxide aqueous solution, and stir at room temperature 25°C for 5 days. After the reaction stops, discard the toluene layer, add deionized water, neutralize with hydrochloric acid to a pH value of about 7, and then dialyze with a dialysis bag with a molecular weight cutoff of 100Da to remove the unreacted phase transfer catalyst tetrabutylammonium hydroxide and small molecule fragments. After the dialysis is completed, the solution is concentrated and freeze-dried to obtain a fullerol solid powder.

[0071] The silver nanoclusters Ag6-NCs used in the embodiment are (NH4)6[Ag6(mna)6], which are prepared according to the literature “J.Shen, X.Xin, et al.Nanoscale, 2017, 9, 19191-19200”;

[0072] The specific process is as follows: 167 mg of silver nitrate and 155 mg of 2-mercaptonicotinic acid are dissolved in 10 mL of water, the mixed solution is ultrasonically treated at room temperature for 20 min to obtain a precipitate, and then a 25% ammonia solution is added dropwise until a clear yellow solution is formed. The solution is slowly evaporated, and yellow block crystals Ag6-NCs (yield: 64%) are obtained after two weeks.

[0073] Preparation of Ag6-NCs / NMP / H2O:

[0074] (1) 9.4 mg (5 mmol) of Ag6-NCs powder was added to 100 μL of water and vortexed for 2 min to prepare an Ag6-NCs aqueous solution;

[0075] (2) 900 μL NMP was added to 100 μL Ag6-NCs aqueous solution and vortexed for 1 min to obtain a mixed solution;

[0076] (3) The mixed solution of step (3) was allowed to stand for 3 days, the supernatant was discarded, the precipitate below and the residual supernatant were centrifuged at 8000 r / min for 5 min, and the supernatant was removed; the precipitate was then washed with a water-NMP mixed solvent with a volume ratio of 1:9, vortexed for 1 min, and then centrifuged at 8000 r / min for 5 min, and the supernatant was removed; this step was repeated three times; the obtained precipitate was freeze-dried to obtain an Ag6-NCs / NMP / H2O powder sample.

[0077] Example 1

[0078] The preparation method of fullerol / silver nanocluster / PMMA film with nonlinear optical properties comprises the following steps:

[0079] (1) Prepare 2 mL of 10 mg / mL C 60 -OH aqueous solution, and take out 100 μL 60 -OH aqueous solution is kept in a vial for later use;

[0080] (2) Add 9.4 mg (5 mmol) of Ag6-NCs powder into 100 μL 60 -OH aqueous solution, vortexed for 2 min, and Ag6-NCs / C 60 -OH mixed aqueous solution;

[0081] (3) Add 900 μL NMP to 100 μL Ag6-NCs / C 60 -OH mixed aqueous solution and vortexed for 1 min to obtain a mixed solution.

[0082] (4) The mixed solution of step (3) was allowed to stand for 3 days, the supernatant was discarded, the lower precipitate and the residual supernatant were centrifuged at 8000 r / min for 5 min, and the supernatant was removed; the precipitate was then washed with a water-NMP mixed solvent with a volume ratio of 1:9, vortexed for 1 min, and then centrifuged at 8000 r / min for 5 min, and the supernatant was removed; this step was repeated three times;

[0083] (5) freeze-drying the precipitate obtained in step (4) to obtain a powder sample of the fullerene alcohol / silver nanocluster composite material;

[0084] (6) Weigh 0.2 g of PMMA (Mw ~ 350000) into a 10 mL sample bottle, add 5 mL of dichloromethane to the sample bottle, and sonicate for 15 min to prepare 5 mL of a 40 mg / mL PMMA dichloromethane solution.

[0085] (7) Weigh 1.0 mg of fullerol / silver nanocluster composite material powder and add it to a dichloromethane solution of PMMA. Homogenize at a speed of 90 r / min for 3 min, quickly transfer it to a quartz watch glass, and let it stand in a fume hood at room temperature for 12 h to volatilize. A fullerol / silver nanocluster / PMMA film with a mass content of 0.5% of fullerol / silver nanocluster composite material and a thickness of 21.5 μm was prepared, named C 60 -OH / Ag6-NCs / NMP / H2O film.

[0086] Figure 1 Schematic diagram of the preparation of the fullerol / silver nanocluster / PMMA film of the present invention. 60 NMP was added to the mixed aqueous solution of -OH and Ag6-NCs and vortexed. After static incubation, the precipitate was washed and freeze-dried to obtain a fullerol / silver nanocluster composite material, which was then dispersed in a dichloromethane solution of PMMA to prepare a polymer film.

[0087] Figure 2 These are SEM and TEM images of the fullerol / silver nanocluster composite material prepared in step (5) of this embodiment. As can be seen from the figure, the prepared composite material is a small spherical structure with a size of about 2-5 μm.

[0088] Figure 3 C 60 -OH, Ag6-NCs, Ag6-NCs / NMP / H2O and composite material C prepared in Example 1 60 Infrared spectrum of -OH / Ag6-NCs / NMP / H2O (a) and local enlarged image (b).

[0089] The infrared spectrum shows that the Ag6-NCs / NMP / H2O is located at 1710 cm -1 The stretching vibration peak of C=O in C 60 -OH / Ag6-NCs / NMP / H2O red-shifted to 1704 cm -1 , indicating that the hydrogen bonding interaction is enhanced. Ag6-NCs / NMP / H2O at 3452cm -1 The broad peak near C 60 -OH / Ag6-NCs / NMP / H2O red shifted to 3441cm -1 The broad peak near represents the stretching vibration peak of -OH, proving that hydrogen bonds are formed in the system.

[0090] Example 2

[0091] The same preparation method as described in Example 1, except that:

[0092] In step (2), the amount of Ag6-NCs was replaced with 3 mmol, that is, 5.6 mg of Ag6-NCs powder was weighed and added to 100 μL of C 60 -OH aqueous solution, vortexed for 2 min, and 100 μL Ag6-NCs / C was obtained. 60 -OH mixed aqueous solution.

[0093] The other steps and conditions are consistent with those in Example 1.

[0094] The fullerol / silver nanocluster composite material obtained in this example has a fullerol / silver nanocluster / PMMA film with a mass content of 0.5% and a film thickness of 25.1 μm, and is named 1-3-90 film.

[0095] Example 3

[0096] The same preparation method as described in Example 1, except that:

[0097] In step (2), the amount of Ag6-NCs was replaced with 8 mmol, that is, 14.9 mg of Ag6-NCs powder was weighed and added to 100 μL of C 60 -OH aqueous solution, vortexed for 2 min, and 100 μL Ag6-NCs / C was obtained. 60 -OH mixed aqueous solution.

[0098] The other steps and conditions are consistent with those in Example 1.

[0099] The fullerol / silver nanocluster composite material obtained in this example has a fullerol-silver nanocluster / PMMA film with a mass content of 0.5% and a film thickness of 98.6 μm, and is named 1-8-90 film.

[0100] Example 4

[0101] The preparation method of fullerol / silver nanocluster / PMMA film with nonlinear optical properties comprises the following steps:

[0102] (1) Prepare 2 mL of 5 mmol / mL Ag6-NCs aqueous solution.

[0103] (2) 0.5 mg C 60 -OH powder was added to 100 μL Ag6-NCs aqueous solution and vortexed for 2 min to prepare 100 μL Ag6-NCs / C 60 -OH mixed aqueous solution.

[0104] (3) Add 900 μL NMP to 100 μL Ag6-NCs / C 60 -OH mixed aqueous solution and vortexed for 1 min to prepare a mixed solution.

[0105] (4) The mixed solution of step (3) was allowed to stand for 3 days, centrifuged at 8000 r / min for 5 min, and the supernatant was removed; the precipitate was then washed with a water-NMP mixed solvent with a volume ratio of 1:9, vortexed for 1 min, and then centrifuged at 8000 r / min for 5 min, and the supernatant was removed; this step was repeated three times.

[0106] (5) freeze-drying the precipitate obtained in step (4) to obtain a powder sample of the fullerene alcohol / silver nanocluster composite material.

[0107] (6) Weigh 0.2 g of PMMA (Mw ~ 350000) into a 10 mL sample bottle, add 5 mL of dichloromethane to the sample bottle, and sonicate for 15 min to prepare 5 mL of a 40 mg / mL PMMA dichloromethane solution.

[0108] (7) Weigh 1.0 mg of fullerol / silver nanocluster composite material powder and add it to the dichloromethane solution of PMMA, and homogenize it at 90 r / min for 3 min. Quickly transfer it to a quartz watch glass and let it stand in a fume hood at room temperature for 12 h to prepare a fullerol / silver nanocluster / PMMA film with a fullerol / silver nanocluster composite material content of 0.5% and a film thickness of 34.7 μm, named 0.5-5-90 film.

[0109] Example 5

[0110] The same preparation method as described in Example 4, except that:

[0111] Step (2), C 60 The mass of -OH is replaced by 2.0 mg, that is: weigh 2.0 mg C 60 -OH powder was added into 100 μL of 5 mmol / mL Ag6-NCs aqueous solution.

[0112] The other steps and conditions are consistent with those in Example 4.

[0113] The fullerol / silver nanocluster composite material obtained in this example has a fullerol / silver nanocluster / PMMA film with a mass content of 0.5% and a film thickness of 69.3 μm, and is named 2-5-90 film.

[0114] Comparative Example 1

[0115] A method for preparing a fullerol / PMMA film, comprising the following steps:

[0116] (1) Weigh 0.2 g of PMMA (Mw ~ 350000) into a 10 mL sample bottle, add 5 mL of dichloromethane to the sample bottle, and ultrasonicate for 15 min to prepare 5 mL of dichloromethane solution of PMMA with a concentration of 40 mg / mL.

[0117] (2) Weigh C 60 1.0 mg of -OH powder was added to the dichloromethane solution of PMMA and homogenized at 90 r / min for 3 min. The mixture was quickly transferred to a quartz watch glass and allowed to stand in a fume hood for 12 h at room temperature to evaporate. A fullerol / PMMA film with a fullerol content of 0.5% and a thickness of 29.2 μm was prepared and named C 60 -OH film.

[0118] Comparative Example 2

[0119] A method for preparing a silver nanocluster / PMMA film, comprising the following steps:

[0120] (1) Weigh 0.2 g of PMMA (Mw ~ 350000) into a 10 mL sample bottle, add 5 mL of dichloromethane to the sample bottle, and ultrasonicate for 15 min to prepare 5 mL of PMMA dichloromethane solution with a concentration of 40 mg / mL;

[0121] (2) Weigh 1.0 mg of Ag6-NCs powder and add it to the dichloromethane solution of PMMA. Homogenize at 90 r / min for 3 min. Quickly transfer it to a quartz watch glass and let it stand in a fume hood at room temperature for 12 h to prepare a silver nanocluster / PMMA film with a Ag6-NCs content of 0.5% and a thickness of 29.6 μm, named Ag6-NCs film.

[0122] Comparative Example 3

[0123] A method for preparing a silver nanocluster assembly / PMMA film, comprising the following steps:

[0124] (1) Weigh 0.2 g of PMMA (Mw ~ 350000) into a 10 mL sample bottle, add 5 mL of dichloromethane to the sample bottle, and ultrasonicate for 15 min to prepare 5 mL of dichloromethane solution of PMMA with a concentration of 40 mg / mL.

[0125] (2) Weigh 1.0 mg of Ag6-NCs / NMP / H2O powder and add it to the dichloromethane solution of PMMA. Homogenize at 90 r / min for 3 min. Quickly transfer it to a quartz watch glass and let it stand in a fume hood for 12 h at room temperature to prepare a silver nanocluster assembly / PMMA film with a mass content of 0.5% Ag6-NCs / NMP / H2O and a thickness of 29.4 μm, named Ag6-NCs / NMP / H2O film.

[0126] Experimental example

[0127] The fullerol / silver nanocluster / PMMA films prepared in Examples 1 to 5, the fullerol / PMMA films prepared in Comparative Example 1, the silver nanocluster / PMMA films prepared in Comparative Example 2, and the silver nanocluster assembly / PMMA film prepared in Comparative Example 3 were tested for nonlinear saturated absorption optical properties using Z-scan technology.

[0128] The third-order nonlinear optical test conditions are: incident wavelength λ = 532nm, lens focal length = 40cm, beam waist radius ω0 = 20μm, pulse width τ = 5ns. The nonlinear optical signal of pure PMMA film can be ignored.

[0129] Figure 4 Digital photographs of the fullerol / silver nanocluster / PMMA film prepared in Example 1, and the fullerol / PMMA film, silver nanocluster / PMMA film and silver nanocluster assembly / PMMA film prepared in Comparative Examples 1-3, as well as the average film thickness measured by SEM, show that the fullerol / silver nanocluster / PMMA film prepared in Example 1 is more uniform.

[0130] Figure 5 This is a nonlinear reverse saturation absorption optical performance diagram of the fullerol / silver nanocluster / PMMA film prepared in Examples 1 to 5. As can be seen from the figure, when the Z-axis position is far away from the focus Z=0, that is, when the input flux is low, all materials show linear optical behavior, and when Z=0 at the focus, that is, when the intensity of the laser beam is the maximum, the normalized transmittance of the sample decreases significantly, which indicates that the synthesized materials all have reverse saturation absorption characteristics.

[0131] The nonlinear reverse saturation absorption optical performance results of the fullerol / PMMA film, silver nanocluster / PMMA film and silver nanocluster assembly / PMMA film prepared in Example 1 and Comparative Examples 1 to 3 are shown in Figure 6 .

[0132] Figure 6 It shows that the nonlinear anti-saturation absorption signal of the fullerol / silver nanocluster / PMMA film prepared in Example 1 is the strongest, the nonlinear anti-saturation absorption signals of the fullerol / PMMA film prepared in Comparative Example 1 and the silver nanocluster assembly / PMMA film prepared in Comparative Example 3 are very poor, and the nonlinear anti-saturation absorption signal of the silver nanocluster / PMMA film prepared in Comparative Example 2 is relatively poor.

[0133] Figure 7 The comparison of the optical limiting curves of the fullerol / silver nanocluster / PMMA film prepared in Examples 1-5, and the fullerol / PMMA film, silver nanocluster / PMMA film and silver nanocluster assembly / PMMA film prepared in Comparative Examples 1-3 proves that the material obtained in the present invention has good anti-saturation absorption properties and optical limiting performance.

[0134] Figure 8 The nonlinear absorption coefficient β and the light limiting threshold F obtained by fitting calculation are the fullerol / silver nanocluster / PMMA film prepared in Example 1, and the fullerol / PMMA film, silver nanocluster / PMMA film and silver nanocluster assembly / PMMA film prepared in Comparative Examples 1-3. ol The nonlinear absorption coefficient β of the material obtained in Example 1 is the highest, and the light limiting threshold F ol The lowest value indicates that the performance is the best, which proves that the material obtained by the method of the present invention has excellent nonlinear anti-saturation absorption optical performance and has a good protective effect when applied in the field of laser protection.

[0135] Although the above describes the specific implementation mode of the present invention in conjunction with the accompanying drawings, it is not intended to limit the scope of protection of the present invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.

Claims

1. A fullerol / silver nanocluster composite material with nonlinear optical properties, wherein the composite material is a small spherical assembly formed by co-assembly of hydroxyl groups on the surface of fullerol and carboxyl groups of silver nanocluster ligands through hydrogen bonding interactions.

2. The fullerol / silver nanocluster composite material with nonlinear optical properties according to claim 1, characterized in that: The silver nanoclusters are Ag6-NCs.

3. A method for preparing the fullerol / silver nanocluster composite material with nonlinear optical properties according to claim 1 or 2, comprising the following steps: Ag6-NCs powder is added to a fullerol aqueous solution, and vortexed to mix evenly to obtain an Ag6-NCs / fullerol mixed aqueous solution; N-methylpyrrolidone (NMP) is added to the Ag6-NCs / fullerol mixed aqueous solution to obtain a mixed solution, which is vortexed to allow sufficient reaction, and then allowed to stand, centrifuged, washed, and freeze-dried to obtain a fullerol / silver nanocluster composite material.

4. The preparation method according to claim 3, characterized in that: The fullerenol is C 60 -OH.

5. The preparation method according to claim 3, characterized in that: Includes one or more of the following conditions: i. The concentration of fullerol in the Ag6-NCs / fullerol mixed aqueous solution is 5-20 mg / mL; ii. Preferably, the concentration of fullerol in the Ag6-NCs / fullerol mixed aqueous solution is 10 mg / mL; ⅲ. The amount of Ag6-NCs contained in the Ag6-NCs / fullerol mixed aqueous solution is 3-8 mmol; iv. Preferably, the amount of Ag6-NCs contained in the Ag6-NCs / fullerol mixed aqueous solution is 5 mmol; ⅴ. The volume ratio of the Ag6-NCs / fullerol mixed aqueous solution to NMP is (1-3): (7-9); ⅵ. Preferably, the volume ratio of the Ag6-NCs / fullerol mixed aqueous solution to NMP is 1:9; ⅶ. The concentration of fullerenol in the mixed solution is 0.5-2 mg / mL; VIII. Preferably, the concentration of fullerenol in the mixed solution is 1 mg / mL; ⅸ. The concentration of Ag6-NCs in the mixed solution is 3-8mmol / mL; ⅹ. Preferably, the concentration of Ag6-NCs in the mixed solution is 5 mmol / mL.

6. The preparation method according to claim 3, characterized in that: Includes one or more of the following conditions: ⅰ. After adding Ag6-NCs powder to the fullerol aqueous solution, vortex at room temperature for 1-5 minutes; after adding NMP, vortex at room temperature for 1-2 minutes; ii. The standing time is 2-3 days; ⅲ. The centrifugal speed is 7000-9000r / min, and the centrifugal time is 5-10min; ⅳ. The centrifugal speed is 8000r / min and the centrifugal time is 8min; v. The washing is performed at room temperature using a mixed solvent of water and NMP in a volume ratio of 1:9; ⅵ. Repeat the centrifugation and washing steps 2-3 times; ⅶ. The freeze-drying temperature is -50 to -70°C, and the freeze-drying time is 2 to 3 days.

7. A fullerol / silver nanocluster / PMMA film with nonlinear optical properties, prepared using the fullerol / silver nanocluster composite material with nonlinear optical properties as claimed in claim 1.

8. The method for preparing the fullerol / silver nanocluster / PMMA film having nonlinear optical properties according to claim 7, comprising the following steps: Dissolve polymethyl methacrylate (PMMA) in dichloromethane, and perform ultrasonic treatment to obtain a dichloromethane solution of PMMA; disperse the fullerol / silver nanocluster composite material in the dichloromethane solution of PMMA, mix evenly, and homogenize to obtain a dispersion; transfer the obtained dispersion to a watch glass, and let it stand at room temperature to form a film, thereby obtaining a fullerol / silver nanocluster / PMMA film.

9. The preparation method according to claim 8, characterized in that: Includes one or more of the following conditions: ⅰ. The mass of PMMA and the volume ratio of dichloromethane is 30-50 mg: 1 mL; ii. The relative molecular mass of the polymethyl methacrylate (PMMA) is 300,000-400,000; iii. Preferably, the relative molecular mass of the polymethyl methacrylate (PMMA) is 350,000; iv. The ultrasonic treatment time is 2-15 min; ⅴ. The mass ratio of the fullerol / silver nanocluster composite material to PMMA is 1:150-250; ⅵ. Further preferably, the mass ratio of the fullerol / silver nanocluster composite material to PMMA is 1:180-220; ⅶ. Most preferably, the mass ratio of the fullerol / silver nanocluster composite material to PMMA is 1:200; VIII. The homogenization is to homogenize the mixture of the fullerol / silver nanocluster composite material and the dichloromethane solution of PMMA through a homogenizer at room temperature for 3-5 minutes at a homogenization speed of 80-110 r / min; ⅸ. Film forming time is 10-24h.

10. Use of the fullerol / silver nanoclusters / PMMA film with nonlinear optical properties as claimed in claim 9 as an optical limiting material for laser protection.

Citation Information

Patent Citations

  • Screening and dehumidifying equipment for flour raw materials

    CN117282657A

  • Method for regulating and controlling nonlinear optical properties of reduced graphene oxide by Au (at) CdS and rGO-Au (at) CdS composite material