Vacuum electron beam seal welding composite blank and assembly process thereof
By designing a vacuum electron beam sealed composite billet with connected grooves in vacuum electron beam welding technology, and using seals to seal the gaps, the problem of metal waste caused by milling of the base material is solved, and the yield rate and market of the composite panel are improved. competitiveness.
Patent Information
- Application Number
- CN202410765109.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-01
AI Technical Summary
In existing vacuum electron beam welding technology, the base material requires a large amount of milling to meet precision requirements, resulting in metal waste and increased production costs, reducing the yield and market competitiveness of composite panels.
A vacuum electron beam sealing and welding composite billet is designed, including a substrate, a cover plate and a seal. By setting connected grooves on the substrate and performing spot welding fixation before vacuum electron beam welding, the seal is used to seal the gap and reduce the risk of damage. Milling processing requirements of base materials.
It improves the yield rate of composite panels, reduces manufacturing costs, and enhances the market competitiveness of products. The yield rate can be increased by 10%-15%.
Smart Images

Figure CN118720385A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite blank welding, in particular to a vacuum electron beam sealing and welding composite blank and a blank assembly process thereof. Background Art
[0002] With the emergence of new industries and new technologies, people's requirements for material properties are becoming increasingly stringent. In many cases, a single material can no longer meet the needs of special properties, so the study of various new composite materials has become an important development direction in the field of materials science. Layered metal composite plates are composite materials that are made of two or more layers of metal plates with different properties that are processed by special processes to achieve a strong metallurgical bond at the interface. Compared with a single metal, a layered metal composite plate combines the advantages of multiple metal components to obtain physical, chemical and mechanical properties that a single-layer metal material does not have, thereby having high strength, wear resistance, corrosion resistance, and excellent electrical and thermal conductivity. At present, metal composite plates are increasingly used in bridges, machinery, ships, offshore platforms, nuclear power plants, containers and other fields.
[0003] As an emerging composite steel plate manufacturing method, rolling composite method is increasingly being used in the production of various composite steel plates due to its advantages of low cost, low pollution, short delivery cycle, and mass industrial production. Rolling composite plates usually adopt two assembly methods: submerged arc welding or vacuum electron beam welding. Among them, electron beam assembly has become the preferred assembly method for high-end composite plate preparation due to its advantages such as high vacuum degree and high bonding strength. However, the electron beam assembly has a thin beam flow and a narrow weld, so the blank is required to have extremely high assembly accuracy, and the gap after assembly is ≤2mm to meet the welding requirements. For the base and cladding materials of the assembly, they themselves have certain unevenness and thickness differences with the same plate. It is difficult to meet the assembly accuracy by direct superposition without processing. Therefore, in order to meet the accuracy requirements, the usual practice is to perform a large amount of milling on the base and cladding materials to ensure the assembly accuracy of the assembly through machining. However, milling causes a large amount of metal to be cut and wasted, and consumes a large amount of milling cutter blades, which reduces production efficiency, increases production costs, and reduces product competitiveness. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the disadvantages of the prior art and provide a vacuum electron beam sealing and welding composite blank and a blank assembly process thereof.
[0005] In order to solve the above technical problems, the technical solution of the present invention is as follows: A vacuum electron beam sealing composite blank, comprising: There are two substrates, each of which has a rectangular cross section, and a groove is provided on the edge of any end surface of each substrate, and any two adjacent grooves are connected; There are two cover plates, the cross section of which is rectangular, and the two cover plates are respectively fixedly arranged on the end surfaces of the two substrates with grooves, and the centers of the cover plates and the substrates are aligned, and the end surfaces of the two cover plates away from the substrates are in contact with each other; A release agent is uniformly coated on the end surface of any cover plate away from the substrate; And, a sealing strip is fixedly disposed in the groove and seals the cover plate between the two substrates.
[0006] As a preferred solution of the vacuum electron beam sealing composite blank of the present invention, the widths of all the grooves are equal, and the depths of all the grooves are equal.
[0007] As a preferred solution of the vacuum electron beam sealing composite blank of the present invention, the length of the cover plate = the length of the substrate - the width of the groove * 2 - (5 ± 1) mm, and the width of the cover plate = the width of the substrate - the width of the groove * 2 - (5 ± 1) mm.
[0008] As a preferred solution of the vacuum electron beam sealing and welding composite blank of the present invention, the sealing strips include long side sealing strips arranged at the long side of the substrate and short side sealing strips arranged at the short side of the substrate; The length of the long side seal = the length of the substrate, the width of the long side seal = the width of the groove ± 2 mm, and the height of the long side seal = (groove depth * 2 + cover plate height * 2 + 5) ± 1 mm; The length of the short side seal = the width of the substrate - the width of the groove * 2 ± 2 mm, the width of the short side seal = the width of the groove ± 2 mm, and the height of the short side seal = (the depth of the groove * 2 + the height of the cover plate * 2 + 5) ± 1 mm.
[0009] As a preferred solution of the vacuum electron beam sealing and welding composite blank of the present invention, the sealing strip is made of non-alloy steel, and its carbon equivalent is less than or equal to 0.30.
[0010] As a preferred solution of the vacuum electron beam sealing composite blank of the present invention, the unevenness of the substrate is less than or equal to 20 mm.
[0011] As a preferred solution of the vacuum electron beam sealing and welding composite blank of the present invention, the straightness of the sealing strip is less than or equal to 2 mm / m, and the surface roughness of the sealing strip is less than or equal to 5 μm.
[0012] As a preferred solution of the vacuum electron beam sealing composite blank of the present invention, the thickness of the isolation agent is 0.3 mm-1 mm.
[0013] The present invention also provides a vacuum electron beam sealing and welding composite blank assembly process, comprising: Grinding the connection surface between the substrate and the cover plate to remove the oxide layer; spraying a release agent on the non-connected surface of the cladding plate; Aligning and fitting the non-connected surfaces of the two cover plates, and fixing them by spot welding, placing the connected cover plates on one of the base plates, and aligning the centers of the cover plates and the base plate, and then fixing them by spot welding; Place the seal strips in the corresponding grooves and assemble them so that the seal strips are attached to the substrate and two adjacent seal strips are attached, and then fix them by spot welding; Placing the other substrate on the connected cover plate, aligning the seal strip with the groove on the seal strip, and then spot welding to form a combined blank; The blank is fed into a vacuum electron beam welding machine, evacuated to a pressure of less than or equal to 0.1 Pa, and then welded.
[0014] As a preferred solution for the assembly process of the vacuum electron beam sealing composite billet described in the present invention, the welding process parameters are: voltage: 45-90KV, welding beam: 80-150mA, welding speed: 100-250mm / min, focusing mode adopts downward focusing, and welding depth is: 30-50mm.
[0015] The beneficial effects of the present invention are: The present invention solves the problem of low yield rate caused by large amount of metal waste due to milling of substrate in traditional method by specially designing composite blank for vacuum electron beam welding, so that the yield rate of composite board substrate can be increased by 10%-15%, which greatly reduces the manufacturing cost and improves the market competitiveness of composite board products. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.
[0017] Figure 1 A schematic cross-sectional view of the vacuum electron beam sealing composite blank provided by the present invention; Figure 2 A front view of a substrate in a vacuum electron beam sealing composite blank provided by the present invention; Figure 3 A schematic diagram of the process flow of the vacuum electron beam sealing and welding composite blank assembly process provided by the present invention; Among them: 1. Base plate; 2. Cover plate; 3. Isolation agent; 4. Seal; 5. Groove; 6. Weld. DETAILED DESCRIPTION
[0018] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific implementation modes and in combination with the accompanying drawings.
[0019] Figure 1 The cross-sectional schematic diagram of the vacuum electron beam sealing composite blank provided in the embodiment of the present application. The composite blank comprises two substrates 1, two cover plates 2, an isolation agent 3 and a sealing strip 4.
[0020] Specifically, the substrate 1 is a continuous casting billet or a steel plate, the unevenness of the entire substrate 1 is ≤20mm, and the surface is not milled. The cross section of each substrate 1 is rectangular. A groove 5 is provided on the edge of any end surface of each substrate 1. Figure 2 Each substrate 1 is provided with four grooves 5, each groove 5 is parallel to the side of the substrate 1, and any two adjacent grooves 5 are connected to each other. The four grooves 5 are connected in sequence to form a rectangular frame-shaped groove 5.
[0021] It should be noted that the widths of all the grooves 5 in the two substrates 1 are equal, and the depths of all the grooves 5 are also equal.
[0022] The covering material is a composite plate covering material such as stainless steel plate, titanium plate or copper plate. The cross section of the covering plate 2 is also rectangular. The two covering plates 2 are respectively fixedly connected to the end faces of the two substrates 1 with grooves 5. Among them, the length of the covering plate 2 = the length of the substrate 1 - the width of the groove 5 * 2-(5±1) mm, and the width of the covering plate 2 = the width of the substrate 1 - the width of the groove 5 * 2-(5±1) mm. The thickness of the covering plate 2 is 5-30 mm. When any covering plate 2 is fixedly connected to the substrate 1, the centers of the covering plate 2 and the substrate 1 are aligned, and the long side of the covering plate 2 is parallel to the long side of the substrate 1.
[0023] The seal 4 includes a long side seal 4 and a short side seal 4. The long side seal 4 is installed in the groove 5 at the long side of the substrate 1, and the short side seal 4 is installed in the groove 5 at the short side of the substrate 1. The length of the long side seal 4 is equal to the length of the substrate 1, the width of the long side seal 4 = the width of the groove 5 ± 2mm, and the height of the long side seal 4 = (the depth of the groove 5 * 2 + the height of the cover plate 2 * 2 + 5) ± 1mm. The length of the short side seal 4 = the width of the substrate 1 - the width of the groove 5 * 2 ± 2mm, the width of the short side seal 4 = the width of the groove 5 ± 2mm, and the height of the short side seal 4 = (the depth of the groove 5 * 2 + the height of the cover plate 2 * 2 + 5) ± 1mm.
[0024] It should be noted that the seal 4 is made of non-alloy steel such as Q235B and 20# steel which are easy to weld, and the carbon equivalent thereof is ≤0.30. The straightness of the seal 4 is ≤2mm / m, and the surface roughness of the seal 4 is ≤5μm.
[0025] See also Figure 1 The composite blank is stacked from top to bottom in the order of substrate 1-covering plate 2-covering plate 2-substrate 1, and the centers of all substrates 1 and covering plates 2 are aligned. A release agent 3 is evenly coated between the two covering plates 2. The thickness of the release agent 3 is 0.3mm-1mm.
[0026] See also Figure 3 The embodiment of the present application also provides a process for assembling a composite blank by vacuum electron beam sealing welding, the process comprising the following steps: Step S101: grinding the connection surface between the substrate 1 and the cover plate 2 to remove the oxide layer.
[0027] Step S102 : spraying a release agent 3 on the non-connected surface of the cover plate 2 .
[0028] Step S103: aligning and fitting the non-connected surfaces of the two cover plates 2, and fixing them by spot welding, placing the connected cover plates 2 on one of the substrates 1, and aligning the centers of the cover plates 2 and the substrate 1, and then fixing them by spot welding.
[0029] Step S104: placing the seal 4 in the corresponding groove 5 and assembling them so that the seal 4 and the substrate 1 are in contact with each other and two adjacent seals 4 are in contact with each other, and then spot welding them to fix them.
[0030] Step S105: placing another substrate 1 on the connected cover plate 2, and aligning and fitting the seal strip 4 with the groove 5 thereon, and then performing spot welding to fix, so as to form a combined blank.
[0031] Step S106: sending the blank into a vacuum electron beam welding machine, evacuating the vacuum to less than or equal to 0.1 Pa, and then welding.
[0032] The following takes a 20+3mm specification Q235B+304 stainless steel composite plate as an example to illustrate the above-mentioned vacuum electron beam sealing and welding composite blank assembly process.
[0033] (1) Material preparation The substrate 1 is made of Q235B steel plate and cut according to the design size of 100mm×2000mm×3000mm. After cutting, the groove 5 is machined to form a groove 5, the width of the groove 5 is 40mm, and the depth of the groove 5 is 20mm. The surface roughness of the groove 5 is controlled to be ≤12μm.
[0034] After measurement, the unevenness of the entire substrate 1 is 15 mm, and the unevenness does not need to be flattened.
[0035] Cut or weld the cladding material according to the size of substrate 1 to ensure that the size of cladding 2 meets the following requirements: The thickness of the covering plate 2 is 15 mm, the width of the covering plate 2 is 1915±1 mm, and the length of the covering plate 2 is 2915±1 mm.
[0036] Select 77mm Q235B non-alloy steel plate. Cut seal 4 from the steel plate and machine it to the following requirements: The straightness of the seal 4 is ≤2mm / m, and the surface roughness of the seal 4 is ≤5μm.
[0037] The length of the short side seal 4 = the length of the short side of the substrate 1 - the width of the groove 5 * 2±2mm = 1920±2mm, and the width of the short side seal 4 = the width of the groove 5 ±2mm = 20±2mm.
[0038] The length of the long side seal 4 = the length of the long side of the substrate 1 ± 5 mm = 3000 ± 5 mm, and the width of the long side seal 4 = the width of the groove 5 ± 2 mm = 20 ± 2 mm.
[0039] The height of the short side and long side seal strips 4 = (depth of groove 5 * 2 + height of cover plate 2 * 2 + 5mm) ± 1mm = 75 ± 1mm.
[0040] (2) Surface treatment The composite surface of the base plate 1 and the cover plate 2 is ground with a belt to remove the iron oxide scale and expose the fresh metal. The non-composite surface does not need to be treated. Compared with the traditional method, the surface of the base and cover materials does not need to be milled.
[0041] (3) Spraying of release agent 3 The release agent 3 is sprayed on the non-composite surface of the cover plate 2, and the release agent 3 is dried to ensure that no gas is released at high temperature.
[0042] (4) Assembly First, align the non-composite surfaces of the two cover plates 2 sprayed with the release agent 3, and fix the cover plates 2 by spot welding. Then, place the assembled cover plates 2 on a substrate 1, ensuring that the center of the cover plates 2 and the substrate 1 are aligned, and the edges of the cover plates 2 are parallel to the edges of the substrate 1. After placement, spot weld the bottom cover plate 2 and the substrate 1 to prevent the cover plates 2 from moving during assembly and lifting. The spot welding position needs to be polished clean and no welding slag should be present.
[0043] Place the edge seals 4 at the grooves 5 on the four sides of the substrate, and assemble them to ensure that the seals 4 fit the substrate 1 and the contact surfaces of two adjacent seals 4 fit well, and then fix them by spot welding. The gap between the seal 4 and the substrate 1 and the gap between the seals 4 and the seals 4 are ≤3mm.
[0044] Place another processed substrate 1 with the surface to be composited facing downward on the composite blank, ensure that the groove 5 and the seal 4 are well combined, and then fix them with spot welding.
[0045] (5) Electron beam welding The assembled blanks are sent into the vacuum electron beam welding machine, vacuumed to ≤0.1Pa, and then welding begins. The welding process is as follows: Voltage: 90KV, welding beam current: 100mA, welding speed 200mm / min, focusing mode adopts downward focusing. After welding, ensure that the welding depth reaches 40mm.
[0046] Welding sequence: first weld the fitting surfaces of two adjacent seals 4 to ensure that the seals 4 will not deform during the subsequent welding process, then weld the fitting surfaces of the two long side seals 4 and the upper and lower substrates, and finally weld the fitting surfaces of the short side seals 4 and the upper and lower substrates.
[0047] All gaps are welded and sealed by welding, so as to obtain welded composite billets with internal vacuum and good sealing. The composite billets have good composite effect and excellent performance after rolling. Compared with the traditional method, the yield rate is increased by 13%.
[0048] Therefore, the technical solution of the present application solves the problem of low yield rate caused by large amount of metal waste caused by milling of the substrate in the traditional method by designing a special blank for the composite blank for vacuum electron beam welding. By adopting the present invention, the yield rate of the composite board substrate can be increased by 10%-15%, which greatly reduces the manufacturing cost and improves the market competitiveness of the composite board product.
[0049] In addition to the above embodiments, the present invention may also have other implementation modes; any technical solutions formed by equivalent replacement or equivalent transformation shall fall within the protection scope required by the present invention.
Claims
1. A vacuum electron beam sealing composite blank, characterized in that: include: Two substrates (1) are provided, and their cross sections are rectangular; a groove (5) is provided on the edge of any end surface of each substrate (1), and any two adjacent grooves (5) are connected; Two cover plates (2) are provided, the cross section of the cover plates (2) is rectangular, the two cover plates (2) are respectively fixedly arranged on the end surfaces of the two substrates (1) provided with the grooves (5), and the centers of the cover plates (2) and the substrates (1) are aligned, and the end surfaces of the two cover plates (2) away from the substrates (1) are in contact with each other; A release agent (3) is evenly coated on the end surface of any of the cover plates (2) away from the substrate (1); And, a sealing strip (4) is fixedly arranged in the groove (5) and seals the cover plate (2) between the two substrates (1).
2. The vacuum electron beam sealing composite blank according to claim 1, characterized in that: The widths of all the grooves (5) are equal, and the depths of all the grooves (5) are equal.
3. The vacuum electron beam sealing composite blank according to claim 2, characterized in that: The length of the cover plate (2) = the length of the base plate (1) - the width of the groove (5) * 2 - (5 ± 1) mm, and the width of the cover plate (2) = the width of the base plate (1) - the width of the groove (5) * 2 - (5 ± 1) mm.
4. The vacuum electron beam sealing composite blank according to claim 2, characterized in that: The seal strip (4) comprises a long side seal strip (4) arranged at the long side of the substrate (1) and a short side seal strip (4) arranged at the short side of the substrate (1); The length of the long side seal (4) = the length of the substrate (1), the width of the long side seal (4) = the width of the groove (5) ± 2 mm, and the height of the long side seal (4) = (depth of the groove (5) * 2 + height of the cover plate (2) * 2 + 5) ± 1 mm; The length of the short edge seal (4) = the width of the substrate (1) - the width of the groove (5) * 2 ± 2 mm, the width of the short edge seal (4) = the width of the groove (5) ± 2 mm, and the height of the short edge seal (4) = (the depth of the groove (5) * 2 + the height of the cover plate (2) * 2 + 5) ± 1 mm.
5. The vacuum electron beam sealing composite blank according to claim 1, characterized in that: The seal (4) is made of non-alloy steel, and its carbon equivalent is less than or equal to 0.
30.
6. The vacuum electron beam sealing composite blank according to claim 1, characterized in that: The unevenness of the substrate (1) is less than or equal to 20 mm.
7. The vacuum electron beam sealing composite blank according to claim 1, characterized in that: The straightness of the seal (4) is less than or equal to 2 mm / m, and the surface roughness of the seal (4) is less than or equal to 5 μm.
8. The vacuum electron beam sealing composite blank according to claim 1, characterized in that: The thickness of the isolation agent (3) is 0.3 mm-1 mm.
9. A process for assembling a composite blank by vacuum electron beam sealing welding according to any one of claims 1 to 8, characterized in that: include: Grinding the connection surface between the substrate (1) and the cover plate (2) to remove the oxide layer; Spraying a release agent (3) on the non-connecting surface of the cover plate (2); Aligning and fitting the non-connected surfaces of the two cover plates (2) and fixing them by spot welding, placing the connected cover plates (2) on one of the base plates (1), aligning the centers of the cover plates (2) and the base plate (1), and then fixing them by spot welding; The seal strip (4) is placed in the corresponding groove (5), and they are assembled so that the seal strip (4) is in contact with the substrate (1), and two adjacent seal strips (4) are in contact with each other, and then they are fixed by spot welding; Placing the other substrate (1) on the connected cover plate (2), and aligning the seal strip (4) with the groove (5) thereon, and then spot welding and fixing them to form a combined blank; The blank is sent into a vacuum electron beam welding machine, evacuated to a pressure of less than or equal to 0.1 Pa, and then welded.
10. The vacuum electron beam sealing composite blank according to claim 9, characterized in that: The welding sequence is: welding process parameters are: voltage: 45-90KV, welding beam: 80-150mA, welding speed: 100-250mm / min, focusing method adopts down focusing, welding depth: 30-50mm.