Preformed aluminum part brazing material and preparation method and application thereof

By using aluminum powder and magnesium mesh to protect the structure of the copper oxide shell, combined with nickel powder, the overheating problem caused by the high melting point of the existing aluminum alloy connector brazing material is solved, and low-temperature brazing and high-strength connection are achieved. Reduces brazing energy consumption.

CN118720524AActive Publication Date: 2024-10-01SOLDERWELL MICROELECTRONIC PACKAGING MATERIALS CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411023336.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-01
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The melting point of the existing brazing materials for aluminum alloy connectors is relatively high, which results in the brazing temperature being close to the melting point of the aluminum alloy connectors, easily causing overheating damage, and high-temperature heating consumes a lot of energy and makes processing more difficult.

Method used

Aluminum powder with a copper oxide shell protective structure is used in combination with magnesium mesh, and nickel powder is introduced to mix. The magnesium mesh is ignited at a lower temperature to generate heat to trigger the thermite reaction, forming an intermetallic compound or solid solution to achieve brazing. Reduce brazing temperature and energy consumption.

Benefits of technology

Brazing is achieved at a lower temperature, which avoids overheating damage to aluminum alloy connectors, reduces brazing energy consumption, and improves brazing quality and shear strength of connectors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004967888130000121
    Figure BDA0004967888130000121
  • Figure BDA0004967888130000131
    Figure BDA0004967888130000131
Patent Text Reader

Abstract

The invention discloses a preformed aluminum piece brazing material and a preparation method and application thereof, and belongs to the technical field of brazing. Composite aluminum powder with a copper oxide shell protection structure and a magnesium net are combined for use, and meanwhile nickel powder is introduced for compounding; the heat generated by igniting the magnesium mesh during low-temperature heating can trigger the thermit reaction to release a large amount of heat, and the aluminum powder, the nickel powder and the copper generated by the thermit reaction are compounded under a large amount of heat to form an intermetallic compound or a solid solution, so that brazing is realized; when the product is used, the aluminum alloy connecting piece does not need to be damaged due to overheating caused by high brazing temperature, meanwhile, the energy consumption during brazing is low, and the brazing quality is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of brazing, and in particular to a preformed aluminum brazing material and a preparation method and application thereof. Background Art

[0002] Aluminum alloys are often used in metal connectors because of their good thermal conductivity, electrical conductivity and corrosion resistance. When preparing connectors, brazing is required. This is a method of heating a brazing material with a melting point lower than that of the connector together with the connector until the brazing material melts, and the molten material quickly fills the gap of the connector to achieve interconnection. The main brazing material for aluminum alloy connectors currently used is aluminum silicon brazing material, but its melting point reaches 577°C. If brazing is to be performed, a brazing temperature of at least 600°C is required, which is very close to the melting point of the aluminum alloy connector. If the temperature is unstable during brazing, it is very easy to cause overheating and damage to the aluminum alloy connector. Additional processes or equipment are required to accurately control the heating temperature, which increases the difficulty of processing, and the energy consumption at such a high temperature is also high. Summary of the invention

[0003] Based on the defects of the prior art, the purpose of the present invention is to provide a preformed aluminum brazing material, which is provided by arranging aluminum powder and magnesium mesh with a copper oxide shell protection structure, and introducing nickel powder for compounding. When heated at a relatively low temperature, the heat generated by the magnesium mesh can be ignited to induce an aluminothermic reaction to release a large amount of heat. The aluminum powder, nickel powder and copper generated by the aluminothermic reaction are compounded under a large amount of heat to form an intermetallic compound or a solid solution to achieve brazing. When using this product, there is no need to worry about overheating and damage of the aluminum alloy connector due to the high brazing temperature. At the same time, the energy consumption during brazing is low and the brazing quality is good.

[0004] In order to achieve the above object, the technical solution adopted by the present invention is:

[0005] A preformed aluminum brazing material, comprising a magnesium mesh and a mixed material filled on the surface and pores of the magnesium mesh;

[0006] The mixed material comprises composite aluminum powder, nickel powder and aluminum brazing flux;

[0007] The composite aluminum powder comprises a core and a shell from the inside to the outside, the core comprises aluminum, and the shell comprises copper oxide.

[0008] The melting point of common aluminum brazing materials is relatively high, and the brazing temperature is very close to the melting point of aluminum alloy connectors. If the temperature is not properly controlled, it is very easy to cause the connectors to melt or even be damaged. For this reason, people consider adding aluminum powder and other powders that can produce aluminothermic reactions with aluminum powder to the brazing materials, and releasing a large amount of heat through the thermite reaction at a lower brazing temperature to achieve brazing. However, aluminum powder itself is extremely easy to age and deactivate, and the rate at which the heat is released by the thermite reaction is extremely fast. It is easy to locally concentrate a large amount of heat in a short period of time, causing overburning, thereby affecting the quality of brazing. In the technical solution of the present invention, the preformed aluminum brazing material uses magnesium mesh as a skeleton structure material, and its pores and surface are filled with a mixture with brazing function, the mixture contains aluminum powder with a core-shell structure, nickel powder and aluminum brazing flux, and the aging and deactivation probability of the aluminum powder in the inner core is significantly reduced by coating with a copper oxide shell. When heated, due to the low ignition point of the magnesium mesh, it only needs to be ignited at less than 500°C, and the heat generated by it will promote the thermite reaction, and the copper oxide shell will slow down the heat release rate of the thermite reaction at this time, so that it can release heat at a relatively uniform rate to avoid overburning, and during the thermite reaction, the heat released by the thermite reaction further causes a part of the aluminum to form an intermetallic compound or solid solution with the nickel powder and the copper generated by the thermite reaction, and this substance can be directly used as a brazing material to achieve the purpose of brazing; at the same time, the aluminum brazing flux can increase the activity of the aluminum powder, break the oxide film on the surface of the connector during brazing, and push the generated oxide slag to the vicinity of the weld during brazing, thereby ultimately improving the quality of brazing. When the preformed aluminum brazing material of the present invention is used for brazing, not only can low heating energy consumption and low heating temperature be ensured, there is no need to worry about overheating loss of the connecting parts, but also the shear strength of the connecting parts after brazing is high and the brazing quality is excellent. However, if the aluminum powder of the core-shell structure is not constructed, or other powders such as cobalt are used instead of nickel powder, the above effects cannot be achieved, or the brazing temperature is high and easily causes the risk of overheating damage, or the brazing quality is poor, and the obtained aluminum parts after brazing cannot meet the use requirements.

[0009] Preferably, the mass content of the magnesium mesh in the preformed aluminum brazing material is 6-8%.

[0010] More preferably, in the preformed aluminum brazing material, the mass content of the magnesium mesh is 6.2-7.4%.

[0011] The inventors noticed that the main function of magnesium is to provide initial initiation heat for thermite reaction, but its addition amount cannot be too much, otherwise it is impossible to form sufficient intermetallic compounds and solid solutions for brazing. If it is introduced in the form of conventional powder, the product prepared at the same addition ratio and without introducing other combustion aids has poor dispersibility, low air circulation and is not easy to ignite. Even if the temperature is increased, it may only be partially ignited. If other combustion aids are introduced, it is likely to cause overburning of the brazing, affecting the quality of the brazing. For this reason, a network structure of magnesium is used as the skeleton support of the brazing functional mixture, and this form of product has the best effect.

[0012] Preferably, the ratio of the average diameter of the inner core of the composite aluminum powder to the thickness of the shell is (5-20):1.

[0013] More preferably, the ratio of the average diameter of the core of the composite aluminum powder to the thickness of the shell is (5-18): 1

[0014] The role of copper oxide is to prevent the aging of aluminum powder and slow down the heat release rate of thermite reaction. At the same time, the copper generated by the reaction of aluminum powder and copper oxide will form a solid solution with nickel powder, and the excess aluminum powder will also form an intermetallic compound with nickel powder. Therefore, when setting the composite aluminum powder, the larger the diameter of the inner core, that is, the higher the proportion of aluminum content in the composite aluminum powder, the more beneficial it is to the brazing effect of the product. However, if the coating thickness of copper oxide is too small, it will lead to insufficient heat of thermite reaction or too fast heat release rate, which is not conducive to the brazing quality. On the other hand, if the proportion of copper oxide is too large and the thickness of the coating shell is too large, based on the limitation of surface tension, the adhesion of the shell to the inner core is reduced, and it is very easy to fall off during processing and brazing, weakening its protective effect. Therefore, the thickness ratio of the inner core and the shell needs to be adapted. When the above-mentioned moderate ratio range is preferably selected, the product further prepared by the composite aluminum powder has a better brazing effect.

[0015] More preferably, the average diameter of the core in the composite aluminum powder is 10 to 45 μm;

[0016] More preferably, the average diameter of the inner core is in the range of one or any two of 10 μm, 15 μm, 18 μm, 20 μm, 22 μm, 25 μm, 28 μm, 30 μm, 32 μm, 36 μm, 38 μm, 40 μm, 42 μm, and 45 μm.

[0017] The inner core is the key structure for the composite aluminum powder to undergo thermite reaction and ultimately achieve brazing. The smaller its diameter is, the larger the specific surface area of ​​the overall particle is when the thickness ratio of the inner and outer layers is constant, the higher the probability of aluminum aging in the inner core is, and it is easy to reduce the coating uniformity during the shell coating process; but if the diameter is too large, the relative melting point of the overall particle is too high, which will be detrimental to the full conduct of thermite reaction and the mutual contact of the materials forming intermetallic compounds or solid solutions, so it needs to be maintained within a moderate range.

[0018] Preferably, the preformed aluminum brazing material meets the following requirements:

[0019] (M1-9M2 / 40):M3=(5~16):1;

[0020] Wherein, M1 is the mass of aluminum in the core of the composite aluminum powder, M2 is the mass of copper oxide in the shell of the composite aluminum powder, M3 is the mass of nickel powder, and the units of M1, M2 and M3 are the same.

[0021] More preferably, the preformed aluminum brazing material satisfies:

[0022] (M1-9M2 / 40): M3=(6~10):1.

[0023] The introduction of nickel powder can improve the overall brazing effect, making the strength of the brazed product higher, and it will mainly react with the copper generated after the thermite reaction and the remaining aluminum. Therefore, it is necessary to build a suitable addition ratio with the two in the composite aluminum powder, and the amount added cannot be too small, otherwise the brazing effect will be weakened. On the other hand, the melting point of nickel powder itself is relatively high. If the addition ratio is too much, it is very easy to cause part of the nickel powder to fail to melt under the same heat release, which will also weaken the brazing effect and cause the brazing temperature of the product to be too high. When the ratio of the three materials is maintained within the above preferred range, the nickel powder can fully react with the composite aluminum powder and achieve a better brazing effect.

[0024] More preferably, the mass content of nickel powder in the preformed aluminum brazing material is 1 to 8.4%.

[0025] Preferably, the average particle size of the nickel powder is 200 to 1200 nm;

[0026] More preferably, the average particle size of the nickel powder is 200 to 1000 nm;

[0027] More preferably, the average particle size of the nickel powder is within the range of one or any two of 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, and 1000 nm.

[0028] The inventors have found through experiments that when nickel powder is heated and reacts with copper or aluminum, its heating uniformity and reaction degree are related to the average particle size of the nickel powder. When the average particle size of the nickel powder is larger, its dispersibility becomes lower, and the uniformity of heating and the uniformity of the subsequently formed intermetallic compounds and solid solutions are also reduced, the temperature required for brazing increases and the strength of the product after brazing decreases; however, the smaller the particle size of the nickel powder, the larger the specific surface area, the easier it is to oxidize, and the powder making cost is also high; therefore, when the average particle size of the nickel powder is preferably within the above range, the brazing temperature and the strength of the obtained product after brazing can be maintained at a better level.

[0029] Preferably, the magnesium mesh is a two-dimensional magnesium mesh or a three-dimensional magnesium mesh.

[0030] It should be noted that the magnesium mesh described in the present invention can be a two-dimensional plane or a three-dimensional magnesium mesh, such as a sponge. As mentioned above, the main function of the magnesium mesh is to provide heat for the thermite reaction, and at the same time requires sufficient ignition space and a lower mass occupancy ratio. Those skilled in the art can easily think that the magnesium mesh can meet the above effects in the case of a two-dimensional or three-dimensional structure, and the magnesium mesh can be directly applied as a commercially available product, or a homemade product can be used, such as a magnesium foil or a magnesium block is hollowed out by laser etching or chemical etching with or without a mold to obtain a two-dimensional or three-dimensional mesh structure.

[0031] More preferably, the magnesium mesh is a two-dimensional magnesium mesh with a thickness of 0.1 to 0.5 mm.

[0032] Preferably, the porosity of the magnesium mesh is 60-90%.

[0033] More preferably, the porosity of the magnesium mesh is 70-85%.

[0034] The porosity of the magnesium mesh is related to the relative content of magnesium, the ventilation degree of the magnesium mesh, the degree of integration of the magnesium mesh and the mixture, and even the difficulty of processing the product during preparation and use. When the porosity is small, the mixture cannot be fully filled in the pores of the magnesium mesh, and the ventilation degree is low, and it cannot be fully burned when ignited. In addition, the relative content of magnesium is relatively high, which leads to less truly feasible brazing materials. However, if the porosity is too large, the processing difficulty of the product will increase, and the magnesium mesh will easily tear during the processing, which will lead to lower compounding and reaction uniformity of the mixture. At the same time, the relative content of magnesium is small, and it cannot provide sufficient initiation heat for the thermite reaction, requiring a higher brazing temperature. When a magnesium mesh with a porosity in the above preferred range is selected, it can exert the optimal use and skeleton support function.

[0035] Preferably, the aluminum brazing flux is a fluoroaluminate aluminum brazing flux.

[0036] More preferably, the aluminum brazing flux is cesium aluminum fluoroaluminate brazing flux.

[0037] More preferably, the mass content of the aluminum brazing agent in the preformed aluminum part brazing material is 5-15%.

[0038] The main function of aluminum brazing flux is to remove the oxide film on the surface of aluminum parts, but introducing too much will not further improve the brazing quality of the product. Instead, it will cause too much aluminum brazing flux to remain after brazing. Therefore, it is sufficient to compound it with an appropriate addition amount.

[0039] Another object of the present invention is to provide a method for preparing the preformed aluminum brazing material, comprising the following steps:

[0040] (1) mixing micron aluminum powder and nano copper oxide powder in an organic solvent to prepare a slurry, followed by spray granulation and drying to obtain a composite aluminum powder with a core-shell structure;

[0041] (2) The composite aluminum powder, nickel powder and aluminum brazing agent are mixed in an organic solvent to form a paste slurry, which is then applied on a magnesium mesh, left to stand, dried, cured and cut to obtain the preformed aluminum brazing material.

[0042] In the preparation method of the product of the present invention, a slurry containing aluminum powder and copper oxide powder is granulated by spray drying. Due to the Wentworth effect, the aluminum powder in the slurry will form highly dispersible small particles under the high shear force of the airflow during spraying. The nano copper oxide powder has a large specific surface area and a large surface tension, so it will spontaneously adsorb on the surface of the aluminum particles to finally form a composite aluminum powder with a core-shell structure. Subsequently, the composite aluminum powder and raw materials such as nickel powder are directly attached to the magnesium mesh and penetrate into the magnesium mesh by direct coating. After drying and curing, the product can be obtained. The preparation method of the product is simple to operate, so it can be produced on an industrial scale.

[0043] Another object of the present invention is to provide application of the preformed aluminum brazing material in aluminum brazing.

[0044] The beneficial effect of the present invention is that the present invention provides a preformed aluminum brazing material, which is used in combination with aluminum powder and magnesium mesh having a copper oxide shell protection structure, and nickel powder is introduced for compounding. When heated at a relatively low temperature, the heat generated by the magnesium mesh can be ignited to initiate an aluminothermic reaction to release a large amount of heat, and the aluminum powder, nickel powder and copper generated by the aluminothermic reaction are compounded under a large amount of heat to form an intermetallic compound or a solid solution to achieve brazing. When using the product, there is no need to worry about overheating and damage of the aluminum alloy connector due to the high brazing temperature. At the same time, the energy consumption during brazing is low and the brazing quality is good. DETAILED DESCRIPTION

[0045] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention, unless otherwise specified, are all commonly used common reagents and instruments.

[0046] Example 1

[0047] An embodiment of a preformed aluminum brazing material and a preparation method and application thereof according to the present invention, wherein the preparation method of the preformed aluminum brazing material comprises the following steps:

[0048] (1) 130 g of aluminum powder with an average particle size of 45 μm and 260 g of copper oxide powder with an average particle size of 60 nm are mixed in 90 g of an organic solvent to form a slurry, and the mixture is sprayed and granulated at a flow rate of 1.9 mL / s in a spray granulator, and dried to obtain a composite aluminum powder having a core and a shell, wherein the average diameter of the core in the composite aluminum powder is 45 μm, and the ratio of the average diameter of the core to the thickness of the shell is 9:1; the organic solvent is a mixed solution obtained by mixing ethyl cellulose, povidone, and isopropyl alcohol in a mass ratio of 4:4:2;

[0049] (2) A magnesium foil with a thickness of 0.2 mm is etched with holes by chemical etching to obtain a magnesium mesh with a porosity of about 80%;

[0050] (3) 195 g of composite aluminum powder, 6 g of nickel powder with an average particle size of 200 nm, 11.3 g of cesium aluminum fluoroaluminate brazing flux and 24 g of anhydrous ethanol were mixed to prepare a paste slurry, which was then applied on the magnesium mesh (mass: 15.3 g) obtained in step (2), allowed to stand for 5 min, dried and solidified by hot air drying at 80° C., and finally cut into a size of 16*16*0.2 mm to obtain the preformed aluminum brazing material; the mass content of the magnesium mesh in the product was 6.7%, the mass content of the nickel powder was 2.6%, and the mass content of the cesium aluminum fluoroaluminate brazing flux was 5%;

[0051] The preformed aluminum brazing material meets the following requirements:

[0052] (M1-9M2 / 40):M3=6:1;

[0053] Wherein, M1 is the mass of aluminum in the core of the composite aluminum powder, M2 is the mass of copper oxide in the shell of the composite aluminum powder, and M3 is the mass of nickel powder.

[0054] Example 2

[0055] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof described in the present invention is different from Example 1 only in that the addition amount of the copper oxide powder is adjusted to 554.2 g, and the ratio of the average diameter of the inner core of the obtained composite aluminum powder to the thickness of the shell is 5:1.

[0056] Example 3

[0057] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof described in the present invention differs from Embodiment 1 only in that the addition amount of the copper oxide powder is adjusted to 186.8 g, and the ratio of the average diameter of the inner core of the obtained composite aluminum powder to the thickness of the shell is 12:1.

[0058] Example 4

[0059] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof described in the present invention is different from Example 1 only in that the addition amount of the copper oxide powder is adjusted to 144.8 g, and the ratio of the average diameter of the inner core of the obtained composite aluminum powder to the thickness of the shell is 15:1.

[0060] Example 5

[0061] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof described in the present invention is different from Example 1 only in that the addition amount of the copper oxide powder is adjusted to 118 g, and the ratio of the average diameter of the inner core of the obtained composite aluminum powder to the thickness of the shell is 18:1.

[0062] Example 6

[0063] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof described in the present invention is different from Example 1 only in that the addition amount of the copper oxide powder is adjusted to 105.2 g, and the ratio of the average diameter of the inner core of the obtained composite aluminum powder to the thickness of the shell is 20:1.

[0064] Example 7

[0065] An embodiment of a preformed aluminum brazing material and a preparation method and application thereof according to the present invention is different from Embodiment 1 only in that the amount of nickel powder added is 5.1 g, the mass content of nickel powder in the product is 2.3%, and the preformed aluminum brazing material meets the following requirements:

[0066] (M1-9M2 / 40):M3=7:1.

[0067] Example 8

[0068] An embodiment of a preformed aluminum brazing material and a preparation method and application thereof according to the present invention is different from Embodiment 1 only in that the amount of nickel powder added is 4 g, the mass content of nickel powder in the product is 1.8%, and the preformed aluminum brazing material meets the following requirements:

[0069] (M1-9M2 / 40):M3=9:1.

[0070] Example 9

[0071] An embodiment of a preformed aluminum brazing material and a preparation method and application thereof according to the present invention is different from Embodiment 1 only in that the amount of nickel powder added is 3.6 g, the mass content of nickel powder in the product is 1.6%, and the preformed aluminum brazing material meets the following requirements:

[0072] (M1-9M2 / 40):M3=10:1.

[0073] Example 10

[0074] An embodiment of a preformed aluminum brazing material and a preparation method and application thereof according to the present invention is different from Embodiment 1 only in that the amount of nickel powder added is 7.2 g, the mass content of nickel powder in the product is 3.2%, and the preformed aluminum brazing material meets the following requirements:

[0075] (M1-9M2 / 40):M3=5:1.

[0076] Embodiment 11

[0077] An embodiment of a preformed aluminum brazing material and a preparation method and application thereof according to the present invention is different from Embodiment 1 only in that the amount of nickel powder added is 2.2 g, the mass content of nickel powder in the product is 1%, and the preformed aluminum brazing material meets the following requirements:

[0078] (M1-9M2 / 40):M3=16:1.

[0079] Example 12

[0080] An embodiment of a preformed aluminum brazing material and a preparation method and application thereof described in the present invention is different from Embodiment 1 only in that the average particle size of the nickel powder is 400 nm.

[0081] Embodiment 13

[0082] An embodiment of a preformed aluminum brazing material and a preparation method and application thereof described in the present invention is different from Embodiment 1 only in that the average particle size of the nickel powder is 600 nm.

[0083] Embodiment 14

[0084] An embodiment of a preformed aluminum brazing material and a preparation method and application thereof described in the present invention is different from Embodiment 1 only in that the average particle size of the nickel powder is 800 nm.

[0085] Embodiment 15

[0086] An embodiment of a preformed aluminum brazing material and a preparation method and application thereof described in the present invention is different from Embodiment 1 only in that the average particle size of the nickel powder is 1200 nm.

[0087] Example 16

[0088] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof described in the present invention is different from Embodiment 1 only in that the etching degree of the magnesium mesh is adjusted so that the porosity of the magnesium mesh is about 70%, and the mass content of the magnesium mesh in the product is 7.4%.

[0089] Embodiment 17

[0090] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof described in the present invention is different from Embodiment 1 only in that the etching degree of the magnesium mesh is adjusted so that the porosity of the magnesium mesh is about 75%, and the mass content of the magnesium mesh in the product is 7.1%.

[0091] Embodiment 18

[0092] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof described in the present invention is different from Embodiment 1 only in that the etching degree of the magnesium mesh is adjusted so that the porosity of the magnesium mesh is about 85%, and the mass content of the magnesium mesh in the product is 6.2%.

[0093] Embodiment 19

[0094] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof described in the present invention is different from Embodiment 1 only in that the etching degree of the magnesium mesh is adjusted so that the porosity of the magnesium mesh is about 60%, and the mass content of the magnesium mesh in the product is 8%.

[0095] Embodiment 20

[0096] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof described in the present invention is different from Embodiment 1 only in that the etching degree of the magnesium mesh is adjusted so that the porosity of the magnesium mesh is about 90%, and the mass content of the magnesium mesh in the product is 6%.

[0097] Embodiment 21

[0098] An embodiment of a preformed aluminum brazing material and a preparation method and application thereof according to the present invention, wherein the preparation method of the preformed aluminum brazing material comprises the following steps:

[0099] (1) 140 g of aluminum powder with an average particle size of 10 μm and 250 g of copper oxide powder with an average particle size of 60 nm were mixed in 90 g of an organic solvent to form a slurry, and the mixture was sprayed and granulated at a flow rate of 2.3 mL / s in a spray granulator, and dried to obtain a composite aluminum powder, wherein the average diameter of the core of the composite aluminum powder was 10 μm, and the ratio of the average diameter of the core to the thickness of the shell was 10:1; the organic solvent was a mixed solution obtained by mixing ethyl cellulose, povidone, and isopropyl alcohol in a mass ratio of 7:5:3;

[0100] (2) A magnesium foil with a thickness of 0.2 mm is etched with holes by chemical etching to obtain a magnesium mesh with a porosity of about 80%;

[0101] (3) 195 g of composite aluminum powder, 7 g of nickel powder with an average particle size of 200 nm, 11.3 g of cesium aluminum fluoroaluminate brazing flux and 24 g of anhydrous ethanol were mixed to prepare a paste slurry, which was then applied on the magnesium mesh (mass 15.3 g) obtained in step (2), allowed to stand for 5 min, dried and solidified by hot air drying at 80° C., and finally cut into a size of 16*16*0.2 mm to obtain the preformed aluminum brazing material; the mass content of the magnesium mesh in the product was 6.7%, the content of the nickel powder was 3%; the mass content of the cesium aluminum fluoroaluminate brazing flux was 5%;

[0102] The preformed aluminum brazing material meets the following requirements:

[0103] (M1-9M2 / 40):M3=6:1.

[0104] Embodiment 22

[0105] An embodiment of a preformed aluminum brazing material and a preparation method and application thereof according to the present invention, wherein the preparation method of the preformed aluminum brazing material comprises the following steps:

[0106] (1) 264 g of aluminum powder with an average particle size of 36 μm and 114 g of copper oxide powder with an average particle size of 60 nm were mixed in 90 g of an organic solvent to form a slurry, and the mixture was sprayed and granulated at a flow rate of 3.1 mL / s in a spray granulator, and dried to obtain a composite aluminum powder, wherein the average diameter of the core of the composite aluminum powder was 36 μm, and the ratio of the average diameter of the core to the thickness of the shell was 18:1; the organic solvent was a mixed solution obtained by mixing ethyl cellulose, povidone, and isopropyl alcohol in a mass ratio of 3:5:2;

[0107] (2) A magnesium foil with a thickness of 0.2 mm is etched with holes by chemical etching to obtain a magnesium mesh with a porosity of about 80%;

[0108] (3) 189 g of composite aluminum powder, 19.9 g of nickel powder with an average particle size of 200 nm, 11.8 g of cesium aluminum fluoroaluminate brazing flux and 24 g of anhydrous ethanol were mixed to prepare a paste slurry, which was then applied on the magnesium mesh (mass 15.3 g) obtained in step (2), allowed to stand for 5 min, dried and solidified with hot air at 80° C., and finally cut into a size of 16*16*0.2 mm to obtain the preformed aluminum brazing material; the mass content of the magnesium mesh in the product was 6.5%, the content of the nickel powder was 8.4%, and the mass content of the cesium aluminum fluoroaluminate brazing flux was 5%;

[0109] The preformed aluminum brazing material meets the following requirements:

[0110] (M1-9M2 / 40):M3=6:1.

[0111] Embodiment 23

[0112] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof described in the present invention is different from Embodiment 1 only in that the added amount of the cesium aluminum fluoroaluminate brazing flux is 38.2 g, and the mass content of the preformed aluminum brazing material is 15%.

[0113] Embodiment 24

[0114] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof described in the present invention is different from Embodiment 1 only in that the added amount of the cesium aluminum fluoroaluminate brazing flux is 4.4 g, and the mass content of the preformed aluminum brazing material is 2%.

[0115] Embodiment 25

[0116] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof described in the present invention is different from Embodiment 1 only in that the added amount of the cesium aluminum fluoroaluminate brazing flux is 72.1 g, and the mass content of the preformed aluminum brazing material is 25%.

[0117] Embodiment 26

[0118] An embodiment of a preformed aluminum brazing material, a preparation method thereof, and an application thereof described in the present invention is different from Embodiment 1 only in that the cesium aluminum fluoroaluminate brazing flux is replaced with an equal mass of potassium aluminum fluoroaluminate brazing flux.

[0119] Comparative Example 1

[0120] An embodiment of a preformed aluminum brazing material, a preparation method thereof, and an application thereof, the difference from embodiment 1 being that the nickel powder is replaced by cobalt powder of the same size and quality.

[0121] Comparative Example 2

[0122] An embodiment of a preformed aluminum brazing material, a preparation method thereof, and an application thereof is different from Embodiment 1 only in that the magnesium mesh is replaced by a tin mesh with the same porosity.

[0123] Comparative Example 3

[0124] An embodiment of a preformed aluminum brazing material, a preparation method and an application thereof, the difference from embodiment 1 is that the composite aluminum powder is replaced by 65g of aluminum powder with an average particle size of 45μm and 130g of copper oxide powder with an average particle size of 60nm.

[0125] Comparative Example 4

[0126] A preformed aluminum brazing material, a preparation method and an application thereof are disclosed in an embodiment, which differs from embodiment 1 only in that the preformed aluminum brazing material is a commercially available Al88Si12 (mass ratio Al:Si=88:12) brazing material, and is cut into samples of the same size as embodiment 1, 16*16*0.2mm, and 5% cesium aluminum fluoroaluminate brazing flux is coated on the surface.

[0127] Effect example

[0128] In order to verify the use effect of the preformed aluminum brazing material of the present invention, the brazing test was carried out on the products of each embodiment and comparative example:

[0129] Two 6061 aluminum parts to be brazed were assembled with the brazing materials of the embodiments and comparative examples (the brazing material was sandwiched between the parts to be brazed of the two aluminum parts), and laser brazing was performed, wherein the size of the brazing material was 16*16*0.2mm, and the area of ​​the part to be overlapped and brazed was also 16mm*16mm, and the following tests were performed:

[0130] 1) Record the temperature required for brazing. The temperature required for brazing is measured with an infrared temperature detector. The lower the temperature, the less likely the aluminum parts will be burned and the more energy-saving it is. The test results are shown in Table 1.

[0131] 2) After brazing, the shear strength of the overlapped brazed parts was tested by an electronic universal testing machine. The greater the shear strength, the better the brazing strength. The test results are shown in Table 1.

[0132] The performance test results are shown in Table 1.

[0133] Table 1 Performance test results

[0134]

[0135]

[0136] It can be seen from the test results that the preformed aluminum brazing material of the present invention has excellent use effect. When brazing, the brazing temperature is low and can be carried out below 570°C. At the same time, the shear strength of the aluminum part after brazing is high, which can reach more than 80MPa, and the highest can reach more than 108MPa. The cost performance is far better than the existing aluminum-silicon brazing material described in Comparative Example 4. The main reason why the product of the present invention can obtain the above performance is that the magnesium mesh structure and design and the composite use of composite aluminum powder and nickel powder are based on the low external temperature to ignite the magnesium mesh, and the heat released by igniting the magnesium mesh triggers the aluminothermic reaction. The heat released by the aluminothermic reaction causes each material to form an intermetallic compound or solid solution to achieve brazing. If, as shown in Comparative Examples 1 to 3, the nickel powder is replaced with cobalt powder, the magnesium mesh is replaced with a tin mesh, or the aluminum powder and copper oxide powder are introduced as raw materials without constructing a core-shell structure, the product not only cannot guarantee a low brazing temperature, but also has a low brazing strength even if the brazing is completed.

[0137] It can be seen from Examples 1 to 6 that in the composite aluminum powder of the present invention, since the core aluminum powder and the shell copper oxide powder are highly correlated and their interactions are relatively complex, it is necessary to take into account the degree of reaction of the thermite reaction, the rate of heat release, and the reaction probability of the intermetallic compound and the solid solution after the thermite reaction. If the content of any one of them is relatively low, the brazing temperature of the product will be relatively high and the shear strength after brazing will be relatively low. The thickness of the core and the shell needs to be maintained at a moderate ratio.

[0138] It can be seen from Example 1 and Examples 7 to 11 that when nickel powder is compounded with composite aluminum powder, the addition ratio thereof needs to be maintained at an appropriate level with the composite aluminum powder. Otherwise, due to the high melting point of nickel powder and the fact that it is a key raw material for forming a brazing layer after thermite reaction, when the preformed aluminum brazing material satisfies the following conditions: the mass content of nickel powder is 1 to 8.4%, and within the preferred range of (M1-9M2 / 40): M3 = (6 to 10): 1, the product can be used at a lower brazing temperature and the aluminum brazing layer can obtain a higher shear strength.

[0139] The particle sizes of the nickel powder used in Example 1 and Examples 12 to 15 are not the same. It can be seen that as the particle size increases, the brazing temperature of the product gradually increases, indicating that it requires more heat to melt and react with the aluminum powder and copper powder. At the same time, the shear strength of the brazing layer gradually decreases, so it is necessary to maintain the nickel powder size at a lower level.

[0140] It can be seen from Examples 1 and 16 to 20 that as the porosity of the magnesium mesh increases, the subsequent reaction effect triggered after ignition is better, and the shear strength of the product after brazing is improved, but the required brazing temperature is also increased. If the porosity is too large, the brazing temperature continues to increase. For example, in the product described in Example 21, the magnesium mesh is not strong enough due to the excessive porosity, and the magnesium mesh will be partially torn, which not only increases the difficulty of processing, but also reduces the composite and reaction uniformity with the mixture, and the shear strength of the product after brazing will be reduced. Therefore, when the preferred porosity is 70 to 85%, the use effect of the obtained product is the best. The greater the porosity of the magnesium mesh, the lower the mass content of the magnesium mesh in the preformed aluminum brazing material. When the mass content of the magnesium mesh in the preformed aluminum brazing material is preferably 6.2 to 7.4%, the use effect of the obtained product is the best.

[0141] It can be seen from Examples 21 and 22 that there is no specific restriction on the size of the inner core aluminum powder when constructing the composite aluminum powder in the product of the present invention. Aluminum powders of other sizes can be used. Even the composite aluminum powder prepared using smaller aluminum powder has better dispersibility. When other conditions are not much different, the product has higher performance.

[0142] It can be seen from Example 1 and Examples 23 to 26 that different amounts of aluminum brazing agents added and types of use have a certain influence on the brazing temperature and brazing effect of the product. The main reason is that the main function of the aluminum brazing agent is to break the oxide film on the surface of the aluminum part, push the oxide slag produced during brazing to the edge of the brazing layer, and activate the composite aluminum powder at the same time. If the aluminum brazing agent content is too little, it will inevitably lead to poor product use effect and reduced shear strength; but if too much aluminum brazing agent is added, as shown in Example 25, not only is the shear strength of the aluminum part after brazing limited, but due to excessive aluminum brazing agent residue, the appearance of the product is deteriorated, and the brazing agent may remain in the brazing layer, which reduces the shear strength. Therefore, in the preformed aluminum brazing material, the mass content of the aluminum brazing agent is preferably 5-15%, and the brazing effect is best.

[0143] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A preformed aluminum brazing material, characterized in that: It includes a magnesium mesh and a mixed material filled on the surface and pores of the magnesium mesh; The mixed material comprises composite aluminum powder, nickel powder and aluminum brazing flux; The composite aluminum powder comprises a core and a shell from the inside to the outside, the core comprises aluminum, and the shell comprises copper oxide.

2. The preformed aluminum brazing material according to claim 1, characterized in that: The mass content of the magnesium mesh in the preformed aluminum brazing material is 6-8%; preferably, the mass content of the magnesium mesh in the preformed aluminum brazing material is 6.2-7.4%.

3. The preformed aluminum brazing material according to claim 1, characterized in that: The ratio of the average diameter of the core of the composite aluminum powder to the thickness of the shell is (5-20):1; preferably, the ratio of the average diameter of the core of the composite aluminum powder to the thickness of the shell is (5-18):

1.

4. The preformed aluminum brazing material according to claim 3, characterized in that: The average diameter of the inner core of the composite aluminum powder is 10 to 45 μm.

5. The preformed aluminum brazing material according to claim 1, characterized in that: The preformed aluminum brazing material meets the following requirements: (M1-9M2 / 40):M3=(5~16):1; Wherein, M1 is the mass of aluminum in the core of the composite aluminum powder, M2 is the mass of copper oxide in the shell of the composite aluminum powder, and M3 is the mass of nickel powder, and the units of M1, M2, and M3 are the same; Preferably, the preformed aluminum brazing material meets the following requirements: (M1-9M2 / 40): M3=(6~10):

1.

6. The preformed aluminum brazing material according to claim 1, characterized in that: The average particle size of the nickel powder is 200-1200 nm; preferably, the average particle size of the nickel powder is 200-1000 nm.

7. The preformed aluminum brazing material according to claim 1, characterized in that: The mass content of nickel powder in the preformed aluminum brazing material is 1-8.4%.

8. The preformed aluminum brazing material according to claim 1, characterized in that: The porosity of the magnesium mesh is 60-90%; preferably, the porosity of the magnesium mesh is 70-85%.

9. The preformed aluminum brazing material according to claim 1, characterized in that: The aluminum brazing flux is a fluoroaluminate aluminum brazing flux; in the preformed aluminum brazing material, the mass content of the aluminum brazing flux is 5-15%.

10. The method for preparing the preformed aluminum brazing material according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) mixing micron aluminum powder and nano copper oxide powder in an organic solvent to prepare a slurry, followed by spray granulation and drying to obtain a composite aluminum powder with a core-shell structure; (2) The composite aluminum powder, nickel powder and aluminum brazing agent are mixed in an organic solvent to form a paste slurry, which is then applied on a magnesium mesh, left to stand, dried, cured and cut to obtain the preformed aluminum brazing material.

Citation Information

Patent Citations

  • Thermite welding lug

    CN101505907A

  • Method for connecting carbon fiber reinforced aluminum-based composite with metal

    CN102658368A

  • Preparation method of nanoscale core-shell structure super thermite

    CN105624647A

  • Exothermic welding powder and preparation process and application method thereof

    CN108672978A

  • Composite solder and preparation method and application thereof

    CN111468857A