Method for preparing high-entropy alloy film based on ink-jet printing and jet printing system

By mixing metal oxide powder with organic solvents and binders to prepare ink, and printing using the Tesla valve structure of the printing system, the problems of poor composition uniformity of high-entropy alloy films and unstable nozzle flow were solved, achieving Efficiently prepare high-performance high-entropy alloy films and reduce costs.

CN118722040AActive Publication Date: 2024-10-01HUAZHONG UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410767793.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

When preparing high-entropy alloy films in the existing technology, poor composition uniformity and unstable nozzle flow lead to poor performance and high cost.

Method used

The ink is prepared by mixing metal oxide powder with organic solvents and binders, printing through the Tesla valve structure nozzle of the printing system, and performing heat treatment to reduce it into a high-entropy alloy film.

Benefits of technology

The uniformity and stability of high-entropy alloy films are improved, the preparation process is simplified, the cost is reduced, and the film-forming effect is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118722040A_ABST
    Figure CN118722040A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of high-entropy alloy preparation, and particularly relates to a method for preparing a high-entropy alloy film based on ink-jet printing and a jet printing system. Mixing the metal oxide powder and the organic solvent, adding the adhesive, and uniformly mixing to obtain the printing ink required by printing; printing ink is sprayed to the surface of a substrate, and an oxide liquid film is obtained; a volatile solvent in the oxide liquid film volatilizes and is cured to form an oxide film, and then the oxide film is subjected to first heat treatment; and then, in the hydrogen environment, the thin film obtained after first-time heat treatment is subjected to second-time heat treatment, the metal oxide powder is firstly reduced into metal, then the metal is sintered, and the high-entropy alloy thin film is obtained. By optimizing the ink formula and improving the jet printing system structure, the dispersion uniformity of the metal oxide powder is improved, then the performance and printing efficiency of the obtained high-entropy alloy film are improved, meanwhile, a new way is provided for preparation of the high-entropy alloy film, and the high-entropy alloy film with excellent performance can be obtained easily.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high entropy alloy preparation, and specifically relates to a method for preparing a high entropy alloy film based on inkjet printing and a printing system. Background Art

[0002] High entropy alloy is a new type of alloy material, which is composed of a variety of metals containing transition elements, and the atomic percentage of each component is between 5% and 35%. The atoms of each element in the high entropy alloy form a grid structure through the most "disordered" mode, so that the thermodynamic parameter entropy of the alloy system is in a high value state. With the development of my country's aerospace industry, new challenges have been raised for high-speed or ultra-high-speed aircraft, such as the requirements of light weight, high reliability and reusability of launch vehicles. During the launch and return to the atmosphere, the nose cone, leading edge and other parts of the high-speed aircraft will be subjected to great thermal shock, requiring high-performance thermal protection system protection. High-temperature resistant materials are the core of the thermal protection system of hypersonic aircraft and the cornerstone of ultra-high temperature thermal sealing design. The more types of metals added to traditional alloys, the easier it is to form brittle intermetallic compounds to make the material embrittled. High entropy alloys, due to the presence of transition elements, generally form simple solid solutions or amorphous phases dominated by fcc or bcc phases, and have better fracture strength, tensile strength, stability, high temperature resistance, wear resistance and other properties than traditional alloys.

[0003] The main preparation technologies of high entropy alloy films include sputtering deposition, electrochemical deposition, evaporation coating, ion plating, etc. Usually, metal powders such as Co, Cr, Fe, Ni, Ti, and Al are mixed in proportion to obtain the ink required for printing. Due to the large number of high entropy alloy components and complex composition, it is difficult to control the uniformity of the components using film-forming methods such as sputtering deposition, and the cost is high, and the structure of the prepared high entropy alloy film is relatively simple. Inkjet printing puts the component mixing link in the ink mixing step, which is conducive to overcoming the problem of poor component uniformity in the raw material preparation stage. However, the ink uniformity of inkjet printing has a great influence on the printing effect and needs to be optimized. In addition, when the existing inkjet printing system prints high-viscosity ink, the flow at the nozzle is easily affected by the solid particles inside the ink, resulting in nozzle blockage and unstable flow, which in turn affects the performance of the printed high entropy alloy film.

[0004] Therefore, it is necessary to provide a method for preparing a high entropy alloy film based on inkjet printing and a printing system to solve the above problems. Summary of the invention

[0005] In view of the defects or improvement needs of the prior art, the purpose of the present invention is to provide a method and a printing system for preparing high entropy alloy films based on inkjet printing, which can synergistically improve the preparation uniformity and stability of high entropy alloy films by optimizing the ink formula, and at the same time provide a new way for the preparation of high entropy alloy films, which is helpful to obtain high entropy alloy films with excellent performance.

[0006] To achieve the above object, the present invention provides a method for preparing a high entropy alloy thin film based on inkjet printing, comprising the following steps:

[0007] S1, mixing metal oxide powder of metal elements required to form the high entropy alloy film and an organic solvent, then adding a binder, and mixing evenly to obtain ink required for printing;

[0008] S2, spraying the ink onto the surface of the substrate through the nozzle of the printing system to obtain an oxide liquid film;

[0009] S3, the oxide liquid film solidifies to form an oxide thin film, which is then subjected to a first heat treatment;

[0010] S4. Under a reducing atmosphere, the oxide film after the first heat treatment is subjected to a second heat treatment, wherein the metal oxide powder is first reduced to metal and then sintered to obtain the high entropy alloy film; the second heat treatment comprises: first treating at 500-650°C for 1-3h, and then heating to 1000-1500°C for 0.5-1h.

[0011] Further, the metal oxide powder includes Fe2O3 15-25%, NiO 15-25%, Co3O4 15-25%, Cr2O3 15-25% and Al2O3 15-25% by mass. Preferably, the metal oxide powder includes Fe2O3 18-22%, NiO 18-22%, Co3O4 18-22%, Cr2O3 18-22% and Al2O3 18-22% by mass.

[0012] Furthermore, the adhesive is polylactic acid-glycolic acid copolymer.

[0013] Furthermore, the solvent is a mixture of dichloromethane, dibutyl phthalate and 2-butoxyethanol.

[0014] Furthermore, the amount of metal oxide powder added to the ink is 25-35%.

[0015] Furthermore, the mass ratio of dibutyl phthalate to 2-butoxyethanol is (1.8-2.2):1.

[0016] Furthermore, the volume ratio of the metal oxide powder to the binder in the ink is (6-8):3.

[0017] Furthermore, the viscosity of the ink is controlled at 15-30 cP, and the viscosity is adjusted by adjusting the amount of the dichloromethane.

[0018] Furthermore, the ink preparation method is: first, dichloromethane is added to a mixture of dibutyl phthalate and 2-butoxyethanol; then, metal oxide powder is added to the mixture by stirring or shaking; finally, the mixture is mixed with a polylactic acid-glycolic acid copolymer solution dissolved in dichloromethane to obtain the ink required for printing; wherein, the amount of dichloromethane added is adjusted according to the viscosity of the ink so that the viscosity of the ink is controlled at 15-30cP.

[0019] Furthermore, the temperature of the first heat treatment is 280-320°C and the time is 0.5-1h;

[0020] And / or, the reducing atmosphere is hydrogen.

[0021] Furthermore, the printing system includes an ink cartridge and a plurality of nozzles arranged at intervals at the bottom of the ink cartridge; each of the nozzles is provided with a microchannel, and the microchannel is a Tesla valve structure; a piezoelectric element is provided on the upper part of the ink cartridge for generating pressure to cause the ink to be ejected from the nozzle through the microchannel.

[0022] Furthermore, during the printing process, the nozzle moves in coordination with the substrate, and the printed ink droplets are deposited on the surface of the substrate to form an oxide liquid film.

[0023] The present invention also provides a printing system, comprising an ink cartridge and a plurality of nozzles arranged at intervals at the bottom of the ink cartridge; each of the nozzles is connected to the ink cartridge through a microchannel, and the microchannel is a Tesla valve structure; a piezoelectric element is arranged on the upper part of the ink cartridge to generate pressure to cause the ink to be sprayed out from the nozzle through the microchannel.

[0024] Furthermore, the piezoelectric element is a piezoelectric ceramic, which is arranged inside the ink cartridge and directly contacts the ink;

[0025] Each of the microchannels comprises a plurality of pipeline branches which are alternately arranged and connected; each pipeline branch has two pipelines, one of which is a straight forward channel which is inclined; and the other is a curved channel which is bent into a semi-circular shape and is connected back to the straight forward channel.

[0026] In general, the above technical solutions conceived by the present invention have the following beneficial effects compared with the prior art:

[0027] 1. The present invention uses metal oxide powder as raw material, and by adding a binder and an organic solvent, it helps to obtain a uniform and fluid ink, which is convenient for inkjet printing and effectively solves the problem of difficult mixing of metal oxide raw materials; in addition, compared with elemental powder, metal oxide powder has lower cost and better stability, and combined with the subsequent heat treatment reduction process, it helps to regulate the morphology of the high entropy alloy film. Therefore, the present invention provides a new way for the preparation of high entropy alloy films. The method is simple and easy to operate, low in cost, high in efficiency, and easy to promote and apply.

[0028] 2. The reduction process and sintering process of the metal oxide component in the present invention are carried out simultaneously, which effectively simplifies the preparation process of the high entropy alloy film. During the heat treatment process, when the temperature gradually increases, the binder begins to decompose, and then the metal oxide powder is reduced to metal; when the temperature reaches the peak temperature, the reduction and sintering of the metal are carried out simultaneously, and different metal particles diffuse and combine with each other to obtain a high entropy alloy film.

[0029] 3. The present invention utilizes a microchannel nozzle with a Tesla valve structure to allow the forward-flowing ink to pass smoothly, effectively prevent clogging, and facilitate obtaining a high-entropy alloy film with better film-forming effect; through the movement and coordination of the ink cartridge and the substrate, the droplet falling position can be precisely controlled, the implementation method is simple and convenient, and the printing result is accurate and efficient. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a flow chart of the high entropy alloy film preparation process constructed by the preferred embodiment of the invention;

[0031] Figure 2 It is a schematic structural diagram of the inkjet printing system of the present invention;

[0032] Figure 3 is a schematic diagram of the microchannel structure of the inkjet printing system;

[0033] Figure 4 The following are actual pictures of the metal powder and ink used in the examples.

[0034] Reference numerals

[0035] 1-ink cartridge, 11-piezoelectric element, 12-microchannel, 13-nozzle, 2-ink, 21-ink droplet, 22-ink line, 23-ink film, 3-light source, 4-XY moving platform, 5-high-speed camera, 6-controller. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0037] The uneven composition of the high entropy alloy film and the easy clogging of the existing nozzle when printing the viscous ink will affect the performance of the printed high entropy alloy film and reduce the printing efficiency. In view of this, the present invention first provides a method for preparing a high entropy alloy film based on inkjet printing, such as Figure 1-3 As shown, the following steps are included:

[0038] S1, mixing metal oxide powder of metal elements required to form the high entropy alloy film and an organic solvent, then adding a binder, and mixing evenly to obtain ink required for printing;

[0039] S2, spraying the ink onto the surface of the substrate through the nozzle of the printing system to obtain an oxide liquid film; in this process, the ink forms ink droplets through the nozzle and is deposited on the substrate under the action of gravity, and the XY moving platform is adjusted (the substrate is placed on the XY moving platform) to print the desired oxide liquid film;

[0040] S3, the volatile solvent in the oxide liquid film gradually evaporates, thereby solidifying to form a stable oxide film, and then performing a first heat treatment on the oxide liquid film; after the oxide liquid film is solidified and subjected to the first heat treatment, the solvent and the binder begin to be removed by thermal degradation, forming a solid oxide film containing a large number of small pores;

[0041] S4. Then, in a hydrogen environment, the film after the first heat treatment is subjected to a second heat treatment, where the metal oxide powder is first reduced to metal and then sintered to obtain a high entropy alloy film.

[0042] The present invention uses metal oxide powder as a starting material, prepares ink with good uniformity, and then prints the film and then thermally reduces it to obtain a high entropy alloy film. In this way, the metal oxide powder has better stability and safety, lower cost, and is easy to promote and apply, and the metal oxide powder has better dispersibility in organic solvents. During the subsequent thermal reduction, oxygen in the metal oxide is released to obtain a single high entropy alloy film. When the temperature is further increased for sintering, different metal particles diffuse and combine with each other, which is helpful for the regulation and improvement of the high entropy alloy structure.

[0043] The quality of the high entropy alloy film finally obtained by the present invention is mainly determined by the composition of the metal oxides in the ink and the sintering temperature and time, and these factors are relatively easy to control. Therefore, the high entropy alloy film is highly controllable and convenient for large-scale application.

[0044] Wherein, the metal oxide powder is a mixture of oxides corresponding to the metal components in the final high entropy alloy film. Preferably, the metal oxide powder includes Fe2O315-25%, NiO15-25%, Co3O415-25%, Cr2O315-25% and Al2O315-25% by mass percentage. Preferably, the metal oxide powder includes Fe2O318-22%, NiO18-22%, Co3O418-22%, Cr2O318-22% and Al2O318-22% by mass percentage; more preferably, the metal oxide powder includes Fe2O320%, NiO20%, Co3O420%, Cr2O320% and Al2O320% by mass percentage. The purity and particle size of the metal oxide powder also have a certain influence on the film forming and sintering effects, and its purity is controlled to be greater than 99% and the particle size is less than 5μm.

[0045] The binder is a polylactic acid-glycolic acid copolymer, and its function is to ensure the stability of the printing process and maintain the shape of the final printed film. The volume ratio of the metal oxide powder and the binder in the ink is (6-8):3, preferably 7:3 (for example, the volume of the metal oxide powder and the binder can be measured by putting them into a measuring cylinder respectively). The amount of metal oxide powder added to the ink is 25-35%. When the amount of metal oxide powder added is too small, the porosity of the solid oxide film may be too high when the binder and the organic solvent are removed, which affects the compactness of the high entropy alloy film obtained by sintering; when the amount of metal oxide powder added is too much, its dispersibility will deteriorate, which is not conducive to printing a uniform oxide liquid film, thereby affecting the uniformity and stability of the high entropy alloy film.

[0046] The organic solvent is preferably a mixture of dichloromethane, dibutyl phthalate and 2-butoxyethanol. The mass ratio of dibutyl phthalate to 2-butoxyethanol is (1.8-2.2):1, preferably 2:1. The viscosity of the ink is preferably 30 cP, which can be adjusted by adjusting the amount of dichloromethane. The surface tension of the ink is preferably 31 mN / m. The present invention shows that this combination of organic solvents is more conducive to the uniform dispersion of metal oxide powders.

[0047] In particular, the ink preparation method is as follows: first, dichloromethane is added to a mixture of dibutyl phthalate and 2-butoxyethanol; then, metal oxide powder is added to the mixture by stirring or shaking; finally, the mixture is mixed with a polylactic acid-glycolic acid copolymer solution dissolved in dichloromethane to obtain the ink required for printing; wherein, the amount of dichloromethane added is adjusted according to the viscosity of the ink so that the viscosity of the ink is controlled at 15 to 30 cP.

[0048] Due to the volatile nature of methylene chloride, ink preparation should usually be carried out in a fume hood.

[0049] like Figure 4 As shown, the ink preparation method of the present invention enables the metal oxide particles to be uniformly dispersed in the organic solvent, which is conducive to finally obtaining a high entropy alloy film with uniform composition. Moreover, the ink has good fluidity and can be smoothly ejected from the nozzle.

[0050] In step S3, the temperature of the first heat treatment is 280-320°C and the time is 0.5-1h;

[0051] In step S4, the second heat treatment includes: first treating at 500-650°C for 1-3h, and then heating to 1000-1500°C for 0.5-1h. When the heat treatment temperature continues to rise and reaches the peak temperature, the reduction and sintering of the metal are carried out simultaneously. Under the action of high-temperature sintering, as time passes, different metal particles diffuse and combine with each other, forming a dense high-entropy alloy phase inside.

[0052] As a preferred solution of the present invention, the structure of the printing system (inkjet printing system) in step S2 is improved, such as Figure 2 As shown, it mainly includes a printing unit and a deposition unit. The printing unit mainly includes an ink cartridge 1 and a plurality of nozzles 13 arranged at intervals at the bottom of the ink cartridge 1; each nozzle 13 is provided with a microchannel 12, and the microchannel 12 is preferably provided with a Tesla valve structure, such as Figure 3 As shown; a piezoelectric element 11 is arranged on the upper part of the ink cartridge 1, which is used to generate pressure to eject the ink from the nozzle 13 through the microchannel 12 to the deposition unit to form an oxide liquid film. The deposition unit is preferably configured as an XY moving platform 4, which is used to fix the substrate. By moving its position, the deposition position of the oxide liquid film can be synchronously adjusted.

[0053] Specifically, the piezoelectric element 11 is a piezoelectric ceramic, which is disposed inside the ink cartridge 1 and directly contacts the ink. The piezoelectric element 11 is connected to a driving device, which can apply a driving voltage to the piezoelectric element 11 to deform it and generate downward pressure, thereby forcing the ink to be squeezed from the microchannel 12 to the nozzle 13.

[0054] like Figure 3As shown, each microchannel 12 includes a number of pipeline branches connected in an alternating arrangement; each pipeline branch has two pipelines, one of which is a straight forward channel, which is inclined; the other is a curved channel, which is bent into a semi-circular shape and connected back to the straight forward channel. The structural design of the microchannel 12 in the printing system can realize the unidirectional flow of ink at the nozzle 13, that is, the ink flowing in the forward direction (toward the nozzle 13) can pass smoothly, and the ink flowing in the reverse direction is suppressed, thereby effectively alleviating the problem of easy blockage of ink at the nozzle.

[0055] In particular, the printing system also includes a controller 6 and a high-speed camera 5. The ink cartridge 1 and the XY moving platform 4 are respectively connected to the controller 6. When the driving voltage is applied to the piezoelectric element 11, the piezoelectric element 11 is deformed, thereby pressurizing the ink to eject the ink. By controlling the parameters such as the amplitude and period of the input voltage through the controller 6, the size and dripping speed of the ink droplets can be accurately controlled, thereby achieving high-precision printing. At the same time, the movement of the ink cartridge 1 and the substrate on the XY moving platform 4 can be accurately controlled through the program control of the controller 6, which can effectively speed up the film printing speed. The high-speed camera 5 is set on the side of the XY moving platform 4 to monitor the fusion between the ink droplets and the printing line, and uses this as a reference to adjust the movement speed of the XY moving platform 4 and the dripping speed of the ink droplets to achieve precise control of the printed film.

[0056] In some preferred embodiments, the structural characteristic parameters of the ink (such as ink viscosity, metal oxide powder content, etc.) can be associated with the structural parameters of the controller 6, and the size and dripping speed of the ink droplets and the movement speed of the substrate can be regulated according to the structural characteristic parameters of the ink, so as to obtain a high-entropy alloy film with better film forming and sintering effects.

[0057] The method for preparing a high entropy alloy thin film based on inkjet printing of the present invention is described below through specific examples.

[0058] (1) The printing system used in this embodiment is as follows Figure 2 As shown, it includes a printing unit and a deposition unit, wherein the droplet printing unit includes an ink cartridge 1, a piezoelectric element 11, a microchannel structure 12, a nozzle 13, ink 2 and ink droplets 21; the droplet deposition unit includes an ink line 22, an ink film 23, a light source 3, an XY moving platform 4 and a high-speed camera 5. In this example, the piezoelectric element 11 is made of piezoelectric ceramics, and the light source 3 is made of high-intensity LED. The ink droplets 21 sprayed from the nozzle 13 vertically collide with the substrate on the XY moving platform 4 under the action of gravity, and adjacent ink droplets 21 will merge to form ink lines 22 during the spreading process, and adjacent ink lines 22 will merge to form ink films 23.

[0059] like Figure 3As shown, the microchannel 12 connects the ink 2 to one end of the nozzle 13. Under the action of the piezoelectric element 11, the ink 2 above flows to the nozzle 13 through the microchannel structure 12 and is ejected under pressure to form ink droplets. Due to the special design of the microchannel 12 structure, the forward flow and reverse flow of the ink 2 are very different. When the piezoelectric element 11 deforms and generates downward pressure, the ink 2 can pass through the microchannel 12 smoothly from top to bottom without resistance; when the piezoelectric element 11 is deformed, a negative pressure is formed inside the ink cartridge 1, and the ink 2 will flow in the reverse direction. The difference is that if the ink 2 flows into the microchannel 12 in the reverse direction, it will be divided into two paths at the first intersection and converge at the second intersection. This time, the flow directions of the two paths of ink 2 are opposite, so a great resistance is formed. As the number of intersections increases, the flow of the ink 2 slows down rapidly, so the microchannel 12 can only pass in the forward direction, and it is difficult to reverse the reverse flow. Such a structural design effectively alleviates the problem of ink 2 being easily blocked at the nozzle 13.

[0060] Before use, the focus and aperture of the high-speed camera should be adjusted so that a bright and uniform real image can be observed.

[0061] (2) Based on the above-mentioned printing system, a high entropy alloy film is prepared, such as Figure 1 As shown, the details are as follows:

[0062] First, add dichloromethane to a mixture of dibutyl phthalate and 2-butoxyethanol (mass ratio is 2:1); then add metal oxide powder to the mixed solvent by stirring; finally, mix the mixture with a polylactic acid-glycolic acid copolymer solution dissolved in dichloromethane to obtain the ink required for printing; wherein, the viscosity of the ink is adjusted by adding an amount of dichloromethane according to the viscosity of the ink so that the viscosity of the ink is controlled at 30cP. The metal oxide powder includes Fe2O3 20%, NiO 20%, Co3O4 20%, Cr2O3 20% and Al2O3 20% by mass percentage. In the final ink, the volume ratio of metal oxide powder to binder is 7:3, and the mass content of metal oxide powder is preferably 30%. As Figure 4 As shown, it can be seen that the obtained ink has good dispersibility and moderate viscosity, which is helpful to improve the quality of the printed high entropy alloy film.

[0063] After the prepared ink is printed by the inkjet printing system, the required oxide liquid film is printed on the substrate. The volatile solvent in the oxide liquid film gradually evaporates, thereby solidifying to form a stable oxide film, which is subjected to the first heat treatment (in this embodiment, it is treated at 300°C for 1h), and then the printed oxide film is heat treated in a hydrogen environment. When the temperature rises to 600°C, polylactic acid-glycolic acid decomposes and detaches from the film, at which time the metal oxide powder begins to be reduced to metal, accompanied by the production of water; when the temperature continues to rise to a peak temperature of 1000°C, the reduction and sintering of the metal are carried out simultaneously. Under the action of high-temperature sintering, as time passes, different metal particles diffuse and combine with each other, forming a dense high-entropy alloy phase inside. The components of the metal oxide in the ink and the temperature and time of sintering determine the quality of the final high-entropy alloy film.

[0064] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a high entropy alloy thin film based on inkjet printing, characterized in that: The following steps are involved: S1, mixing metal oxide powder of metal elements required to form the high entropy alloy film and an organic solvent, then adding a binder, and mixing evenly to obtain ink required for printing; S2, spraying the ink onto the surface of the substrate through the nozzle of the printing system to obtain an oxide liquid film; S3, the oxide liquid film solidifies to form an oxide thin film, which is then subjected to a first heat treatment; S4. Under a reducing atmosphere, the oxide film after the first heat treatment is subjected to a second heat treatment, wherein the metal oxide powder is first reduced to metal and then sintered to obtain the high entropy alloy film; the second heat treatment comprises: first treating at 500-650°C for 1-3h, and then heating to 1000-1500°C for 0.5-1h.

2. The method for preparing a high entropy alloy thin film based on inkjet printing according to claim 1, characterized in that: The metal oxide powder comprises, by mass percentage, 15-25% Fe2O3, 15-25% NiO, 15-25% Co3O4, 15-25% Cr2O3 and 15-25% Al2O3; and / or, the adhesive is polylactic acid-glycolic acid copolymer; And / or, the organic solvent is a mixture of dichloromethane, dibutyl phthalate and 2-butoxyethanol.

3. The method for preparing a high entropy alloy thin film based on inkjet printing according to claim 2, characterized in that: The mass fraction of the metal oxide powder in the ink is 25-35%.

4. The method for preparing a high entropy alloy thin film based on inkjet printing according to claim 2, characterized in that: The mass ratio of dibutyl phthalate to 2-butoxyethanol is (1.8-2.2):1; And / or, the relative volume ratio of the metal oxide powder to the binder in the ink is (6-8):3; And / or, the viscosity of the ink is controlled at 15-30 cP, and the viscosity is adjusted by adjusting the amount of the dichloromethane.

5. The method for preparing a high entropy alloy thin film based on inkjet printing according to any one of claims 2 to 4, characterized in that: The ink preparation method comprises the following steps: firstly, adding dichloromethane to a mixture of dibutyl phthalate and 2-butoxyethanol; then, adding metal oxide powder to the mixture by stirring or shaking; finally, mixing the mixture with a polylactic acid-glycolic acid copolymer solution dissolved in dichloromethane to obtain the ink required for printing; wherein, the amount of dichloromethane added is adjusted according to the viscosity of the ink so that the viscosity of the ink is controlled within the range of 15 to 30 cP.

6. The method for preparing a high entropy alloy thin film based on inkjet printing according to any one of claims 1 to 4, characterized in that: The temperature of the first heat treatment is 280-320°C and the time is 0.5-1h; And / or, the reducing atmosphere is hydrogen.

7. The method for preparing a high entropy alloy thin film based on inkjet printing according to any one of claims 1 to 4, characterized in that: The printing system includes an ink cartridge and a plurality of nozzles arranged at intervals at the bottom of the ink cartridge; each of the nozzles is provided with a microchannel, and the microchannel is a Tesla valve structure; a piezoelectric element is provided on the upper part of the ink cartridge for generating pressure to cause the ink to be ejected from the nozzle through the microchannel.

8. The method for preparing a high entropy alloy thin film based on inkjet printing according to claim 7, characterized in that: During the printing process, the nozzle moves in coordination with the substrate, and the printed ink droplets are deposited on the surface of the substrate to form an oxide liquid film.

9. A printing system used in the method for preparing a high entropy alloy thin film based on inkjet printing according to any one of claims 1 to 8, characterized in that: It comprises an ink cartridge and a plurality of nozzles arranged at intervals at the bottom of the ink cartridge; each of the nozzles is connected to the ink cartridge via a microchannel, and the microchannel is a Tesla valve structure; a piezoelectric element is arranged on the upper part of the ink cartridge to generate pressure to eject ink from the nozzle through the microchannel.

10. The printing system according to claim 9, characterized in that: The piezoelectric element is a piezoelectric ceramic, which is arranged inside the ink cartridge and directly contacts the ink; Each of the microchannels comprises a plurality of pipeline branches which are alternately arranged and connected; each pipeline branch has two pipelines, one of which is a straight forward channel which is inclined; and the other is a curved channel which is bent into a semi-circular shape and is connected back to the straight forward channel.

Citation Information

Patent Citations

  • Ink for inkjet printing and preparation method as well as zirconia film printed by ink for inkjet printing

    CN107151483A

  • Method for preparing high-entropy alloy by combining direct-writing 3D printing and hot isostatic pressing technology

    CN117961084A

  • Ink jet printing method for preparing metal film

    CN1400106A

  • Ink jet printing method for preparing metal oxide functional film

    CN1400107A

  • Systems and methods for manufacturing sintered metals

    US20220055113A1