Hydrogen energy storage method
By using aromatic hydrocarbons as hydrogenation carriers and NiO catalysts in the hydrogenation reactor, and using the waste heat of the raw hydrogen for low-temperature hydrogen storage, the problem of high energy consumption when the hydrogen production system and hydrogen storage system are coupled is solved, and low energy consumption is achieved of hydrogen storage.
Patent Information
- Application Number
- CN202310316552.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-28
AI Technical Summary
In the existing technology, additional energy is required when the hydrogen production system and the hydrogen storage system are coupled, resulting in high energy consumption and difficulty in matching.
In the hydrogenation reactor, aromatic hydrocarbons are used as the hydrogenation carrier and NiO is used as the catalyst. Through the low-temperature hydrogenation reaction, the waste heat of the raw material hydrogen is used for hydrogen storage treatment, thereby reducing the energy consumption of the hydrogen storage treatment.
It achieves hydrogen storage at a lower temperature, avoids the use of additional heating devices, reduces the difficulty of coupling the hydrogen storage processing and hydrogen production systems, and reduces energy consumption.
Smart Images

Figure CN118723922A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of new energy, and in particular, to a method for storing hydrogen energy. Background Art
[0002] Among the many chemical hydrogen storage technologies, liquid organic hydrogen carrier hydrogen storage technology is considered to be the technology most likely to achieve large-scale, cross-time and space hydrogen storage in the future. It uses a pair of reversible addition and dehydrogenation reactions between liquid organic compounds and their corresponding alkanes to achieve hydrogen storage and release. It has the advantages of high mass hydrogen storage density and can use existing petrochemical facilities for storage and transportation. The hydrogenation reaction is an exothermic reaction, and the dehydrogenation is an endothermic reaction. 30% of hydrogen is lost in this exothermic / endothermic reaction process, so how to reduce energy consumption in the hydrogenation and dehydrogenation links is a topic worth discussing. For this reason, the development of low-temperature hydrogen storage and release technology is very important. The temperature of the electrolyzer in the water electrolysis hydrogen production system is generally around 80-90°C. At present, the ideal temperature for toluene hydrogen storage is 95-105°C. Therefore, it is difficult to simply couple the green hydrogen manufacturing system and the hydrogen storage system, and additional energy is required. Summary of the invention
[0003] The purpose of the present disclosure is to provide a method for storing hydrogen energy to solve the problem in the prior art that additional energy needs to be provided when a hydrogen production system and a hydrogen storage system are coupled.
[0004] In order to achieve the above-mentioned purpose, the present disclosure provides a method for storing hydrogen energy, which comprises: contacting raw hydrogen produced by a hydrogen production device, a hydrogenation carrier and a catalyst in a hydrogenation reactor for hydrogen storage treatment to obtain a hydrogen storage product; the temperature of the hydrogen storage treatment is 25 to 90° C.; the hydrogenation carrier is selected from one or more of aromatic hydrocarbons; the catalyst comprises a carrier and an active metal oxide; the carrier comprises a porous body with a pore size of 1 to 100 nm, and the active metal element in the active metal oxide is Ni.
[0005] Optionally, the carrier includes MCM-41 porous body and / or SBA-15 porous body; and the active metal oxide is NiO.
[0006] Optionally, the carrier has a pore size of 1 to 10 nm and a specific surface area of 300 to 800 m 2 / g.
[0007] Optionally, based on the total weight of the catalyst, the content of the carrier is 80 to 95 weight %; the content of the active metal oxide is 5 to 20 weight %.
[0008] Optionally, based on the total weight of the catalyst, the content of the carrier is 85 to 93% by weight, and the content of the active metal oxide is 7 to 15% by weight.
[0009] Optionally, the hydrogenation carrier is selected from aromatic hydrocarbons having 6 carbon atoms and / or aromatic hydrocarbons having 7 carbon atoms.
[0010] Optionally, the hydrogenation carrier is benzene and / or toluene.
[0011] Optionally, the conditions of the hydrogen storage treatment include: temperature of 25-80°C, pressure of 0.1-0.15 MPa, time of 2-10 seconds, volume space velocity of 0.5-5h -1 .
[0012] Optionally, the hydrogen content in the raw hydrogen is 50-100%; the temperature of the raw hydrogen is 25-90°C.
[0013] Optionally, the hydrogen storage product is used directly; and / or the hydrogen storage product is transported to a dehydrogenation device for dehydrogenation treatment, and the obtained hydrogen enters a downstream hydrogen use device.
[0014] Through the above technical scheme, the use of the catalyst disclosed in the present invention can make the hydrogenation carrier react with the raw hydrogen at a relatively low temperature, and the hydrogenation carrier can be converted into a hydrogen storage product only by the waste heat of the upstream raw hydrogen, without the need for an additional heating device, thereby reducing the difficulty of coupling the hydrogen storage process and the hydrogen production system, and thereby reducing the energy consumption of the hydrogen storage process.
[0015] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0017] Figure 1 It is a schematic diagram of a method for storing hydrogen energy disclosed in the present invention.
[0018] Description of Reference Numerals
[0019] 1. Hydrogen production device; 2. Hydrogenation reactor; 3. Dehydrogenation device; 4. Downstream hydrogen use device. DETAILED DESCRIPTION
[0020] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0021] The first aspect of the present disclosure provides a method for storing hydrogen energy, which comprises: contacting raw hydrogen produced by a hydrogen production device 1, a hydrogenation carrier and a catalyst in a hydrogenation reactor 2 for hydrogen storage treatment to obtain a hydrogen storage product; the temperature of the hydrogen storage treatment is 25 to 90° C.; the hydrogenation carrier is selected from one or more of aromatic hydrocarbons; the catalyst comprises a carrier and an active metal oxide; the carrier comprises a porous body with a pore size of 1 to 100 nm, and the active metal element in the active metal oxide is Ni.
[0022] Through the above technical scheme, the use of the catalyst disclosed in the present invention can make the hydrogenation carrier react with the raw hydrogen at a relatively low temperature, and the hydrogenation carrier can be converted into a hydrogen storage product only by the waste heat of the upstream raw hydrogen, without the need for an additional heating device, thereby reducing the difficulty of coupling the hydrogen storage process and the hydrogen production system, and thereby reducing the energy consumption of the hydrogen storage process.
[0023] The raw hydrogen used in the present disclosure is prepared by a hydrogen production device 1, and the content of hydrogen in the raw hydrogen is 30-100 volume%, preferably 50-100 volume%, and more preferably 70-100 volume%. Among them, the raw hydrogen can be selected from one or more of by-product hydrogen, gray hydrogen, blue hydrogen and green hydrogen. In this embodiment, gray hydrogen refers to hydrogen produced by the combustion of fossil fuels, and there will be emissions such as carbon dioxide during the production process; blue hydrogen refers to natural gas through steam methane reforming or autothermal steam reforming coupled with CCUS (carbon dioxide capture application) technology; green hydrogen refers to hydrogen produced by using renewable energy, with no carbon emissions at all, and by-product hydrogen refers to hydrogen by-products produced in hydrogen devices and / or hydrogen production devices.
[0024] The raw hydrogen used in the present disclosure is green hydrogen, and the electric energy generated by renewable energy is directly used in the water electrolysis device, and the hydrogen obtained by electrolysis is used as the raw hydrogen, and the temperature of the raw hydrogen is 25 to 90°C, preferably 30 to 85°C, and more preferably 55 to 80°C. The hydrogen production device 1 is a conventional choice in the art, and this application does not make special requirements. For example, the hydrogen production device 1 disclosed in the present disclosure is a water electrolysis device. The renewable energy includes light energy and / or wind energy.
[0025] The hydrogenation carrier used in the present disclosure is a liquid hydrogen storage material, preferably an aromatic hydrocarbon with 6 carbon atoms and / or an aromatic hydrocarbon with 7 carbon atoms, and more preferably benzene and toluene. In this embodiment, the liquid hydrogen storage material selects an aromatic hydrocarbon compound with a high degree of unsaturation, and through hydrogenation treatment, hydrogen can react with the hydrogenation carrier to convert the corresponding aromatic hydrocarbon into the corresponding cycloalkane, so that the hydrogen can be stored in the hydrogenation carrier. Among them, the higher the unsaturation of the hydrogenation carrier, the better the hydrogen storage capacity.
[0026] The catalyst used in the present disclosure is composed of a carrier and an active metal oxide.
[0027] The carrier comprises MCM-41 porous body and / or SBA-15 porous body; the pore size of the carrier is 1-10 nm, and the specific surface area is 300-800 m 2 / g.
[0028] Among them, SBA-15 porous body refers to SBA-15 mesoporous silica molecular sieve, which has highly ordered hexagonal straight pores. The pore diameter of the straight pores can be flexibly adjusted within 4-10nm, the pore wall thickness is within the range of 3.1nm to 6.0nm, and the specific surface area is 400-800m 2 / g, preferably 500-700m 2 / g. The skeleton structure is stable, the wall is thick and it is easy to dope.
[0029] Among them, MCM-41 is an ordered mesoporous material and a typical representative of the M41S group. At the nanoscale, MCM-41 presents an ordered "honeycomb" porous structure, that is, it has a one-dimensional linear pore array in a hexagonal close-packed array; the pore size of the MCM-41 porous body can be continuously adjusted in the range of 2-10nm, preferably 3-5nm. During electron microscopy observation, it was found that the pores can run through the entire molecular sieve particle, and the pore wall thickness is generally around 1nm; the specific surface area is 350-800m 2 / g, preferably 500-700m 2 / g.
[0030] The active metal element in the active metal oxide includes one or more of Ni, Pd, Pt, V, Cr and Co, preferably Ni.
[0031] Wherein, the active metal oxide includes Ni2O3 and / or NiO, preferably NiO.
[0032] In a preferred embodiment, the carrier is a SBA-15 porous body, and the active metal oxide is NiO.
[0033] In one embodiment, based on the total weight of the catalyst, the content of the carrier is 80 to 95 weight %; and the content of the active metal oxide is 5 to 20 weight %.
[0034] In a preferred embodiment, based on the total weight of the catalyst, the content of the carrier is 85-93% by weight, and the content of the active metal oxide is 7-15% by weight.
[0035] In a specific embodiment, the preparation method of the SBA-15 porous body loaded with NiO comprises: dissolving a polyoxyethylene-polyoxypropylene-polyoxyethylene triblock polymer (abbreviated as P123) in distilled water at room temperature, then adding tetraethyl orthosilicate, stirring evenly, adding a hydrochloric acid solution, and then heating the reaction. After the reaction is completed, filtering, washing, and drying and calcining the solid product to obtain a mesoporous SBA-15 porous body. Dissolve an appropriate amount of nickel nitrate in an ethanol solvent, add the SBA-15 porous body, and after the reaction, volatilize the solvent and calcine to obtain a SBA-15 porous body loaded with NiO.
[0036] In the above embodiment, in the presence of hydrogen, the active metal oxide in the catalyst undergoes a reduction reaction with hydrogen to reduce the active metal oxide to an active metal. The active metal can enhance the reaction activity of the hydrogenation reaction between the hydrogenation carrier and the raw hydrogen, and reduce the reaction temperature and pressure of the hydrogenation reaction. For example, the hydrogenation temperature of toluene can be reduced from the lowest ideal temperature of 95-105°C recorded in the literature to a preferred 40°C, and the pressure can be reduced to normal pressure.
[0037] In one embodiment, the conditions of the hydrogen storage treatment include: temperature of 25-90°C, preferably 25-80°C, more preferably 25-50°C; pressure of 0.1-0.3MPa, preferably 0.1-0.15MPa; time of 2-10 seconds, preferably 5-10 seconds; volume space velocity of 0.5-50h -1 , preferably 1 to 20 hours -1 .
[0038] Among them, the hydrogenation reactor 2 used for hydrogen storage treatment is a conventional choice in the field, and this application does not make special requirements. For example, the hydrogenation reactor 2 used in the present disclosure is a microreactor, and the inner diameter of the reaction tube of the microreactor is 0.6 cm.
[0039] Wherein, the flow rate of the raw hydrogen is 20 to 50 mL / min.
[0040] The method further includes first adding a catalyst into the hydrogenation reactor 2 and performing a reduction treatment under raw hydrogen conditions, and then adding a hydrogenation carrier into the hydrogenation reactor 2 to perform a hydrogenation reaction to obtain a hydrogen storage product.
[0041] The temperature of the reduction treatment is 450-550° C. and the time is 4-6 hours, so that the active metal oxides loaded in the catalyst can be reduced to the corresponding active metals to enhance the reaction activity of the hydrogenation reaction.
[0042] In a specific embodiment, the hydrogen storage treatment includes: placing a catalyst in a microreactor, reducing it for 4 to 6 hours under the conditions of raw hydrogen and 450 to 550° C., and then cooling it to room temperature. Under the conditions of raw hydrogen, a hydrogenation carrier is added to carry out a hydrogenation reaction to obtain a hydrogen storage product.
[0043] In one embodiment, the hydrogen storage product is used directly. Specifically, the hydrogen storage product can be used as fuel to supply oil-using equipment such as automobiles, ships and airplanes. The hydrogen storage product can also be used as a solvent or a conventional chemical.
[0044] In another embodiment, the hydrogen storage product is sent to the dehydrogenation device 3 of the downstream hydrogen device 4 for dehydrogenation treatment to obtain hydrogen and a hydrogenation carrier; the obtained hydrogen is sent to the downstream hydrogen device 4 for use, and the obtained hydrogenation carrier is sent out or circulated to the hydrogenation reactor 2 or used directly.
[0045] The dehydrogenation device 3 used in the present disclosure is a conventional choice in the art, and this application does not make any special requirements. The dehydrogenation method used in the present disclosure is a conventional choice in the art, and this application does not make any special requirements.
[0046] In one embodiment, a method for storing hydrogen energy includes:
[0047] Catalyst preparation: P123 is dissolved in distilled water at room temperature, followed by addition of ethyl orthosilicate, stirring evenly, adding hydrochloric acid solution, and then heating for reaction. After the reaction is completed, filter, wash with water, dry and calcine the solid product to obtain a mesoporous SBA-15 porous body. Dissolve an appropriate amount of nickel nitrate in an ethanol solvent, add the SBA-15 porous body, react, evaporate the solvent, and calcine to obtain the catalyst;
[0048] Hydrogen storage treatment: The raw hydrogen produced by the hydrogen production device 1, the hydrogenation carrier and the catalyst are contacted in the hydrogenation reactor 2 for hydrogen storage treatment to obtain a hydrogen storage product; the conditions of the hydrogen storage treatment include: temperature of 25-90°C, pressure of 0.1-0.15MPa, time of 2-10 seconds, volume space velocity of 0.5-5h -1 ; The hydrogenation carrier is selected from one or more aromatic hydrocarbons; the hydrogen storage product is directly used as a fuel; and / or, the hydrogen storage product is transported to a dehydrogenation device 3 for dehydrogenation treatment, and the obtained hydrogen enters a downstream hydrogen use device 4.
[0049] The method provided by the present invention is further described below by means of specific examples, but the present invention is not limited thereby.
[0050] Preparation Example 1
[0051] Preparation of catalyst A1: 4g of P123 was dissolved in 105g of distilled water at room temperature, followed by the addition of 8.52g of ethyl orthosilicate, and stirred for 30 minutes, followed by the addition of 28.6g of hydrochloric acid solution. Then, the mixture was immediately placed in a 60-degree oil bath and heated for 24 hours under stirring. After the reaction, the mixture was filtered and washed with water. The solid product was dried at 80 degrees for one night and calcined at 550 degrees for 10 hours to obtain a pore size of 6.8nm and a specific surface area of 650m 2 / g of mesoporous SBA-15 carrier. An appropriate amount of nickel nitrate was placed in 10g of ethanol solvent, and after being oscillated and dissolved under ultrasonic wave, 3g of mesoporous carrier was added, and after continuing to oscillate for half an hour, the ethanol was allowed to evaporate naturally in a fume hood, and then calcined at 500 degrees for 10 hours to obtain NiO-loaded catalyst A1. Based on the total weight of catalyst A1, the content of SBA-15 carrier was 85% by weight, and the content of NiO was 15% by weight.
[0052] Preparation Example 2
[0053] The method for preparing catalyst A2 is the same as that of Example 1, except that the pore size of the SBA-15 porous body in catalyst A2 is 15 nm and the specific surface area is 900 m 2 / g.
[0054] Preparation Example 3
[0055] The method for preparing catalyst A3 is the same as that of Example 1, except that, based on the total weight of catalyst A3, the content of SBA-15 porous body is 95 wt % and the content of NiO is 5 wt %.
[0056] Preparation Comparative Example 1
[0057] Preparation of comparative catalyst D1: As the main load metal liquid preparation, 1.328 g of chloroplatinic acid hexahydrate was dissolved in 200 mL of distilled water aqueous solution; as the secondary load metal liquid preparation, 0.128 g of rhodium chloride trihydrate was dissolved in 100 mL of distilled water aqueous solution; the two aqueous solutions were mixed to prepare about 300 mL of a mixed solution.
[0058] 4.45 g of activated carbon as a carrier was immersed in the mixed solution and stirred thoroughly. After standing overnight, the activated carbon was taken out from the mixed solution, washed thoroughly with water and dried. Then, the dried activated carbon was immersed in 500 mL of an aqueous solution of sodium borohydride at a concentration of 10% to reduce and activate the supported metal, and further washed with water and dried to prepare about 5 g of comparative catalyst D1. The contents of the main supported metal platinum and the secondary supported metal rhodium in the prepared comparative catalyst D1 were 10 wt% and 1 wt%, respectively. It should be noted that the atomic ratio of platinum to rhodium in this case is rhodium / platinum = 0.053.
[0059] Preparation Comparative Example 2
[0060] The method for preparing catalyst D2 is the same as that of Example 1, except that iron oxide is used instead of nickel oxide as the active metal oxide of the catalyst.
[0061] Preparation Comparative Example 3
[0062] The method for preparing catalyst D3 is the same as that of Example 1, except that non-porous silica (Kyoto Chemical) is used as a carrier instead of SBA-15. The comparative catalyst D3 is obtained by the method of Preparation Example 1.
[0063] Example 1
[0064] Hydrogen storage treatment: Catalyst A1 (catalyst bed height 2 cm) was placed in a microreactor (reaction tube inner diameter 0.3 cm), and reduced at 500°C for 5 h under a hydrogen flow of 34 mL / min, and then cooled to 20°C; under a hydrogen flow of 34 mL / min, 0.2 μmL of benzene was injected with a syringe for hydrogen storage treatment to obtain cyclohexane. The conditions of the hydrogen storage treatment include: temperature 25°C, pressure 0.1013 MPa, time 2 seconds, volume space velocity 0.67 h -1 ; The hydrogenation carrier is selected from one or more aromatic hydrocarbons.
[0065] The hydrogen storage product is used directly as a fuel; and / or the hydrogen storage product is transported to a dehydrogenation device 3 for dehydrogenation treatment, and the obtained hydrogen enters a downstream hydrogen use device 4.
[0066] Example 2
[0067] The method for hydrogen energy storage is the same as that in Example 1, except that the hydrogenation carrier is 0.2 μmL of toluene, and the conditions for the hydrogen storage treatment include: temperature of 40°C, pressure of 0.1013 MPa, time of 2 seconds, and volume space velocity of 0.67 h -1 .
[0068] Example 3
[0069] The method for storing hydrogen energy is the same as that in Example 2, except that the catalyst used is catalyst A2.
[0070] Example 4
[0071] The method for storing hydrogen energy is the same as that in Example 2, except that the catalyst used is catalyst A3.
[0072] Comparative Example 1
[0073] The method for storing hydrogen energy is the same as that in Example 1, except that catalyst D1 is used.
[0074] Comparative Example 2
[0075] The method for storing hydrogen energy is the same as that in Example 2, except that catalyst D1 is used.
[0076] Comparative Example 3
[0077] The method for storing hydrogen energy is the same as that in Example 2, except that catalyst D2 is used.
[0078] Comparative Example 4
[0079] The method for storing hydrogen energy is the same as that in Example 2, except that catalyst D3 is used.
[0080] Table 1 Hydrogen storage treatment conditions and product properties
[0081]
[0082]
[0083] As shown in Table 1, according to the comparison of the data in Examples 1 to 2 and Comparative Examples 1 to 4, it can be seen that the catalyst disclosed in the present invention can make benzene and toluene hydrogenated at a relatively low reaction temperature and normal pressure. According to the comparison of the data in Examples 2, 3 and 4, it can be seen that the parameters of the carrier in the catalyst meet the requirements of a pore size of 1 to 10 nm and a specific surface area of 300 to 800 m 2 / g, the content satisfies that the content of the carrier is 85-93% by weight and the content of the active metal oxide is 7-15% by weight based on the total weight of the catalyst, which can improve the conversion rate of the hydrogenation carrier and thus improve the hydrogen storage effect. In addition, the temperature matching of the hydrogen production device and the hydrogenation device disclosed in the present invention is good, and no heat supplementation is required during the hydrogenation reaction, which can not only reduce the difficulty of coupling the hydrogen storage device and the hydrogen production device, but also reduce the energy consumption of hydrogen storage treatment.
[0084] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0085] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0086] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A method for storing hydrogen energy, characterized in that: The method includes: The raw hydrogen produced by the hydrogen production device, the hydrogenation carrier and the catalyst are contacted in a hydrogenation reactor for hydrogen storage treatment to obtain a hydrogen storage product; the temperature of the hydrogen storage treatment is 25 to 90° C.; The hydrogenation carrier is selected from one or more aromatic hydrocarbons; The catalyst comprises a carrier and an active metal oxide; the carrier comprises a porous body with a pore size of 1-100 nm, and the active metal element in the active metal oxide is Ni.
2. The method according to claim 1, characterized in that The carrier includes MCM-41 porous body and / or SBA-15 porous body; The active metal oxide is NiO.
3. The method according to claim 2, characterized in that The carrier has a pore size of 1 to 10 nm and a specific surface area of 300 to 800 m 2 / g.
4. The method according to claim 2, characterized in that: Based on the total weight of the catalyst, the content of the carrier is 80-95 weight %; the content of the active metal oxide is 5-20 weight %.
5. The method according to claim 2, characterized in that: Based on the total weight of the catalyst, the content of the carrier is 85-93% by weight, and the content of the active metal oxide is 7-15% by weight.
6. The method according to claim 1, characterized in that The hydrogenation carrier is selected from aromatic hydrocarbons having 6 carbon atoms and / or aromatic hydrocarbons having 7 carbon atoms.
7. The method according to claim 6, characterized in that The hydrogenation carrier is benzene and / or toluene.
8. The method according to claim 1, characterized in that The conditions of the hydrogen storage treatment include: temperature of 25-80°C, pressure of 0.1-0.15 MPa, time of 2-10 seconds, volume space velocity of 0.5-5h -1 .
9. The method according to claim 1, characterized in that: The hydrogen content in the raw hydrogen is 50-100 volume %; the temperature of the raw hydrogen is 25-90°C.
10. The method according to claim 1, characterized in that Using the hydrogen storage product directly; and / or, The hydrogen storage product is transported to a dehydrogenation device for dehydrogenation treatment, and the obtained hydrogen enters a downstream hydrogen use device.