Method for preparing lithium bis (fluorosulfonyl) imide solution under low-temperature condition

By reacting lithium salts with carbonate solvents under low temperature conditions, lithium bisfluorosulfonyl imide is directly generated, which solves the problems of high reaction temperature and water generation in the existing technology, and achieves high purity and high yield of bisfluorosulfonyl imide. The preparation of lithium fluorosulfonyl imide is suitable for the application of new energy vehicle battery electrolyte.

CN118723944APending Publication Date: 2024-10-01WANHUA CHEM GRP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411047775.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing preparation method of lithium bisfluorosulfonyl imide has problems such as too high reaction temperature, excessive ion concentration caused by the generation of water, and difficulty in separating impurities, which affects the purity and yield of the product.

Method used

Mix lithium salt and carbonate solvent under low temperature conditions, and control the reaction temperature between 0 and 35°C to directly generate lithium bisfluorosulfonyl imide, avoiding the generation of water and impurities, and obtaining high purity through solid-liquid and gas-liquid separation. A solution of lithium bisfluorosulfonimide.

Benefits of technology

The preparation of lithium bisfluorosulfonimide with high purity and high yield is achieved. The operation is simple, the reaction conditions are mild, and no synthetic intermediates are required. It is green, efficient, and low-cost, and is suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723944A_ABST
    Figure CN118723944A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a lithium bis (fluorosulfonyl) imide solution under a low-temperature condition, which comprises the following steps: (1) mixing a lithium salt and a carbonic ester solvent to obtain a turbid liquid; (2) carrying out reaction on the turbid liquid and imidodisulfuryl fluoride at the temperature of 0-35 DEG C in the presence of inert gas to obtain a solution containing lithium imidodisulfuryl fluoride; and (3) sequentially carrying out solid-liquid separation and gas-liquid separation on the solution containing the lithium bis (fluorosulfonyl) imide to obtain the lithium bis (fluorosulfonyl) imide solution. The method is mild in reaction condition, water and other impurities difficult to separate are not generated in the reaction process, the lithium bis (fluorosulfonyl) imide solution is high in yield and purity, and the method has large-scale popularization and application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium battery materials, and in particular to a method for preparing a lithium bis(fluorosulfonyl)imide solution under low temperature conditions. Background Art

[0002] With the depletion of traditional fossil fuel reserves and the increasing severity of air pollution, fuel-powered vehicles are gradually being replaced by new energy vehicles. As the core energy storage device of new energy vehicles, lithium batteries, with their advanced technology and materials, will directly impact their promotion and development, and are currently attracting widespread attention from researchers. Lithium batteries primarily consist of a positive electrode, a negative electrode, an electrolyte, and a separator. The electrolyte, a key component of a lithium battery, carries the charge between the positive and negative electrodes. Its performance significantly impacts the battery's energy density, cyclability, lifespan, and safety.

[0003] Lithium bis(fluorosulfonyl)imide is a new type of electrolyte lithium salt. Compared with traditional lithium hexafluorophosphate, the lithium ions in lithium bis(fluorosulfonyl)imide are easier to dissociate and have higher conductivity. Its decomposition temperature is higher than 200°C. Its thermal stability and safety performance are significantly better than lithium hexafluorophosphate, and it has good compatibility with electrodes. It is a new type of electrolyte that has received widespread attention in the industry.

[0004] Currently, the most common synthesis route of lithium bis(fluorosulfonyl)imide is mainly divided into three steps: 1) chlorination reaction: synthesis of bis(chlorosulfonyl)imide; 2) fluorination reaction: further synthesis of bis(fluorosulfonyl)imide; 3) salt formation reaction: further synthesis of lithium bis(fluorosulfonyl)imide.

[0005] CN115231532A discloses a method for preparing lithium bis(fluorosulfonyl)imide. Bis(fluorosulfonyl)imide and lithium chloride are mixed at 125-150°C to react to obtain a crude product of lithium bis(fluorosulfonyl)imide, which is then dissolved, concentrated, crystallized, filtered, washed, and dried to obtain the product. The reaction temperature is too high, and bis(fluorosulfonyl)imide is easily decomposed to produce impurities at high temperatures. The product is dissolved, filtered, and recrystallized, which is cumbersome to operate and has high energy consumption. If lithium bis(fluorosulfonyl)imide is prepared by reacting bis(fluorosulfonyl)imide with an alkaline lithium reagent, water is inevitably generated in the system, and lithium salts are hydrolyzed when exposed to water, generating impurities that are difficult to separate, resulting in a low product yield. To solve this problem, CN114804043A and CN115367719A respectively use thionyl chloride to remove water and a solvent azeotropic dehydration method to remove the water generated by the reaction. However, the solution still needs to be crystallized again to obtain a qualified lithium bis(fluorosulfonyl)imide product. CN113800485A discloses a method for preparing lithium bis(fluorosulfonyl)imide, wherein bis(fluorosulfonyl)imide and lithium phosphate are reacted in a non-aqueous solvent to obtain a reaction solution containing lithium bis(fluorosulfonyl)imide, which is then filtered and the resulting filtrate is concentrated, crystallized, and dried to obtain the product. However, the reaction produces lithium dihydrogen phosphate as a by-product, resulting in loss of lithium, and a small amount of phosphoric acid may be generated in the reaction, which cannot be effectively separated from the product. CN115818591A discloses another method for preparing lithium bis(fluorosulfonyl)imide, wherein an ammonia source, an organic base, and SO2F are reacted to obtain a reaction solution containing lithium bis(fluorosulfonyl)imide. x Cl y The reaction is carried out in an organic solvent to first obtain an intermediate of a bisfluorosulfonyl imide salt, which is then reacted with a lithium source to prepare lithium bisfluorosulfonyl imide.

[0006] It can be seen that the current preparation method has problems such as excessively high reaction temperature, excessive ion concentration caused by reaction water, and difficult-to-separate impurities generated by the reaction. It is of great significance to continue to optimize the preparation process of lithium bis(fluorosulfonyl)imide. Summary of the Invention

[0007] In response to the problems existing in the prior art, the present invention provides a method for preparing a lithium bis(fluorosulfonyl)imide solution under low-temperature conditions. The method first involves mixing a lithium salt and a carbonate solvent, followed by adding a bis(fluorosulfonyl)imide and reacting the mixture. The resulting lithium bis(fluorosulfonyl)imide can be directly dissolved in the carbonate solvent. The reaction temperature is low, water and other difficult-to-separate impurities are not generated during the reaction, and no intermediates are required. This method produces a high-purity product, easily separates impurities, and allows for recycling of raw materials, resulting in a high yield. This method is a green, efficient, and low-cost process for preparing lithium bis(fluorosulfonyl)imide.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for preparing a lithium bis(fluorosulfonyl)imide solution under low temperature conditions, the method comprising the following steps:

[0010] (1) mixing a lithium salt and a carbonate solvent to obtain a suspension;

[0011] (2) reacting the suspension and bis(fluorosulfonyl)imide at a temperature of 0 to 35° C. in the presence of an inert gas to obtain a solution containing lithium bis(fluorosulfonyl)imide;

[0012] (3) The solution containing lithium bis(fluorosulfonyl)imide is sequentially subjected to solid-liquid separation and gas-liquid separation to obtain a lithium bis(fluorosulfonyl)imide solution.

[0013] The method for preparing a lithium bis(fluorosulfonyl)imide solution under low-temperature conditions disclosed herein first disperses a solid lithium salt in a carbonate solvent, and then dropwise adds liquid bis(fluorosulfonyl)imide (HFSI). The reaction occurs at extremely low temperatures and at a very high reaction rate. The generated lithium bis(fluorosulfonyl)imide (LiFSI) can be directly dissolved in the carbonate solvent, eliminating the step of preparing an electrolyte.

[0014] Taking lithium fluoride LiF as an example, the reaction equation is as follows:

[0015] HFSI+LiF→LiFSI+HF

[0016] If the bis(fluorosulfonyl)imide reacts incompletely, it will be difficult to remove from the lithium bis(fluorosulfonyl)imide solution. Therefore, the reaction needs to control the excess lithium fluoride. Excess lithium fluoride solids are insoluble in the system and can be removed by simple filtration. The filtered solids can be used as raw materials to participate in the reaction again. The hydrogen fluoride generated by the reaction has a boiling point of only 19°C at normal pressure. A simple nitrogen stripping can remove most of the hydrogen fluoride. The removal of hydrogen fluoride from the solution system can shift the reaction equilibrium to the right and increase the reaction conversion rate. In addition, the introduction of nitrogen can cause a strong disturbance to the solution in the reactor. With a reasonable design, the stirring paddle of the reactor can be omitted. The resulting solution containing lithium bis(fluorosulfonyl)imide still contains a small amount of hydrogen fluoride. After solid-liquid separation and gas-liquid separation, a qualified lithium bis(fluorosulfonyl)imide solution can be obtained.

[0017] The reaction temperature in step (2) of the present invention is 0-35°C, for example, it can be 0°C, 5°C, 8°C, 10°C, 15°C, 20°C or 35°C, but is not limited to the listed values. Other values ​​not listed within this numerical range are also applicable.

[0018] Preferably, the lithium salt in step (1) includes Li m A lithium compound of the form X, wherein m is a positive integer, X represents an anion with a valence of -m, and its corresponding hydride H m The boiling point of X at a pressure of 101 kPa is lower than 20°C and it will not decompose to produce water.

[0019] Preferably, the lithium salt in step (1) comprises any one or a combination of at least two of lithium fluoride, lithium chloride or lithium bromide, wherein typical but non-limiting combinations include a combination of lithium fluoride and lithium chloride, a combination of lithium bromide and lithium fluoride, or a combination of lithium chloride and lithium bromide.

[0020] Preferably, the carbonate solvent comprises any one of dimethyl carbonate, ethyl methyl carbonate or diethyl carbonate, or a combination of at least two thereof, wherein typical but non-limiting combinations include a combination of dimethyl carbonate and ethyl methyl carbonate, a combination of diethyl carbonate and dimethyl carbonate, or a combination of ethyl methyl carbonate and diethyl carbonate.

[0021] Preferably, the molar ratio of the carbonate solvent to the lithium salt is (3-5):1, for example, 3:1, 3.5:1, 3.8:1, 4:1, 4.3:1, 4.5:1, 4.7:1 or 5:1, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable; preferably (3.5-4.5):1.

[0022] Preferably, the molar ratio of the lithium salt to the bis(fluorosulfonyl)imide in step (1) is (1-1.2):1, for example, 1:1, 1.05:1, 1.08:1, 1.1:1, 1.15:1, 1.17:1 or 1.2:1, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; preferably, it is (1.05-1.1):1.

[0023] Preferably, the reaction temperature in step (2) is below 25°C, for example, it can be 25°C, 23°C, 20°C, 18°C, 15°C, 10°C or 5°C, etc., but is not limited to the listed values, and other unlisted values ​​within this numerical range are also applicable.

[0024] Preferably, the reaction pressure is 0 to 20 kPaG, for example, 0 kPaG, 3 kPaG, 5 kPaG, 10 kPaG, 15 kPaG, 18 kPaG or 20 kPaG, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable; preferably, it is below 5 PaG.

[0025] Preferably, the reaction in step (2) is carried out in n-stage continuous tank reactors connected in series, where n≥2, for example, 2, 3, 4, 5, 6 or 7, etc., but is not limited to the listed values, and other unlisted values ​​within this numerical range are also applicable; the liquid enters and exits from the top and flows by gravity to the next-stage continuous tank reactor.

[0026] The reaction of bisfluorosulfonyl imide with the suspension in the present invention involves an inert gas, liquid bisfluorosulfonyl imide and solid lithium salt, which is a three-phase heterogeneous reaction with low mass transfer efficiency. Therefore, it is necessary to design two or more fully mixed flow reactors in series.

[0027] Preferably, the residence time of the reaction in the n-stage continuous tank reactors connected in series is independently 30 min to 3 h, for example, it can be 30 min, 45 min, 50 min, 55 min, 1 h, 1.5 h, 2 h or 3 h, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; preferably 1 h.

[0028] Preferably, during the reaction in step (2), nitrogen is introduced to blow off the light components, and the light components enter the distillation tower to recover the carbonate solvent.

[0029] Preferably, the operating pressure of the distillation column is 0 to 20 kPaG, for example, 0 kPaG, 1 kPaG, 3 kPaG, 5 kPaG, 10 kPaG, 15 kPaG or 20 kPaG, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0030] The reflux ratio is 20 to 60, for example, 20, 30, 40, 50, 55 or 60, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0031] Preferably, the solid-liquid separation in step (3) comprises filtration.

[0032] The filtration of the present invention can adopt a filtration device with a backwashing function, and use a carbonate solvent to wash the insoluble matter back into the pulping kettle.

[0033] Preferably, the insoluble matter obtained by the solid-liquid separation is returned to step (1) for recycling.

[0034] Preferably, the gas-liquid separation in step (3) includes gas stripping.

[0035] Preferably, the gas stripping is carried out in a gas stripping tower.

[0036] Preferably, the operating pressure of the stripping tower is 1 to 20 kPaA, for example, 1 kPaA, 3 kPaA, 5 kPaA, 10 kPaA, 13 kPaA, 15 kPaA or 20 kPaA, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable; preferably, it is 5 kPaA.

[0037] The present invention can reduce the hydride concentration in the solution containing lithium bis(fluorosulfonyl)imide to a qualified level through gas stripping treatment, and the separated hydride can be returned for reuse.

[0038] As a preferred technical solution of the present invention, the method comprises the following steps:

[0039] (1) mixing a lithium salt and a carbonate solvent to obtain a suspension; the lithium salt comprises any one of lithium fluoride, lithium chloride, or lithium bromide, or a combination of at least two thereof; the carbonate solvent comprises any one of dimethyl carbonate, ethyl methyl carbonate, or diethyl carbonate, or a combination of at least two thereof; the molar ratio of the carbonate solvent to the lithium salt is (3-5):1;

[0040] (2) reacting the suspension and bis(fluorosulfonyl)imide at a temperature of 0 to 35° C. in the presence of an inert gas to obtain a solution containing lithium bis(fluorosulfonyl)imide;

[0041] The reaction pressure is 0-20 kPaG; the molar ratio of the lithium salt to the bis(fluorosulfonyl)imide is (1-1.2):1;

[0042] The reaction is carried out in n-stage continuous tank reactors connected in series, where n is greater than or equal to 2, and the liquid flows from top to bottom by gravity to the next-stage continuous tank reactor; the residence time of the reaction in the n-stage continuous tank reactors connected in series is independently 30 minutes to 3 hours;

[0043] The inert gas includes nitrogen; the inert gas is used for stirring and stripping light components, and the light components enter the distillation tower to recover carbonate solvents; the operating pressure of the distillation tower is 0 to 20 kPaG, and the reflux ratio is 20 to 60;

[0044] (3) The solution containing lithium bis(fluorosulfonyl)imide is sequentially subjected to solid-liquid separation and gas-liquid separation to obtain a lithium bis(fluorosulfonyl)imide solution;

[0045] The insoluble matter obtained from the solid-liquid separation is returned to step (1) for recycling; the gas stripping is carried out in a gas stripping tower; the operating pressure of the gas stripping tower is 1 to 20 kPaA.

[0046] Compared with the prior art, the present invention has at least the following beneficial effects:

[0047] The method for preparing a lithium bis(fluorosulfonyl)imide solution under low-temperature conditions provided by the present invention is simple to operate, has mild reaction conditions, does not generate water and other difficult-to-separate impurities during the reaction process, does not require the synthesis of intermediates, and the prepared lithium bis(fluorosulfonyl)imide solution has high purity and high yield. The method is a green, efficient, and low-cost lithium bis(fluorosulfonyl)imide preparation process and has prospects for large-scale promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 Schematic diagram of the apparatus system for preparing lithium bis(fluorosulfonyl)imide solution under low temperature conditions in Examples 1 to 6 of the present invention.

[0049] In the figure: 1-beating kettle; 2-first reactor; 3-second reactor; 4-filter; 5-gas stripping tower; 6-distillation tower; 7-lithium salt delivery pipeline; 8-carbonate solvent delivery pipeline; 9-insoluble matter delivery pipeline; 10-first nitrogen delivery pipeline; 11-second nitrogen delivery pipeline; 12-bis(fluorosulfonyl)imide delivery pipeline; 13-recycled solvent pipeline; 14-third nitrogen delivery pipeline; 15-vacuum pump; 16-bis(fluorosulfonyl)imide lithium solution delivery pipeline; 17-condenser; 18-reboiler. DETAILED DESCRIPTION

[0050] The technical solution of the present invention will be further described below with reference to the accompanying drawings and through specific implementation methods.

[0051] The schematic diagram of the apparatus system for preparing lithium bis(fluorosulfonyl)imide solution under low temperature conditions in the following Examples 1 to 6 is as follows: Figure 1 As shown, the device system includes a beating kettle 1, a first reactor 2, a second reactor 3, a filter 4, a stripping tower 5 and a distillation tower 6 connected in sequence;

[0052] The top of the beating kettle 1 is provided with a lithium salt delivery pipeline 7, a carbonate solvent delivery pipeline 8 and an insoluble matter delivery pipeline 9; the bottoms of the first reactor 2 and the second reactor 3 are respectively provided with a first nitrogen delivery pipeline 10 and a second nitrogen delivery pipeline 11; the top of the first reactor 2 is provided with a bis(fluorosulfonyl)imide delivery pipeline 12; the top of the filter 4 is provided with a recycled solvent pipeline 13; the filter 4 is connected to the beating kettle 1 via the insoluble matter delivery pipeline 9; the side of the stripping tower 5 is provided with a third nitrogen delivery pipeline 14; a vacuum pump 15 is provided between the stripping tower 5 and the distillation tower 6; the bottom of the stripping tower 5 is provided with a bis(fluorosulfonyl)imide lithium solution delivery pipeline 16; the top of the distillation tower is provided with a condenser 17; the bottom of the distillation tower is provided with a reboiler 18.

[0053] The present invention is further described in detail below. However, the following examples are merely simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0054] Example 1

[0055] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution under low temperature conditions, the method comprising the following steps:

[0056] (1) 69 g of lithium fluoride and 964 g of dimethyl carbonate were mixed in a stirred tank to obtain a suspension; the stirring speed of the stirred tank was 500 rpm;

[0057] (2) feeding the reactor 1 with a peristaltic pump at a rate of 258 g / h, and simultaneously adding bis(fluorosulfonyl)imide to the reactor 1 at a rate of 100 g / h to react to obtain a solution containing lithium bis(fluorosulfonyl)imide;

[0058] The stirring speed in reactor 1 is 500 rpm. When the liquid level reaches 60%, the solution in reactor 1 is fed to reactor 2 at a rate of 358 g / h via a peristaltic pump. Reactors 1 and 2 are each provided with a gas phase pipeline inserted below the liquid level, and nitrogen is introduced into the reactor at a rate of 200 g / h. Both reactors are placed in an ice-water bath, and the reaction temperature is controlled not to exceed 20° C. and the reaction pressure is 20 kPaG. The tail gas is condensed using ice water, the condensate is collected and stored, and the non-condensable gas is absorbed by alkaline solution and discharged into the tail gas system; the solution containing lithium bis(fluorosulfonyl)imide is produced from reactor 2; the residence time in both reactors is 30 minutes;

[0059] During the reaction, nitrogen is introduced to blow off light components, and the light components enter a distillation tower to recover carbonate solvents; 50 g of gaseous condensate from reactors 1 and 2 is collected and placed in a batch distillation tower kettle; the tower kettle is placed in an oil bath, the temperature of which is controlled at 90° C., the distillation tower uses random packing, has 20 theoretical plates, and the tower top pressure is controlled at 5 kPaG, and the tower top gas is condensed with ice water; the distillation tower is initially operated in a total reflux mode, and after the tower operation stabilizes, the tower top is extracted at a reflux ratio of 20:1, and the tower kettle temperature is always controlled at 90° C. After no liquid is extracted from the tower top, dimethyl carbonate after light removal is obtained in the tower kettle;

[0060] (3) The solution containing lithium bis(fluorosulfonyl)imide is filtered to obtain a solid and a clear liquid; the filtered solid is returned to step (1) for recycling, the clear liquid is added to the top of the stripping tower at a rate of 100 g / min, nitrogen is introduced into the bottom of the tower at a rate of 50 mL / min, the stripping tower uses random packing, the top of the tower is maintained at a pressure of 5 kPaA by a vacuum pump, and the bottom of the tower obtains a lithium bis(fluorosulfonyl)imide solution.

[0061] The dimethyl carbonate obtained in step (2) of this embodiment after light removal was analyzed by ion chromatography and gas chromatography. The dimethyl carbonate content was 99.9% and the HF content was 165 ppm, which met the requirements for carbonate recycling.

[0062] Example 2

[0063] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution under low temperature conditions, the method comprising the following steps:

[0064] (1) The solid obtained by filtration in Example 1 was dried, 10 g was weighed and added to a stirred tank, 964 g of dimethyl carbonate and 50 g of lithium fluoride solid were added thereto, and stirring was started at a stirring speed of 500 rpm;

[0065] (2) feeding the reactor 1 with a peristaltic pump at a rate of 256 g / h, and simultaneously adding bis(fluorosulfonyl)imide to the reactor 1 at a rate of 100 g / h to react to obtain a solution containing lithium bis(fluorosulfonyl)imide;

[0066] The stirring speed in reactor 1 is 500 rpm. When the liquid level reaches 60%, the solution in the reactor is fed to reactor 2 at a rate of 356 g / h via a peristaltic pump. Reactors 1 and 2 are each provided with a gas phase pipeline inserted below the liquid level, and nitrogen is introduced into the reactor at a rate of 200 g / h. Both reactors are placed in an ice-water bath, and the reaction temperature is controlled not to exceed 20° C. The reaction pressure is 5 kPaG. The tail gas is condensed using ice water, and the non-condensable gas is absorbed by alkaline solution and discharged into the tail gas system; the solution containing lithium bis(fluorosulfonyl)imide is produced from reactor 2; the residence time in both reactors is 1 hour;

[0067] During the reaction, nitrogen is introduced to blow off the light components, and the light components enter the distillation tower to recover the carbonate solvent; the operating pressure of the distillation tower is 10kPaG, and the reflux ratio is 20;

[0068] (3) The solution containing lithium bis(fluorosulfonyl)imide is filtered to obtain a solid and a clear liquid; the filtered solid is returned to step (1) for recycling, the clear liquid is added to the top of the stripping tower at a rate of 100 g / min, nitrogen is introduced into the bottom of the tower at a rate of 50 mL / min, the stripping tower uses random packing, the top of the tower is maintained at a pressure of 3 kPaA by a vacuum pump, and the bottom of the tower obtains a lithium bis(fluorosulfonyl)imide solution.

[0069] Example 3

[0070] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution under low temperature conditions, the method comprising the following steps:

[0071] (1) 211 g of lithium bromide and 767 g of ethyl methyl carbonate were mixed in a stirred tank to obtain a suspension; the stirring speed of the stirred tank was 400 rpm;

[0072] (2) feeding the reactor 1 with a peristaltic pump at a rate of 245 g / h, and simultaneously adding bis(fluorosulfonyl)imide to the reactor 1 at a rate of 100 g / h to react to obtain a solution containing lithium bis(fluorosulfonyl)imide;

[0073] The stirring speed in reactor 1 is 500 rpm. When the liquid level reaches 60%, the solution in reactor 1 is fed to reactor 2 at a rate of 345 g / h via a peristaltic pump. Reactors 1 and 2 are each provided with a gas phase pipeline inserted below the liquid level, and nitrogen is introduced into the reactor at a rate of 200 g / h. Both reactors are placed in an ice-water bath, and the reaction temperature is controlled not to exceed 10° C. and the reaction pressure is 10 kPaG. The tail gas is condensed using ice water, the condensate is collected and stored, and the non-condensable gas is absorbed by alkaline solution and discharged into the tail gas system; the solution containing lithium bis(fluorosulfonyl)imide is produced from reactor 2; the residence time in both reactors is 3 hours;

[0074] During the reaction, nitrogen is introduced to blow off the light components, and the light components enter the distillation tower to recover the carbonate solvent; the operating pressure of the distillation tower is 10kPaG, and the reflux ratio is 20;

[0075] (3) The solution containing lithium bis(fluorosulfonyl)imide is filtered to obtain a solid and a clear liquid; the filtered solid is returned to step (1) for recycling, the clear liquid is added to the top of the stripping tower at a rate of 120 g / min, nitrogen is introduced into the bottom of the tower at a rate of 50 mL / min, the stripping tower uses random packing, the top of the tower is maintained at a pressure of 15 kPaA by a vacuum pump, and the bottom of the tower obtains a lithium bis(fluorosulfonyl)imide solution.

[0076] Example 4

[0077] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution under low temperature conditions. The method is the same as that of Example 1, except that in step (1), 69 g of lithium fluoride and 477 g of dimethyl carbonate are mixed in a stirred tank, i.e., the molar ratio of lithium salt to carbonate solvent is 1:2.

[0078] Example 5

[0079] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution under low temperature conditions. The method is the same as that of Example 1, except that in step (1), 69 g of lithium fluoride and 1432 g of dimethyl carbonate are mixed in a stirred tank, i.e., the molar ratio of the lithium salt to the carbonate solvent is 1:6.

[0080] Example 6

[0081] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution under low temperature conditions. The method is the same as that of Example 1 except that the reaction pressure in step (2) is 25 kPaG.

[0082] Example 7

[0083] This embodiment provides a method for preparing a lithium bis(fluorosulfonyl)imide solution under low temperature conditions. The method is the same as that of Example 1, except that step (2) is only performed in the reactor 1 and the residence time is 1 hour.

[0084] Comparative Example 1

[0085] This comparative example provides a method for preparing a lithium bis(fluorosulfonyl)imide solution under low temperature conditions. The method is the same as Example 1 except that the reaction temperature in step (2) is -5°C.

[0086] Comparative Example 2

[0087] This comparative example provides a method for preparing a lithium bis(fluorosulfonyl)imide solution under low temperature conditions. The method is the same as Example 1 except that the reaction temperature in step (2) is 40°C.

[0088] Ion chromatography and gas chromatography were used to analyze the reaction yield, purity, acidity (in terms of HF), aminosulfonate ion content, and fluorosulfonate ion content of the above examples and comparative examples. The results are shown in Table 1.

[0089] Table 1

[0090]

[0091] From Table 1 we can see that:

[0092] (1) Based on Examples 1 to 3, it can be seen that the method for preparing lithium bis(fluorosulfonyl)imide solution under low temperature conditions provided by the present invention is simple to operate, has mild reaction conditions, and has a high yield and high purity of lithium bis(fluorosulfonyl)imide, which meets the quality standards of battery-grade electrolyte products.

[0093] (2) From Example 1 and Examples 4 to 5, it can be seen that the molar ratio of the lithium salt to the carbonate solvent in Example 4 is large, which will lead to a large adiabatic temperature rise of the reaction and difficulty in heat transfer. At the same time, the concentration of the product lithium bis(fluorosulfonyl)imide is too high, and part of the lithium bis(fluorosulfonyl)imide product fails to dissolve in the solvent and is filtered out along with the lithium fluoride, affecting the product yield. The molar ratio of the lithium salt to the carbonate solvent in Example 5 is small, which will lead to a decrease in the reaction mass transfer efficiency, severe reaction tailing, and a decrease in yield.

[0094] (3) Combining Example 1 and Example 6, it can be seen that the reaction pressure in Example 6 is relatively high, which makes it difficult to remove the generated light component impurities in the reactor, affecting the acidity of the product;

[0095] (4) From the perspective of Example 1 and Example 7, it can be seen that in Example 7, the reaction was carried out only in reactor 1, which resulted in incomplete reaction and low product yield.

[0096] (5) From Example 1 and Comparative Examples 1 to 2, it can be seen that the reaction temperature in Comparative Example 1 is relatively low, which will lead to a decrease in the reaction rate, and the light component impurities are not easy to remove, affecting the yield and acidity of the product; the reaction temperature in Comparative Example 2 is relatively high, which will lead to an increase in side reactions, excessively high concentrations of aminosulfonate ions and fluorosulfonate ions, and the product is prone to discoloration.

[0097] The applicant declares that the above is only a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention fall within the scope of protection and disclosure of the present invention.

Claims

1. A method for preparing a lithium bis(fluorosulfonyl)imide solution under low temperature conditions, characterized in that: The method comprises the following steps: (1) mixing a lithium salt and a carbonate solvent to obtain a suspension; (2) reacting the suspension and bis(fluorosulfonyl)imide at a temperature of 0 to 35° C. in the presence of an inert gas to obtain a solution containing lithium bis(fluorosulfonyl)imide; (3) The solution containing lithium bis(fluorosulfonyl)imide is sequentially subjected to solid-liquid separation and gas-liquid separation to obtain a lithium bis(fluorosulfonyl)imide solution.

2. The method according to claim 1, characterized in that The lithium salt in step (1) comprises Li m A lithium compound of the form X, wherein m is a positive integer, X represents an anion with a valence of -m, and its corresponding hydride H m The boiling point of X at a pressure of 101 kPa is lower than 20°C and it will not decompose to produce water.

3. The method according to claim 1 or 2, characterized in that: The lithium salt in step (1) includes any one of lithium fluoride, lithium chloride or lithium bromide, or a combination of at least two thereof; Preferably, the carbonate solvent includes any one of dimethyl carbonate, ethyl methyl carbonate or diethyl carbonate, or a combination of at least two thereof; Preferably, the molar ratio of the carbonate solvent to the lithium salt is (3-5):1, preferably (3.5-4.5):

1.

4. The method according to any one of claims 1 to 3, characterized in that: The molar ratio of the lithium salt to bis(fluorosulfonyl)imide in step (1) is (1-1.2):1, preferably (1.05-1.1):

1.

5. The method according to any one of claims 1 to 4, characterized in that: The reaction temperature in step (2) is below 25°C; Preferably, the reaction pressure is 0 to 20 kPaG, preferably below 5 PaG.

6. The method according to any one of claims 1 to 5, characterized in that: The reaction in step (2) is carried out in n-stage continuous tank reactors connected in series, where n≥2, and the liquid flows by gravity from top to bottom into the next-stage continuous tank reactor; Preferably, the residence time of the reaction in the n-stage continuous tank reactors connected in series is independently 30 min to 3 h, preferably 1 h.

7. The method according to any one of claims 1 to 6, characterized in that: The inert gas in step (2) comprises nitrogen; Preferably, the inert gas is used for stirring and stripping light components, and the light components enter the distillation tower to recover carbonate solvents; Preferably, the operating pressure of the distillation tower is 0-20 kPaG, and the reflux ratio is 20-60.

8. The method according to any one of claims 1 to 7, characterized in that: The solid-liquid separation in step (3) comprises filtration; Preferably, the insoluble matter obtained by the solid-liquid separation is returned to step (1) for recycling.

9. The method according to any one of claims 1 to 8, characterized in that: The gas-liquid separation in step (3) includes gas stripping; Preferably, the gas stripping is carried out in a gas stripping tower; Preferably, the operating pressure of the stripping tower is 1-20 kPaA, preferably 5 kPaA.

10. The method according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: (1) mixing a lithium salt and a carbonate solvent to obtain a suspension; the lithium salt comprises any one of lithium fluoride, lithium chloride or lithium bromide or a combination of at least two of them; the carbonate solvent comprises any one of dimethyl carbonate, ethyl methyl carbonate or diethyl carbonate or a combination of at least two of them; the molar ratio of the carbonate solvent to the lithium salt is (3-5):1; (2) reacting the suspension and bis(fluorosulfonyl)imide at a temperature of 0 to 35° C. in the presence of an inert gas to obtain a solution containing lithium bis(fluorosulfonyl)imide; The reaction pressure is 0-20 kPaG; the molar ratio of the lithium salt to the bis(fluorosulfonyl)imide is (1-1.2):1; The reaction is carried out in n-stage continuous tank reactors connected in series, n≥2, and the liquid flows by gravity from top to bottom to the next-stage continuous tank reactor; the residence time of the reaction in the n-stage continuous tank reactors connected in series is independently 30 minutes to 3 hours; The inert gas includes nitrogen; the inert gas is used for stirring and blowing off the light components, and the light components enter the distillation tower to recover the carbonate solvent; the operating pressure of the distillation tower is 0-20kPaG, and the reflux ratio is 20-60; (3) The solution containing lithium bis(fluorosulfonyl)imide is subjected to solid-liquid separation and gas-liquid separation in sequence to obtain a lithium bis(fluorosulfonyl)imide solution; The insoluble matter obtained by the solid-liquid separation is returned to step (1) for recycling; The gas stripping is carried out in a gas stripping tower; the operating pressure of the gas stripping tower is 1-20 kPaA.

Citation Information

Patent Citations

  • Process for the removal of HF from HF containing organic carbonates

    CN101981022A

  • Lithium bis (fluorosulfonyl) imide preparation process system

    CN217756905U

  • A continuous reaction device for synthesizing bis(chlorosulfonyl)imide

    CN220940642U

  • Method for Producing Lithium Bis(fluorosulfonyl)imide

    JP2018520981A

  • Substrate procesing apparatus

    KR1020250031394A