Preparation method and application of high-magnification long-cycle sodium ferric pyrophosphate material
By using complexation and reduction methods and carbon coating technology in sodium ferric pyrophosphate materials, the problem of poor cycle performance at high rates is solved, the material's efficient electrochemical performance is improved, and the process flow is simplified. It is compatible with the existing lithium iron phosphate production process, ensuring safety and industrial application prospects.
Patent Information
- Application Number
- CN202410985234.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The sodium ferric pyrophosphate material has poor cycle performance at high rates, and existing improvement methods have failed to effectively improve its capacity and cycle performance. The production process is complex, and there are great safety risks for equipment and operators.
Complexation and reduction methods are used to achieve uniform dispersion of materials at the molecular level, and ferric iron is reduced to divalent iron before sintering. Coupled with carbon coating, high-rate long cycles are prepared through sanding, spraying and sintering processes. Sodium iron pyrophosphate material.
The electrochemical performance of the material at high rates is improved, especially the capacity and cycle performance, and the process is simple, compatible with the existing lithium iron phosphate production process, and has good safety and industrial application prospects.
Smart Images

Figure CN118723965A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a preparation method and application of a high-rate and long-cycle sodium iron pyrophosphate material. Background Art
[0002] With the development of new energy, the demand for lithium-ion batteries is increasing, but lithium resources are limited. The working principle of sodium-ion batteries is the same as that of lithium-ion batteries. In comparison, sodium-ion batteries have advantages in resource abundance and material cost. At present, the research on positive electrode materials for sodium-ion batteries is mainly divided into three major systems: layered oxides, polyanions, and Prussian blue. Among them, sodium-ion layered oxide positive electrode materials have become the most industrialized materials due to their high specific capacity and convenient synthesis process. However, due to the unstable crystal structure and rapid capacity decay of this material, the cost is higher than that of the other two materials. Prussian blue materials have strict requirements on the production environment because the water in the crystal structure is difficult to control and remove. Polyanion materials, such as sodium iron pyrophosphate, have a production process that is compatible with the existing lithium iron phosphate process flow. The material has a stable crystal structure and good cycle performance, and has broad application prospects in energy storage. However, sodium iron pyrophosphate has the problem of low capacity and poor cycle at high rates.
[0003] To solve the above problems, Chinese patent CN117766710A discloses a "modified sodium ferric pyrophosphate positive electrode material, preparation method and application thereof", which introduces sulfate to increase the voltage platform and capacity, but the introduced sulfate is corrosive and poses a certain hazard to equipment and operators, and does not improve the material's cycle performance at high rates; CN117945378A provides a "method for doping multi-element modified sodium ferric pyrophosphate by sol-gel method", but does not substantially improve the material's capacity and cycle performance at high rates.
[0004] Therefore, it is of great significance to develop a preparation method and application of sodium iron pyrophosphate material with high rate and long cycle. Summary of the invention
[0005] The task of the present invention is to overcome the shortcomings of the prior art and propose a preparation method and application of a high-rate and long-cycle sodium iron pyrophosphate material, which can not only improve the electrochemical properties of the material, but also be compatible with the existing lithium iron phosphate production process, and the preparation method is simple and has good prospects for industrial application.
[0006] The preparation method of sodium iron pyrophosphate material with high rate and long cycle, in view of the problems of low capacity and poor cycle at high rate of sodium iron pyrophosphate, the complexation and reduction method is adopted to achieve uniform dispersion of the material at the molecular level, and at the same time, a reducing agent is added to reduce trivalent iron to divalent iron before sintering, and carbon coating is added, which is beneficial to improve the electrochemical performance of the material, especially the capacity and cycle performance at high rate. The specific process steps and conditions are as follows:
[0007] A. mixing a sodium source, an iron source, a phosphorus source, a carbon source, a complexing agent, and a reducing agent to obtain a slurry having a solid content of 20-60 wt %;
[0008] B. The mixed slurry is sequentially sand-milled, sprayed, and sintered to obtain the sodium iron pyrophosphate material.
[0009] The high-rate and long-cycle sodium iron pyrophosphate material is used in the positive electrode plate of a sodium ion battery.
[0010] Compared with the prior art, the present invention has the following advantages or effects:
[0011] Because of the complexation and reduction methods, uniform dispersion of materials at the molecular level can be achieved; at the same time, since trivalent Fe is reduced to divalent iron before sintering, coupled with doping modification and carbon coating, it is beneficial to improve the electrochemical properties of the material, especially the capacity and cycle performance at high rates; in addition, since it does not depend on changing the lithium iron phosphate production process, it is compatible with the existing lithium iron phosphate production process, and the method is simple and has good industrial prospects.
[0012] The sodium-ion battery involved in the application documents includes an electrolyte, a separator, a negative electrode sodium sheet and a positive electrode sheet. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a SEM image of the sodium iron pyrophosphate positive electrode material prepared according to Example 1 proposed by the present invention.
[0014] Figure 2 This is the SEM image of the sodium iron pyrophosphate positive electrode material prepared in Comparative Example 1.
[0015] Figure 3 XRD diagram of the sodium iron pyrophosphate positive electrode material prepared in Example 1 and Comparative Example 1.
[0016] Figure 4 This is a first cycle charge and discharge curve diagram of the sodium iron pyrophosphate positive electrode material prepared in Example 1 and Comparative Example 1.
[0017] Figure 5 This is a cycle capacity diagram of the sodium iron pyrophosphate positive electrode material prepared in Example 1 and Comparative Example 1.
[0018] The present invention is further described in detail below in conjunction with the accompanying drawings. DETAILED DESCRIPTION
[0019] like Figures 1 to 5 As shown, the preparation method of sodium iron pyrophosphate material with high rate and long cycle, in view of the problems of low capacity and poor cycle at high rate of sodium iron pyrophosphate, the complexation and reduction method is adopted to achieve uniform dispersion of the material at the molecular level, and at the same time, a reducing agent is added to reduce trivalent iron to divalent iron before sintering, and carbon coating is added, which is beneficial to improve the electrochemical performance of the material, especially the capacity and cycle performance at high rate. The specific process steps and conditions are as follows:
[0020] A. mixing a sodium source, an iron source, a phosphorus source, a carbon source, a complexing agent, and a reducing agent to obtain a slurry having a solid content of 20-60 wt %;
[0021] B. The mixed slurry is sequentially sand-milled, sprayed, and sintered to obtain the sodium iron pyrophosphate material.
[0022] The high-rate and long-cycle sodium iron pyrophosphate material is used in the positive electrode plate of a sodium ion battery.
[0023] The process of the present invention may further be:
[0024] The sodium source material in step A is any one or more of sodium carbonate, sodium hydroxide, sodium chloride, disodium hydrogen phosphate, disodium hydrogen phosphate dodecahydrate, sodium dihydrogen phosphate, sodium dihydrogen phosphate dihydrate, sodium borohydride, sodium formate, sodium acetate, sodium oxalate, sodium pyrophosphate, and sodium carboxymethyl cellulose.
[0025] The iron source material in step A is any one or more of ferric phosphate, ferric oxide, ferric sulfate, ferric chloride, ferric perchlorate, ferric hydroxide, ferric tribromide, ferrous dihydrogen phosphate, ferrous oxalate, ferric nitrate, ferric acetate, and ferric formate.
[0026] The phosphorus source material in step A is any one or more of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ferric phosphate, ferric dihydrogen phosphate, phosphorus pentoxide, phosphoric acid, disodium hydrogen phosphate, sodium dihydrogen phosphate, and disodium hydrogen phosphate and dodecahydrate.
[0027] The carbon source material in step A is any one or more of glucose, ethanol, methanol, propanol, acetone, formic acid, ethyl acetate, sucrose, isopropanol, starch, citric acid, maltose, sodium formate, sodium acetate, sodium oxalate, formic acid, acetic acid, oxalic acid, and sodium carboxymethyl cellulose.
[0028] The complexing agent in step A is any one or more of sodium tripolyphosphate, sodium pyrophosphate, sodium hexametaphosphate, ascorbic acid, N,N-dimethylformamide, N,N-dimethylacetamide, malic acid, malonic acid, succinic acid, succinic acid, glycolic acid, aminoacetic acid, lactic acid, tartaric acid, ethylenediaminetetraacetic acid, citric acid, mercaptopropanol, sodium dimercaptosuccinate, sodium dimercaptopropanesulfonate, penicillamine, sodium β-mercaptoethylamine formate, benzoic acid, phenylacetic acid, ethyl acetate, sodium acetate, hydroxyethylidene diphosphonic acid, sodium oxalate, aminotri(methylene)phosphonic acid, formic acid, acetic acid, oxalic acid, and sodium carboxymethyl cellulose.
[0029] The reducing agent in step A is any one or more of sodium thiosulfate, sodium thiophenol, ascorbic acid, N,N-dimethylformamide, N,N-dimethylacetamide, citric acid, sodium borohydride, formic acid, benzoic acid, phenylacetic acid, ethyl acetate, formaldehyde, acetaldehyde, maltose, acetic acid, erythritol, oxalic acid, ethyl formate, sodium formate, sodium oxalate, and sodium acetate.
[0030] The solid content of the slurry in step A is preferably 30-50 wt%.
[0031] The particle size d50 of the slurry after sand grinding in step B is 0.1-2.0 um.
[0032] The particle size d50 of the slurry after sand grinding in step B is preferably 0.1 to 0.4 um.
[0033] The spraying temperature of the slurry in step B is 100-250° C., and the particle size D50 of the sprayed material is 2-20 μm.
[0034] The spraying temperature of the slurry in step B is preferably 140-200° C., and the particle size D50 of the sprayed material is preferably 5-10 um.
[0035] The sintering conditions in step B are: firstly maintaining the temperature at 200-300°C for 3-5 hours, then maintaining the temperature at 500-700°C for 8-15 hours, the heating rate is 2-5°C / min, and the sintering atmosphere is any one or more of nitrogen and argon.
[0036] The sintering conditions in step B are preferably 300° C. and constant temperature for 3 hours, and then preferably 500-600° C. and constant temperature for 12 hours. The heating rate is preferably 3° C. / minute, and the sintering atmosphere is preferably a nitrogen atmosphere.
[0037] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.
[0038] Example 1
[0039] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof, and the preparation method steps are as follows:
[0040] Take 50g of iron oxide, 50g of iron phosphate, 30g of ammonium dihydrogen phosphate, 20g of sodium carbonate, 20g of disodium hydrogen phosphate, 10g of sodium hexametaphosphate, and 20g of sodium pyrophosphate and disperse them in 300ml of water, with a solid content of 44%, stir for 30 minutes, and the speed is 400rpm. Weigh 5g of sodium borohydride, 10g of ascorbic acid, and 15g of acetic acid, add them to the slurry, and continue stirring for 30 minutes. Then add the dispersed slurry to the sand mill for sand milling. The sand mill speed is set to 1000-2000rpm, and the sand milling time is 3 hours. At this time, the D50 of the test slurry is 0.3um. Take the slurry out of the sand mill, and then add 10g of malic acid and 10g of sodium carboxymethyl cellulose to the slurry. The slurry is then spray dried at a spray temperature of 200°C to obtain a spray material, and the spray material D50 is controlled to 5um. Part of the sprayed material was sintered in a tubular furnace. The sintering conditions were: constant temperature at 300°C for 3 hours, then constant temperature at 530°C for 8 hours, with a heating rate of 3°C / min. The sintering atmosphere was nitrogen. Finally, a positive electrode material with a chemical formula of Na4.11Fe3(P04)2P207 / C was obtained, and the C coating amount was 3%.
[0041] Example 2
[0042] The present embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Example 2 is that the amount of raw materials used in the present embodiment is: 50g iron oxide, 50g iron nitrate, 40g diammonium hydrogen phosphate, 20g sodium carbonate, 20g disodium hydrogen phosphate, 10g sodium hexametaphosphate, 20g sodium pyrophosphate, 5g sodium borohydride, 10g ascorbic acid, and 15g benzoic acid.
[0043] Example 3
[0044] The present embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Examples 1 and 2 is that the amount of raw materials used in the present embodiment is: 100g iron oxide, 40g diammonium hydrogen phosphate, 20g sodium carbonate, 20g disodium hydrogen phosphate, 10g sodium hexametaphosphate, 20g sodium pyrophosphate, 5g sodium borohydride, 10g ascorbic acid, and 15g benzoic acid.
[0045] Example 4
[0046] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Examples 1, 2, and 3 is that in this embodiment, the amount of raw materials used is: 100g iron phosphate, 40g diammonium hydrogen phosphate, 20g sodium carbonate, 20g disodium hydrogen phosphate, 10g sodium hexametaphosphate, 20g sodium pyrophosphate, 5g sodium borohydride, 10g ascorbic acid, 15g formic acid, and 10g manganese carbonate. The sintering conditions are constant temperature at 300°C for 3 hours, and then constant temperature at 500°C for 8 hours. Finally, a positive electrode material with a chemical formula of Na4.11Fe2.8Mn0.2(P04)2P207 / C is obtained.
[0047] Example 5
[0048] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Examples 1-4 is that the amount of raw materials used in this embodiment is: 100g of iron phosphate, 40g of diammonium hydrogen phosphate, 20g of sodium carbonate, 20g of disodium hydrogen phosphate, 10g of sodium hexametaphosphate, 20g of sodium pyrophosphate, 5g of sodium borohydride, 10g of ascorbic acid, 15g of formic acid, and 10g of vanadium pentoxide. The sintering conditions are constant temperature at 300°C for 3 hours, and then constant temperature at 500°C for 8 hours. Na4.11Fe2.65V0.35(P04)2P207 / C positive electrode material
[0049] Example 6
[0050] The present embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Example 1 is that in the present embodiment, the slurry is evaporated to dryness to form a gel-like substance by evaporation, and the gel-like substance is then placed in an oven and dried at 150°C for 12 hours. The dried material is then ground and sieved, and then placed in a tubular furnace for sintering to finally obtain the positive electrode material.
[0051] Example 7
[0052] The present embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Example 1 is that in the present embodiment, the slurry is evaporated to dryness to form a gel-like substance by evaporation, and then the gel-like substance is placed in an oven and dried at 200°C for 12 hours. The dried material is then ground and sieved, and then placed in a tubular furnace for sintering to finally obtain the positive electrode material.
[0053] Example 8
[0054] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Example 1 is that in this embodiment, the amount of water used is 553 ml, and the solid content is controlled to be 30%.
[0055] Example 9
[0056] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Examples 1 and 8 is that in this embodiment, the amount of water used is 236 ml and the solid content is 50%.
[0057] Example 10
[0058] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Example 1 is that in this embodiment, the sanding time is 6 hours and the slurry D50 is controlled to be 0.1 um.
[0059] Embodiment 11
[0060] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Examples 1 and 10 is that in this embodiment, the sanding time is 1 hour and the slurry D50 is controlled to be 0.4 um.
[0061] Example 12
[0062] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Example 1 is that in this embodiment, the slurry is spray-dried at a spray temperature of 140° C. to obtain a spray material.
[0063] Example 13
[0064] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Examples 1 and 14 is that in this embodiment, the slurry is spray-dried at a spray temperature of 250° C. to obtain a spray material.
[0065] Embodiment 14
[0066] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1, and the difference from Example 1 is that in this embodiment, the spray material D50 is controlled to 5 umm.
[0067] Embodiment 15
[0068] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Examples 1 and 16 is that in this embodiment, the spray material D50 is controlled to be 10 um.
[0069] Example 16
[0070] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Example 1 is that in this embodiment, the material is kept at a constant temperature of 500° C. for 8 hours.
[0071] Embodiment 17
[0072] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Examples 1 and 18 is that in this embodiment, the material is kept at a constant temperature of 550° C. for 8 hours.
[0073] Embodiment 18
[0074] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof, the preparation method is the same as that of Example 1, and the difference from Example 1 is that in this embodiment, the amount of raw material used is: 20g ascorbic acid. The C content of the final sintered product is 2%.
[0075] Embodiment 19
[0076] This embodiment provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof, the preparation method is the same as that of embodiment 1, and the difference from embodiments 1 and 20 is that in this embodiment, the amount of raw material used is: 40g ascorbic acid. The C content of the final sintered product is 4%.
[0077] Comparative Example 1
[0078] This comparative example provides a conventional sodium iron pyrophosphate positive electrode material and a preparation method thereof, and the preparation method steps are as follows:
[0079] Take 100g of iron phosphate, 33g of diammonium hydrogen phosphate and 50g of sodium carbonate and disperse them in 1000ml of water, stir for 30 minutes, and rotate at 400rpm. Weigh 60g of glucose, add it to the slurry, and continue stirring for 30 minutes. Then add the dispersed slurry to the sand mill for sand milling. The speed of the sand mill is 1000-2000rpm, and the sand milling time is 3 hours. At this time, the D50 of the test slurry is 0.35um. The slurry is then spray dried at a spray temperature of 200℃ to obtain a spray material. Take part of the spray material and sinter it in a tubular furnace. The sintering conditions are constant temperature at 300℃ for 3 hours, then constant temperature at 500℃ for 12 hours, the heating rate is 3℃ / min, and the sintering atmosphere is nitrogen. Finally, a positive electrode material with a chemical formula of Na4Fe3(P04)2P207 / C is obtained.
[0080] Comparative Example 2
[0081] This comparative example provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1, and the difference from Example 1 is that in this comparative example, reducing agents such as sodium borohydride, ascorbic acid, and acetic acid are not added.
[0082] Comparative Example 3
[0083] This comparative example provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that of Example 1, and the difference from Example 1 is that in this comparative example, no complexing agent such as sodium hexametaphosphate and sodium pyrophosphate is added.
[0084] Comparative Example 4
[0085] This comparative example provides a sodium iron pyrophosphate positive electrode material and a preparation method thereof. The preparation method is the same as that in Example 1. The difference from Example 1 is that in this comparative example, reducing agents such as sodium borohydride, ascorbic acid, acetic acid and complexing agents such as sodium hexametaphosphate and sodium pyrophosphate are not added.
[0086] Electrical performance test
[0087] The electrical performance of the sodium ion battery positive electrode materials obtained in each embodiment and comparative example was tested respectively, and the testing method is as follows:
[0088] The obtained sodium ion battery positive electrode material, polyvinylidene fluoride (PVDF), and conductive carbon black (SP) are mixed in a mass ratio of 8:1:1, and stirred evenly in a stirrer to form a positive electrode slurry with good fluidity. The positive electrode slurry is coated on an aluminum foil current collector, dried in a vacuum drying oven, and then punched into a pole piece. Then the sodium ion battery electrolyte, diaphragm, negative electrode sodium sheet, positive electrode sheet, and button battery shell are assembled in a vacuum glove box to obtain a CR2032 button battery. The prepared button battery is placed in a Xinwei battery test cabinet, and the first week discharge capacity is tested at a rate of 0.2C at a voltage of 2.0-4.0V, and then the discharge capacity is tested at a rate of 0.5C / 0.5C, 1C / 1C, 5C / 5C, and 10C / 10C. Finally, the cycle retention rate after 200 cycles is tested at a rate of 10C / 10C.
[0089] The test results are shown in Table 1.
[0090] Table 1 Test results
[0091]
[0092]
[0093] As described above, the present invention can be better implemented. The above embodiments are only the best implementation methods of the present invention, but the implementation methods of the present invention are not limited by the above embodiments. Other changes, modifications, replacements, combinations, and simplifications made without departing from the spirit and principle of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a high-rate and long-cycle sodium iron pyrophosphate material, which is characterized by the following problems: sodium iron pyrophosphate has low capacity and poor cycle at high rates. The complexation and reduction methods are used to achieve uniform dispersion of the material at the molecular level. At the same time, the addition of a reducing agent can reduce trivalent iron to divalent iron before sintering. In addition, carbon coating is beneficial to improve the electrochemical properties of the material, especially the capacity and cycle performance at high rates. The specific process steps and conditions are as follows: A. mixing a sodium source, an iron source, a phosphorus source, a carbon source, a complexing agent, and a reducing agent to obtain a slurry having a solid content of 20-60 wt %; B. The mixed slurry is sequentially sand-milled, sprayed, and sintered to obtain the sodium iron pyrophosphate material.
2. The method according to claim 1, characterized in that The sodium source material in step A is any one or more of sodium carbonate, sodium hydroxide, sodium chloride, disodium hydrogen phosphate, disodium hydrogen phosphate dodecahydrate, sodium dihydrogen phosphate, sodium dihydrogen phosphate dihydrate, sodium borohydride, sodium formate, sodium acetate, sodium oxalate, sodium pyrophosphate, and sodium carboxymethyl cellulose.
3. The method according to claim 1, characterized in that The iron source material in step A is any one or more of ferric phosphate, ferric oxide, ferric sulfate, ferric chloride, ferric perchlorate, ferric hydroxide, ferric tribromide, ferrous dihydrogen phosphate, ferrous oxalate, ferric nitrate, ferric acetate, and ferric formate.
4. The method according to claim 1, characterized in that The phosphorus source material in step A is any one or more of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ferric phosphate, ferric dihydrogen phosphate, phosphorus pentoxide, phosphoric acid, disodium hydrogen phosphate, sodium dihydrogen phosphate, and disodium hydrogen phosphate and dodecahydrate.
5. The method according to claim 1, characterized in that The carbon source material in step A is any one or more of glucose, ethanol, methanol, propanol, acetone, formic acid, ethyl acetate, sucrose, isopropanol, starch, citric acid, maltose, sodium formate, sodium acetate, sodium oxalate, formic acid, acetic acid, oxalic acid, and sodium carboxymethyl cellulose.
6. The method according to claim 1, characterized in that The complexing agent in step A is any one or more of sodium tripolyphosphate, sodium pyrophosphate, sodium hexametaphosphate, ascorbic acid, N,N-dimethylformamide, N,N-dimethylacetamide, malic acid, malonic acid, succinic acid, succinic acid, glycolic acid, aminoacetic acid, lactic acid, tartaric acid, ethylenediaminetetraacetic acid, citric acid, mercaptopropanol, sodium dimercaptosuccinate, sodium dimercaptopropanesulfonate, penicillamine, sodium β-mercaptoethylamine formate, benzoic acid, phenylacetic acid, ethyl acetate, sodium acetate, hydroxyethylidene diphosphonic acid, sodium oxalate, aminotri(methylene)phosphonic acid, formic acid, acetic acid, oxalic acid, and sodium carboxymethyl cellulose.
7. The method according to claim 1, characterized in that The reducing agent in step A is any one or more of sodium thiosulfate, sodium thiophenol, ascorbic acid, N,N-dimethylformamide, N,N-dimethylacetamide, citric acid, sodium borohydride, formic acid, benzoic acid, phenylacetic acid, ethyl acetate, formaldehyde, acetaldehyde, maltose, acetic acid, erythritol, oxalic acid, ethyl formate, sodium formate, sodium oxalate, and sodium acetate.
8. The method according to claim 1, characterized in that The solid content of the slurry in step A is preferably 30-50 wt%.
9. The method according to claim 1, characterized in that The particle size d50 of the slurry after sand grinding in step B is 0.1-2.0 um.
10. The method according to claim 1 or 9, characterized in that The particle size d50 of the slurry after sand grinding in step B is preferably 0.1 to 0.4 um.
11. The method according to claim 1, characterized in that The spraying temperature of the slurry in step B is 100-250° C., and the particle size D50 of the sprayed material is 2-20 μm.
12. The method according to claim 1 or 11, characterized in that The spraying temperature of the slurry in step B is preferably 140-200° C., and the spraying particle size D50 is preferably 5-10 um.
13. The method according to claim 1, characterized in that The sintering conditions in step B are: firstly maintaining the temperature at 200-300°C for 3-5 hours, then maintaining the temperature at 500-700°C for 8-15 hours, the heating rate is 2-5°C / min, and the sintering atmosphere is any one or more of nitrogen and argon.
14. The method according to claim 1 or 13, characterized in that The sintering conditions in step B are preferably 300° C. and constant temperature for 3 hours, and then preferably 500-600° C. and constant temperature for 12 hours. The heating rate is preferably 3° C. / minute, and the sintering atmosphere is preferably a nitrogen atmosphere.
15. The application of the high-rate and long-cycle sodium iron pyrophosphate material is characterized in that Used in positive electrode plates of sodium ion batteries.