Resin-based hard carbon based on aromatic group steric hindrance effect as well as preparation method and application of resin-based hard carbon

By introducing aromatic group condensation polymerization and high-temperature pyrolysis carbonization into resin-derived hard carbon materials, a resin-based hard carbon with high sodium storage capacity and good cycle performance is formed, which solves the problem of insufficient performance of existing resin-derived hard carbon materials and achieves Performance improvement and industrial application of sodium-ion batteries.

CN118723972AActive Publication Date: 2024-10-01江西云威新材料股份有限公司 +1

Patent Information

Application Number
CN202410732015.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-01
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

Existing resin-derived hard carbon anode materials have problems such as low sodium storage capacity, low first Coulombic efficiency, and poor rate performance. Moreover, it is difficult to control the microstructure due to the technology of polymer cross-linked structure, which affects the performance of sodium-ion batteries.

Method used

By introducing the polycondensation of aldehyde compounds containing aromatic groups and phenolic compounds to form phenolic resin, and performing pyrolysis and carbonization at high temperatures, a resin-based hard carbon material with rich micron-scale closed pore structure and high thermal stability is formed, and its microscopic properties are adjusted. Structure to improve sodium storage capacity and cycle stability.

Benefits of technology

It achieves high sodium storage capacity, improved first-time Coulombic efficiency and rate performance, simplifies the preparation process, is suitable for large-scale production, and advances the industrialization process of sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723972A_ABST
    Figure CN118723972A_ABST
Patent Text Reader

Abstract

The invention provides resin-based hard carbon based on an aromatic group steric hindrance effect as well as a preparation method and application thereof, and belongs to the technical field of sodium-ion battery negative electrode materials. According to the invention, aldehyde monomers containing aromatic groups and phenolic monomers are subjected to condensation polymerization to obtain a phenolic resin hard carbon precursor, and then the phenolic resin hard carbon precursor is sequentially subjected to post-curing and high-temperature pyrolysis carbonization to prepare the aromatic group steric hindrance effect-based resin-based hard carbon. The aromatic group contained in the side chain of the phenolic resin can change the steric hindrance of the polymer and construct pi-pi accumulation, and the free volume in the resin and the rigidity of the molecular chain are improved; furthermore, excessive graphitization of a carbon layer can be effectively inhibited in the subsequent carbonization process, and formation of a large number of closed pores is promoted. The aromatic group steric hindrance strategy provided by the invention plays a positive role in regulating and controlling the microstructure of the hard carbon material, and the resin-based hard carbon material shows high specific capacity and first coulombic efficiency when being used as a negative electrode of a sodium-ion battery, and also has relatively good rate capability and cycle stability characteristic.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of negative electrode materials for sodium ion batteries, and particularly relates to resin-based hard carbon based on the steric hindrance effect of aromatic groups, and a preparation method and application thereof. Background Art

[0002] Since its commercialization, lithium-ion batteries have played a very important role in new energy fields such as mobile power supplies and electric vehicles; however, with the increasing demand for energy storage, the problems of limited lithium resources and uneven distribution have gradually become prominent. Sodium ions are highly similar to lithium ions. At the same time, sodium elements have large reserves, wide distribution, and low prices, which can alleviate the problem of lithium resource shortages. Therefore, the development of sodium-ion batteries is more suitable for the construction of the next generation of large-scale energy storage systems. However, current sodium-ion batteries are severely limited by negative electrode materials, especially the traditional graphite negative electrode, which has different sodium and lithium storage mechanisms and cannot store sodium with larger ion radius. + Effective electrochemical storage, therefore, the development of new negative electrode materials has become a research hotspot in this field. Hard carbon is composed of closed pores formed by the curling of disordered chaotic layers of graphite microcrystals and nanodomains. It has the characteristics of small crystallite size, large interlayer spacing, and a large number of micron-level closed pores. It is a good choice for negative electrode materials for sodium ion batteries. However, the current resin-derived hard carbon negative electrode materials have problems such as low specific capacity, low first coulombic efficiency, and poor rate performance. In addition, due to the influence of the polymer cross-linked structure, the technical energy barrier for regulating the microstructure of resin-derived hard carbon at the molecular level is high. To solve the above problems, domestic and foreign research teams have done a lot of work on this. Hu Yongsheng's research group used ethanol vapor to generate pores in the cross-linked phenolic resin during the solvothermal process, and converted them into closed pores during the subsequent high-temperature carbonization process, increasing the sodium storage capacity to 410mAh / g (ACS Energy Lett. 2019, 4, 2608-2612). Although the above method improves the electrochemical properties of resin-based carbon materials to a certain extent, the ethanol solvothermal method is limited by the reactor process and is not conducive to large-scale production. Shinichi Komaba's team used polyvinyl alcohol as a pore-forming agent, formaldehyde and maleic anhydride as a cross-linking agent and catalyst in a liquid phenolic resin system to prepare a microporous phenolic resin precursor for the preparation of hard carbon. The hard carbon material exhibited a high specific capacity of 386 mAh / g at a current density of 10 mA / g (ACS Appl. Energy Mater. 2020, 3, 135-140), but its high specific surface area resulted in a low first coulombic efficiency, which made it difficult to meet commercial applications. Therefore, it is urgent to develop a method for preparing a resin-based hard carbon material with a simple process and easy commercialization, so that the prepared hard carbon material has both high sodium storage capacity and first coulombic efficiency, as well as good cycle performance and rate performance. Summary of the invention

[0003] In view of this, the purpose of the present invention is to provide a resin-based hard carbon based on the steric hindrance effect of aromatic groups and a preparation method and application thereof, aiming to solve at least one technical problem in the background technology.

[0004] The present invention is achieved through the following technical solutions:

[0005] The present invention provides a method for preparing resin-based hard carbon based on the steric hindrance effect of aromatic groups, the preparation method comprising:

[0006] Step (1): stirring and mixing an aldehyde compound containing an aromatic group, a phenolic compound, ethanol and a sodium hydroxide solution, heating and polycondensing in a condensation reflux device until gelation, and air-drying at room temperature to obtain a phenolic resin containing a steric hindrance effect of an aromatic ring group;

[0007] Step (2): transferring the phenolic resin obtained in step (1) to a muffle furnace for post-curing, washing with deionized water, filtering, and drying;

[0008] Step (3): The phenolic resin obtained in step (2) is subjected to high-temperature pyrolysis and carbonization under the protection of an inert atmosphere to obtain the resin-based hard carbon material.

[0009] Preferably, the phenolic resin containing the steric hindrance effect of the aromatic ring group obtained in step (1) has the structure shown in the following formulas (1) to (3):

[0010]

[0011] In Formulae 1 to 3, R represents a side chain group containing an aromatic ring.

[0012] Preferably, the aromatic ring side chain group R contained in the phenolic resin has a structure as shown in the following formulas (1) to (4):

[0013]

[0014] Preferably, the thermal decomposition temperature of the aromatic ring-containing side chain group R is 400-600°C.

[0015] Preferably, the molar ratio of the aldehyde compound, the phenolic compound and the sodium hydroxide in step (1) is 1.25:1:0.55.

[0016] Preferably, the heating polycondensation temperature in step (1) is 60° C., and the heating polycondensation time is 10-25 h.

[0017] Preferably, the post-curing temperature of step (2) is 200° C. and the post-curing time is 2 hours.

[0018] Preferably, the high-temperature pyrolysis carbonization temperature of step (3) is 1200-1500° C., and the carbonization time is 1-3 h.

[0019] The second aspect of the present invention provides resin-based hard carbon based on the steric hindrance effect of aromatic groups obtained by the above preparation method.

[0020] The third aspect of the present invention provides the use of the resin-based hard carbon based on the steric hindrance effect of the aromatic group obtained by the above preparation method in the preparation of negative electrode materials for sodium ion batteries.

[0021] Compared with the prior art, the present invention has the following advantages and technical effects:

[0022] (1) The preparation process of the present invention is simple, the hard carbon yield is high, and large-scale production is easy to achieve.

[0023] (2) The present invention introduces an aldehyde compound containing an aromatic group to undergo a polycondensation reaction with a phenolic compound to form a phenolic resin with a large side group, thereby adjusting the steric hindrance of the polymer side chain and increasing the spatial free volume of the resin, which helps to form a richer micron-level closed-pore structure during the carbonization process of the phenolic resin and improve the reversible sodium storage capacity of the resin-based hard carbon;

[0024] (3) The aromatic side chain groups introduced in the present invention have a relatively high thermal stability temperature (400-600°C) and construct π-π stacking to enhance the rigidity of the molecular chain, which can improve the stability of the carbon skeleton structure during the high-temperature carbonization process of phenolic resin, reduce the number of cracking and rearrangement, and effectively inhibit the excessive graphitization of the carbon layer, forming a carbon layer with a large interlayer spacing and short-range disorder, and promoting the intercalation / deintercalation and diffusion of sodium ions, thereby improving the cycle stability and rate performance of hard carbon.

[0025] Therefore, the present invention provides a method for preparing resin-based hard carbon based on the steric hindrance effect of aromatic groups, which enables the hard carbon material to have both high sodium storage capacity and first coulombic efficiency, as well as good cycle performance and rate performance, which is conducive to promoting the industrialization process of sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The infrared spectra of the phenolic resin containing vinylphenyl side chain groups prepared in Example 1 of the present invention at different pyrolysis temperatures;

[0027] Figure 2 The first cycle charge and discharge curve diagram of the battery prepared in Example 1 of the present invention;

[0028] Figure 3 This is a rate performance curve diagram of the battery prepared in Example 1 of the present invention;

[0029] Figure 4This is a cycle stability curve of the battery prepared in Example 1 of the present invention.

[0030] Figure 5 The first cycle charge and discharge curve of the battery prepared in Comparative Example 1 of the present invention;

[0031] Figure 6 This is a rate performance curve of the battery prepared in Comparative Example 1 of the present invention;

[0032] Figure 7 This is a cycle stability curve of the battery prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific implementation cases described herein are only used to explain the present invention and are not intended to limit the present invention. The experimental methods in the following embodiments are conventional methods unless otherwise specified.

[0034] Example 1

[0035] 1) 2 g of resorcinol and 9 mL of anhydrous ethanol were added to a three-necked flask. After the resorcinol was completely dissolved, 2.8 mL of cinnamaldehyde was added. After stirring for 10 minutes, 10 mL of 1 mol / L sodium hydroxide aqueous solution was added. The mixture was heated at 60° C. for 20 hours under a condensation reflux device, and finally polycondensed to gelation. The molecular structure of the gel product in step 1) is shown below:

[0036]

[0037] Wherein, R is a vinylphenyl side chain group.

[0038] 2) The gel product obtained in step 1) is air-dried at room temperature, then transferred to a muffle furnace and cured at 200° C. for 2 h, and then ground into powder after cooling to room temperature, washed and filtered with deionized water, and dried in a blast oven at 80° C. for 24 h to obtain a phenolic resin containing vinylphenyl side chain groups.

[0039] 3) The phenolic resin obtained in step 2) is carbonized at 1400° C. for 1 hour under the protection of an argon inert atmosphere to obtain the resin-based hard carbon material based on the steric hindrance effect of the vinylphenyl group.

[0040] 4) The resin-based hard carbon material obtained in step 3) is used as the negative electrode, metallic sodium is used as the counter electrode, glass fiber is used as the separator, and 1MNaPF6 in DIGLYME (diethylene glycol dimethyl ether) is used as the electrolyte, and a sodium ion battery is assembled under an argon atmosphere.

[0041] Figure 1The infrared spectra of the phenolic resin containing vinylphenyl side chain groups obtained in Example 1 at different pyrolysis temperatures show that: the characteristic infrared peak of the vinylphenyl group (~699cm -1 ) still exists at 400-600℃, proving that it effectively improves the thermal stability of the carbon skeleton.

[0042] Figure 2 The first cycle charge and discharge curve of the resin-based hard carbon material based on the steric hindrance effect of the vinylphenyl group obtained in Example 1 when applied to a sodium ion battery shows that the hard carbon negative electrode material for the sodium ion battery has a first coulombic efficiency of up to 88.5% and a reversible specific capacity of 340.3 mAh / g.

[0043] Figure 3 The rate performance curve of the resin-based hard carbon material based on the steric hindrance effect of the vinylphenyl group obtained in this embodiment 1 when applied to a sodium ion battery shows that the reversible specific capacity of the hard carbon negative electrode material for a sodium ion battery at a current density of 5C (1C = 30mA / g) is 210.7mAh / g.

[0044] Figure 4 This is the cycle stability curve of the resin-based hard carbon material based on the steric hindrance effect of the vinylphenyl group obtained in Example 1 applied to sodium ion batteries. It can be seen that the sodium ion battery hard carbon negative electrode material can be stably cycled for 1000 cycles at a current density of 2C, and the cycle capacity retention rate is higher than 86.4%.

[0045] Compared with Comparative Example 1, Example 1 can significantly improve the comprehensive electrochemical performance of its resin-based hard carbon negative electrode material due to the steric hindrance effect of the vinylphenyl group.

[0046] Comparative Example 1

[0047] 1) 2 g of resorcinol and 9 mL of anhydrous ethanol were added to a three-necked flask. After the resorcinol was completely dissolved, 1.6 mL of 37 wt% formaldehyde solution was added. After stirring for 10 minutes, 10 mL of 1 mol / L sodium hydroxide aqueous solution was added. The mixture was heated at 60° C. for 20 hours under a condensation reflux device and finally polycondensed to gelation.

[0048] 2) The gel product obtained in step 1) is air-dried at room temperature, then transferred to a muffle furnace and cured at 200° C. for 2 h, and then ground into powder after cooling to room temperature, washed and filtered with deionized water, and dried in a blast oven at 80° C. for 24 h to obtain a phenolic resin without any aromatic ring side chain group modification.

[0049] 3) The phenolic resin obtained in step 2) is carbonized at 1400° C. for 1 hour under the protection of an argon inert atmosphere to obtain the resin-based hard carbon material without any aromatic ring side chain group modification.

[0050] 4) The resin-based hard carbon material obtained in step 3) is used as the negative electrode, metallic sodium is used as the counter electrode, glass fiber is used as the separator, and 1MNaPF6 in DIGLYME (diethylene glycol dimethyl ether) is used as the electrolyte, and a sodium ion battery is assembled under an argon atmosphere.

[0051] Figure 5 From the first cycle charge and discharge curve of the resin-based hard carbon material without any aromatic ring side chain group modification obtained in Comparative Example 1 and applied to a sodium ion battery, it can be seen that the sodium ion battery hard carbon negative electrode material has a first coulombic efficiency of 83.7% and a reversible specific capacity of 302.7 mAh / g.

[0052] Figure 6 The rate performance curve of the resin-based hard carbon material without any aromatic ring side chain group modification obtained in Comparative Example 1 applied to a sodium ion battery shows that the reversible specific capacity of the sodium ion battery hard carbon negative electrode material at a current density of 5C (1C = 30mA / g) is only 79.5mAh / g.

[0053] Figure 7 This is the cycle stability curve of the resin-based hard carbon material without any aromatic ring side chain group modification obtained in Comparative Example 1 applied to sodium ion batteries. It can be seen that the sodium ion battery hard carbon negative electrode material can stably cycle 1000 times at a current density of 2C, and the cycle capacity retention rate decays to 76.2%.

[0054] Example 2

[0055] 1) Take 2g of resorcinol and 9mL of anhydrous ethanol and add them into a three-necked flask. After the resorcinol is completely dissolved, add 4.1g of p-phenylbenzaldehyde, stir for 10 minutes, then add 10mL of 1mol / L sodium hydroxide aqueous solution, heat at 60°C in a condensation reflux device for 20h, and finally condense to gelation.

[0056] 2) The gel product obtained in step 1) is air-dried at room temperature, then transferred to a muffle furnace for curing at 200° C. for 2 h, ground into powder after cooling to room temperature, washed and filtered with deionized water, and dried in a forced air oven at 80° C. for 24 h to obtain a phenolic resin containing a biphenyl group having a steric hindrance effect.

[0057] 3) The phenolic resin obtained in step 2) is carbonized at 1400° C. for 1 hour under the protection of an argon inert atmosphere to obtain the resin-based hard carbon material based on the steric hindrance effect of the biphenyl group.

[0058] 4) The resin-based hard carbon material obtained in step 3) is used as the negative electrode, metallic sodium is used as the counter electrode, glass fiber is used as the separator, and 1MNaPF6 in DIGLYME (diethylene glycol dimethyl ether) is used as the electrolyte, and a sodium ion battery is assembled under an argon atmosphere.

[0059] Example 3

[0060] 1) Take 2g of resorcinol and 9mL of anhydrous ethanol and add them into a three-necked flask. After the resorcinol is completely dissolved, add 2.2mL of 5-methylfurfural, stir for 10 minutes, then add 10mL of 1mol / L sodium hydroxide aqueous solution, heat at 60°C under a condensation reflux device for 20h, and finally condense to gelation.

[0061] 2) The gel product obtained in step 1) is air-dried at room temperature, then transferred to a muffle furnace for curing at 200° C. for 2 h, ground into powder after cooling to room temperature, washed and filtered with deionized water, and dried in a forced air oven at 80° C. for 24 h to obtain a phenolic resin containing a steric hindrance effect of a 5-methylfuran group.

[0062] 3) The phenolic resin obtained in step 2) is carbonized at 1400° C. for 1 hour under the protection of an argon inert atmosphere to obtain the resin-based hard carbon material based on the steric hindrance effect of the 5-methylfuran group.

[0063] 4) The resin-based hard carbon material obtained in step 3) is used as the negative electrode, metallic sodium is used as the counter electrode, glass fiber is used as the separator, and 1MNaPF6 in DIGLYME (diethylene glycol dimethyl ether) is used as the electrolyte, and a sodium ion battery is assembled under an argon atmosphere.

[0064] Table 1: Sodium ion battery test results of Example 13 and Comparative Example 1

[0065] Group First cycle reversible capacity First coulombic efficiency Rate performance (5C) Example 1 340.3mAh / g 88.5% 210.7mAh / g Comparative Example 1 302.7mAh / g 83.7% 79.5mAh / g Example 2 334.3mAh / g 88.1% 258.9mAh / g Example 3 321.8mAh / g 88.3% 205.4mAh / g

[0066] (Note: 5C = 1500mA / g)

[0067] It can be seen from Table 1 that the first-cycle reversible capacity and first coulomb efficiency of Examples 1 to 3 are significantly better than those of Comparative Example 1, indicating that the steric hindrance effect of the aromatic group can bring a larger spatial free volume and molecular chain rigidity to the resin, thereby effectively regulating the microstructure of the resin-based hard carbon during the pyrolysis carbonization process, forming a more compact short-range graphitized carbon layer and more abundant closed pores, thereby improving the reversible sodium storage capacity of the hard carbon. In addition, the rate performance of Examples 1 to 3 still maintains a capacity of more than 200mAh / g at a current density of 5C, which is better than Comparative Example 1. This shows that the steric hindrance effect of the aromatic group can reduce the number of pyrolysis rearrangements during the pyrolysis process of the resin, forming a more short-range disordered carbon layer structure, which is conducive to the rapid diffusion of sodium ions, thereby improving the rate performance of the battery. In addition, Example 2 has the best rate performance (258.9 mAh / g), indicating that a larger number of benzene rings in biphenyl can bring higher thermal stability, effectively inhibit excessive graphitization of the carbon layer and form a larger graphite layer spacing, confirming that reasonable aromatic groups have a positive effect on constructing a high-rate resin-based hard carbon negative electrode.

[0068] Example 4

[0069] 1) 1.71 g of phenol and 9 mL of anhydrous ethanol were added to a three-necked flask. After the resorcinol was completely dissolved, 2.8 mL of cinnamaldehyde was added. After stirring for 10 minutes, 10 mL of 1 mol / L sodium hydroxide aqueous solution was added. The mixture was heated at 60° C. for 10 hours under a condensation reflux device, and finally polycondensed to gelation. The molecular structure of the gel product in step 1) is shown below:

[0070]

[0071] Wherein, R is a vinylphenyl side chain group.

[0072] 2) The gel product obtained in step 1) is air-dried at room temperature, then transferred to a muffle furnace and cured at 200° C. for 2 h, and then ground into powder after cooling to room temperature, washed and filtered with deionized water, and dried in a blast oven at 80° C. for 24 h to obtain a phenolic resin containing vinylphenyl side chain groups.

[0073] 3) The phenolic resin obtained in step 2) is carbonized at 1400° C. for 1 hour under the protection of an argon inert atmosphere to obtain the resin-based hard carbon material based on the steric hindrance effect of the vinylphenyl group.

[0074] 4) The resin-based hard carbon material obtained in step 3) is used as the negative electrode, metallic sodium is used as the counter electrode, glass fiber is used as the separator, and 1MNaPF6 in DIGLYME (diethylene glycol dimethyl ether) is used as the electrolyte, and a sodium ion battery is assembled under an argon atmosphere.

[0075] Example 5

[0076] 1) 2.29 g of phloroglucinol and 9 mL of anhydrous ethanol were added to a three-necked flask. After the phloroglucinol was completely dissolved, 2.8 mL of cinnamaldehyde was added. After stirring for 10 minutes, 10 mL of 1 mol / L sodium hydroxide aqueous solution was added. The mixture was heated at 60° C. for 25 hours under a condensation reflux device, and finally polycondensed to gelation. The molecular structure of the gel product of step 1) is shown below:

[0077]

[0078] Wherein, R is a vinylphenyl side chain group.

[0079] 2) The gel product obtained in step 1) is air-dried at room temperature, then transferred to a muffle furnace and cured at 200° C. for 2 h, and then ground into powder after cooling to room temperature, washed and filtered with deionized water, and dried in a blast oven at 80° C. for 24 h to obtain a phenolic resin containing vinylphenyl side chain groups.

[0080] 3) The phenolic resin obtained in step 2) is carbonized at 1200° C. for 3 h under the protection of an argon inert atmosphere to obtain the resin-based hard carbon material based on the steric hindrance effect of the vinylphenyl group.

[0081] 4) The resin-based hard carbon material obtained in step 3) is used as the negative electrode, metallic sodium is used as the counter electrode, glass fiber is used as the separator, and 1MNaPF6 in DIGLYME (diethylene glycol dimethyl ether) is used as the electrolyte, and a sodium ion battery is assembled under an argon atmosphere.

[0082] Example 6

[0083] 1) Take 2 g of resorcinol and 9 mL of anhydrous ethanol and add them into a three-necked flask. After the resorcinol is completely dissolved, add 2.4 g of benzaldehyde, stir for 10 minutes, then add 10 mL of 1 mol / L sodium hydroxide aqueous solution, heat at 60° C. in a condensation reflux device for 20 hours, and finally condense to gelation.

[0084] 2) The gel product obtained in step 1) is air-dried at room temperature, then transferred to a muffle furnace for curing at 200° C. for 2 h, ground into powder after cooling to room temperature, washed and filtered with deionized water, and dried in a blast oven at 80° C. for 24 h to obtain a phenolic resin containing a steric hindrance effect of a benzyl group.

[0085] 3) The phenolic resin obtained in step 2) is carbonized at 1500° C. for 1 hour under the protection of an argon inert atmosphere to obtain the resin-based hard carbon material based on the steric hindrance effect of the biphenyl group.

[0086] 4) The resin-based hard carbon material obtained in step 3) is used as the negative electrode, metallic sodium is used as the counter electrode, glass fiber is used as the separator, and 1MNaPF6 in DIGLYME (diethylene glycol dimethyl ether) is used as the electrolyte, and a sodium ion battery is assembled under an argon atmosphere.

[0087] The above embodiments are preferred implementations of the present invention and are only used to explain the present invention, not to limit the present invention. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principle of the present invention shall be equivalent replacement modes and shall be included in the protection scope of the present invention.

Claims

1. A method for preparing resin-based hard carbon based on the steric hindrance effect of aromatic groups, characterized in that: The preparation method comprises the following steps: The aldehyde compound containing aromatic groups, phenolic compounds, ethanol and sodium hydroxide solution are stirred and mixed, heated and polycondensed in a condensation reflux device until gelation occurs, and air-dried at room temperature to obtain a phenolic resin containing a steric hindrance effect of an aromatic ring group; The phenolic resin is transferred to a muffle furnace for post-curing, and then washed, filtered and dried with deionized water; The phenolic resin after curing is subjected to high-temperature pyrolysis and carbonization under the protection of an inert atmosphere to obtain the resin-based hard carbon.

2. The method for preparing resin-based hard carbon based on the steric hindrance effect of aromatic groups according to claim 1, characterized in that: The phenolic resin containing the steric hindrance effect of the aromatic group has a structure shown in one of formulas (1) to (3): In formulae (1) to (3), R represents a side chain group containing an aromatic ring.

3. The method for preparing resin-based hard carbon based on the steric hindrance effect of aromatic groups according to claim 2, characterized in that: The aromatic ring-containing side chain group R is one of the following formulas (1) to (4):

4. The method for preparing resin-based hard carbon based on the steric hindrance effect of aromatic groups according to claim 2 or 3, characterized in that: The R is an aromatic ring side chain group with a thermal decomposition temperature of 400 to 600°C.

5. The method for preparing resin-based hard carbon based on the steric hindrance effect of aromatic groups according to claim 1, characterized in that: The molar ratio of the aldehyde compound, the phenol compound and the sodium hydroxide is 1.25:1:0.

55.

6. The method for preparing resin-based hard carbon based on the steric hindrance effect of aromatic groups according to claim 1, characterized in that: The temperature of the heating polycondensation is 60° C., and the heating polycondensation time is 10-25 hours.

7. The method for preparing resin-based hard carbon based on the steric hindrance effect of aromatic groups according to claim 1, characterized in that: The post-curing temperature is 200° C. and the post-curing time is 2 hours.

8. The method for preparing resin-based hard carbon based on the steric hindrance effect of aromatic groups according to claim 1, characterized in that: The temperature of the high-temperature pyrolysis carbonization is 1200-1500° C. and the time is 1-3 hours.

9. Resin-based hard carbon based on the steric hindrance effect of aromatic groups obtained by the preparation method according to any one of claims 1 to 8.

10. Use of the resin-based hard carbon based on the steric hindrance effect of aromatic groups obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The resin-based hard carbon based on the steric hindrance effect of the aromatic group is used as the negative electrode material of the sodium ion battery.

Citation Information

Patent Citations

  • Modified hard carbon negative electrode material and preparation method thereof

    CN111029578A

  • Aromatic phenolic resin-based hard carbon material, sodium ion battery and preparation method of sodium ion battery

    CN116812904A

  • Mesoporous carbons

    GB0019417D0

  • Spherical phenol resin cured product, spherical carbon and manufacturing method of spherical activated carbon

    JP2020169299A

Cited By

  • Polyimide-based porous carbon and preparation method thereof, silicon-carbon electrode material and battery

    CN122187037A