One-step pressure-induced coal-based compact hard carbon negative electrode material, preparation method thereof and low-temperature sodium ion battery
Through a one-step pressure-induced preparation method of coal-based dense hard carbon materials, the problem of complex process and low efficiency of sodium-ion battery anode materials has been solved, and efficient and controllable preparation of sodium-ion battery anode materials has been achieved, which has significantly improved the performance of sodium-ion battery anode materials in low-temperature environments. Performance.
Patent Information
- Application Number
- CN202411075882.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-10-01
AI Technical Summary
The existing sodium-ion battery anode materials have complex preparation processes, low efficiency, and poor controllability, which limit the performance of sodium-ion batteries in low-temperature environments, especially in applications in severely cold areas.
A one-step pressure-induced coal-based dense hard carbon negative electrode material preparation method is adopted, and a coal-based hard carbon material with high tap density is obtained through physical pressing and one-step thermal carbonization of the delimed coal precursor without the need for long-term gas phase pre-oxidation. Or other auxiliary materials, adjust the pressure and time during the pressing process to control the growth space and closed pore structure of the carbon sheet.
The hard carbon anode material has achieved high density and high sodium storage performance, significantly improved the tap density, first-cycle Coulombic efficiency and low-voltage platform capacity, improved the performance advantages of sodium-ion batteries at low temperatures, simplified the process flow and reduced the cost.
Smart Images

Figure CN118723974A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion battery negative electrode materials, and in particular to a one-step pressure-induced coal-based dense hard carbon negative electrode material and a preparation method thereof, and a low-temperature sodium ion battery. Background Art
[0002] The accelerated advancement of global energy transformation has promoted the demand for large-scale, low-cost energy storage devices in the energy storage market. As a low-cost, resource-rich energy storage solution, sodium-ion batteries are gradually attracting widespread attention. However, the poor performance of existing sodium-ion batteries in low-temperature environments limits their widespread application in cold regions, especially in electric vehicles and outdoor energy storage systems. The research on high-energy-density sodium-ion batteries has important scientific significance and practical value for realizing large-scale energy storage and its application in low-temperature and harsh environments. The long sodium storage platform and high density of the negative electrode at low potential are of vital importance to improving the battery energy density. Therefore, the development of new negative electrode materials with high tap density, first-week coulomb efficiency and low-potential platform capacity is the key to the development of high-energy-density sodium-ion battery negative electrode materials.
[0003] Carbon materials have the advantages of stable chemical properties, designable morphology and structure, diverse preparation methods, and low cost, and are widely used as negative electrode materials for sodium ion batteries. Although coal is used as raw material, coal-based carbon materials can be obtained through coal selection and carbonization, but the carbon materials obtained by directly carbonizing anthracite with a high degree of metamorphism have a high degree of order and low sodium storage capacity; while lignite with a low degree of metamorphism has the problems of low carbonization yield and low material tap density. Researchers can improve the electrochemical sodium storage performance of coal-based carbon materials through pre-oxidation treatment, template method, chemical vapor deposition method and other means, but there are problems such as complex process flow, the need to add template agents or activators, and the need for template removal process. In the application of pressing process, one or more auxiliary raw materials are usually required to achieve cross-linking polymerization. Before pressing, the raw materials need to be ball-milled and mixed. During the pressing process, a mold of a special shape is required. After being pressed into tablets, multiple preliminary treatments such as preheating and activation are required, and finally carbonization is performed to obtain a multi-phase composite material. However, there are problems with the phase interface, including large ion diffusion resistance, difficulty in controlling the uniformity of multiphase mixing, reduced volume energy density, etc. The above existing processes all lead to increased preparation costs and difficult to control the process, making it difficult to achieve practical application.
[0004] In summary, there is an urgent need to develop a low-cost, simple, efficient, and highly controllable method for preparing carbon negative electrode materials for sodium ion batteries to meet the current demand for sodium ion batteries in the energy storage field. Summary of the invention
[0005] The purpose of the present invention is to provide a one-step pressure-induced coal-based dense hard carbon negative electrode material and a preparation method thereof and a low-temperature sodium ion battery, so as to solve the technical problems of complex preparation process, low efficiency and poor controllability of the existing sodium ion battery negative electrode material.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a one-step pressure-induced method for preparing a coal-based dense hard carbon negative electrode material, comprising the following steps:
[0008] (1) crushing the deashed coal precursor and physically pressing it into a dense body;
[0009] (2) carbonizing the dense body under protective gas, and then crushing and acid washing to obtain a coal-based hard carbon negative electrode material;
[0010] The carbonization treatment is a one-step heat treatment, and the temperature of the one-step heat treatment is 1000-2200° C. Further, the coal precursor subjected to the deashing treatment comprises one or more of lignite, bituminous coal, anthracite, coal tar, petroleum tar, coal coke and petroleum coke.
[0011] Furthermore, the crushed particle size is ≤200 mesh.
[0012] Furthermore, the pressure of the physical pressing is 0.5 to 50 MPa, and the time of the physical pressing is 1 to 30 min.
[0013] Furthermore, the protective gas includes an inert gas or a vacuum environment.
[0014] Furthermore, the one-step heat treatment lasts for 1 to 8 hours, and the heating rate is 0.5 to 10° C. / min.
[0015] The invention also provides a coal-based dense hard carbon negative electrode material.
[0016] The present invention also provides a low-temperature sodium ion battery, which is assembled from a negative electrode sheet, a counter electrode and a GF / D glass fiber separator;
[0017] The negative electrode sheet is obtained by coating a mixture of coal-based dense hard carbon negative electrode material, acetylene black and sodium carboxymethyl cellulose on a copper foil; the counter electrode is a sodium sheet.
[0018] Beneficial effects of the present invention:
[0019] 1. The present invention can obtain a dense hard carbon material with high tap density by carbonization after strengthening the cross-linking between carbon precursor molecules by simple physical compression. It does not require long-term gas phase pre-oxidation or HNO3 liquid phase oxidation to promote cross-linking, nor does it require other auxiliary materials such as templates and activators or complicated processing processes to obtain a hard carbon negative electrode material with high density and high sodium storage performance.
[0020] 2. By regulating the pressure and time of the pressing process, the degree of cross-linking between precursor molecules can be adjusted, the spatial distribution density and intermolecular distance of the precursor molecules can be adjusted, thereby controlling the growth space of the carbon sheet layer and adjusting the closed-pore structure in the hard carbon, thereby achieving an increase in high tap density and high-capacity storage of sodium ions at low potential. The coal-based dense hard carbon negative electrode material induced by one-step pressure has controllable microstructure.
[0021] 3. The coal-based dense hard carbon based on one-step pressure induction described in the present invention is applied as the negative electrode material of sodium ion battery. Compared with the carbon material obtained without pressing or without controlling the pressing pressure, this method can achieve simultaneous and significant improvement in tap density, first-week coulomb efficiency and specific capacity, and significantly improve the capacity of the low-voltage platform below 0.1V, and has obvious performance advantages at low temperatures. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 A schematic diagram of the molecular aggregation morphology and carbon structure in the one-step pressure-induced method for preparing coal-based dense hard carbon of the present invention;
[0023] Figure 2 This is a transmission electron microscope image of a coal-based dense hard carbon negative electrode material obtained by the one-step pressure-induced coal-based dense hard carbon preparation method obtained in Example 1;
[0024] Figure 3 This is a scanning electron microscope image of a coal-based dense hard carbon negative electrode material obtained by the one-step pressure-induced coal-based dense hard carbon preparation method obtained in Example 1;
[0025] Figure 4 The XRD spectrum of the coal-based dense hard carbon negative electrode material obtained by the one-step pressure-induced coal-based dense hard carbon preparation method obtained in Comparative Example 1;
[0026] Figure 5 Transmission electron microscope images of coal-based dense hard carbon negative electrode materials obtained in Examples 4, 5, 6 and Comparative Example 1;
[0027] Figure 6The cyclic voltammetry curves of the sodium ion batteries obtained in Examples 1, 4, 6 and Comparative Example 1, wherein (a) is the cyclic voltammetry curve of the sodium ion battery obtained in Example 1, (b) is the cyclic voltammetry curve of the sodium ion battery obtained in Example 4, (c) is the cyclic voltammetry curve of the sodium ion battery obtained in Example 6, and (d) is the cyclic voltammetry curve of the sodium ion battery obtained in Comparative Example 1;
[0028] Figure 7 The constant current charge and discharge curves of the sodium ion batteries obtained in Examples 1, 4, 6 and Comparative Example 1 are shown. DETAILED DESCRIPTION
[0029] The present invention provides a one-step pressure-induced method for preparing a coal-based dense hard carbon negative electrode material, comprising the following steps:
[0030] (1) crushing the deashed coal precursor and physically pressing it into a dense body;
[0031] (2) carbonizing the dense body under protective gas, and then crushing and acid washing to obtain a coal-based hard carbon negative electrode material;
[0032] The carbonization treatment is a one-step heat treatment, and the temperature of the one-step heat treatment is 1000-2200°C.
[0033] In the present invention, the temperature of the one-step heat treatment is preferably 1150-1800°C, more preferably 1200-1700°C, and even more preferably 1400-1500°C.
[0034] In the present invention, the deashing coal precursor comprises one or more of lignite, bituminous coal, anthracite, coal tar, petroleum tar, coal coke and petroleum coke, preferably one or more of lignite, bituminous coal, anthracite and coal tar.
[0035] In the present invention, the crushed particle size is ≤200 mesh.
[0036] In the present invention, the physical pressing pressure is 0.5 to 50 MPa, preferably 1 to 40 MPa, more preferably 3 to 30 MPa, and more preferably 5 to 20 MPa; the physical pressing time is 1 to 30 min, preferably 5 to 25 min, more preferably 8 to 20 min, and more preferably 10 to 18 min.
[0037] In the present invention, the protective gas comprises an inert gas or a vacuum environment, preferably an inert gas, more preferably one or more of argon, nitrogen, helium and neon, more preferably argon and / or nitrogen.
[0038] In the present invention, the time of the one-step heat treatment is 1 to 8 hours, preferably 2 to 7 hours, and more preferably 3 to 6 hours; the heating rate is 0.5 to 10°C / min, preferably 1 to 9°C / min, more preferably 2 to 8°C / min, and more preferably 3 to 6°C / min.
[0039] The invention also provides a coal-based dense hard carbon negative electrode material.
[0040] The present invention also provides a low-temperature sodium ion battery, which is assembled from a negative electrode sheet, a counter electrode and a GF / D glass fiber separator;
[0041] The negative electrode sheet is obtained by coating a mixture of coal-based dense hard carbon negative electrode material, acetylene black and sodium carboxymethyl cellulose on a copper foil; the counter electrode is a sodium sheet.
[0042] In the present invention, the mass ratio of the coal-based dense hard carbon negative electrode material, acetylene black and sodium carboxymethyl cellulose is preferably 92:3:5.
[0043] In the present invention, the preparation method of the low-temperature sodium ion battery comprises the following steps:
[0044] Coal-based dense hard carbon negative electrode material, acetylene black, and sodium carboxymethyl cellulose were weighed in a mass ratio of 92:3:5 and then evenly coated on copper foil. After drying at 60°C for 12 hours, a battery electrode was obtained. The active material loading of the negative electrode was greater than 1 mg cm -2 The obtained battery pole piece was used as the working electrode, the sodium sheet was used as the counter electrode, the separator was made of GF / D glass fiber, and the electrolyte was 1M NaPF6 (the solvent included ethylene carbonate and diethyl carbonate, with a volume ratio of 1:1). All assembly processes were carried out in a glove box.
[0045] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0046] Example 1
[0047] This embodiment provides a one-step pressure-induced method for preparing a coal-based dense hard carbon negative electrode, and the process flow is as follows: Figure 1 As shown, the preparation method comprises the following steps: weigh 10g of deashed lignite, crush it and pass it through a 200-mesh sieve, press it into blocks by a powder press, the pressing pressure is 5MPa, and the pressing time is 10 minutes. Put it into an alumina crucible, place it in a tubular furnace under argon protection, and carbonize it at high temperature at 5℃min -1 The heating rate was increased to 1500°C and kept warm for 3 hours. After crushing, the product was pickled to obtain a coal-based dense hard carbon negative electrode material.
[0048] The coal-based dense hard carbon negative electrode material obtained in this example is in powder form, and its tap density is 0.83 g·cm -3 , ID / IG value is 1.10, specific surface area is 2.6m 2 ·g -1 .
[0049] Figure 2 The transmission electron microscope image of the coal-based dense hard carbon negative electrode material obtained in this embodiment is shown. It can be seen from the image that the coal-based dense hard carbon has a large number of closed-pore structures formed by stacking microcrystals.
[0050] Figure 3 The scanning electron microscope image of the coal-based dense hard carbon negative electrode material obtained in this example is shown. It can be seen from the image that the coal-based dense hard carbon particles present a typical irregular shape.
[0051] Figure 4 The XRD spectrum of the coal-based dense hard carbon negative electrode material obtained in this embodiment is shown. It can be seen from the figure that the XRD spectrum of the coal-based dense hard carbon shows two broad diffraction peaks at 22° and 43°, which are typical diffraction peaks of the (002) and (100) crystal planes in disordered carbon.
[0052] Figure 6 (a) shows the cyclic voltammetry curve of the coal-based dense hard carbon negative electrode material obtained in this embodiment. It can be seen from the figure that the coal-based dense hard carbon obtained in this embodiment has good redox reversibility and cycle stability, and the irreversible capacity of the first cycle is small;
[0053] Figure 7 The charge-discharge curve of the coal-based dense hard carbon negative electrode material prepared in this embodiment is shown. It can be seen from the figure that the coal-based hard carbon presents a typical charge-discharge curve. The discharge curve consists of a high-voltage slope segment and a low-voltage platform segment. It has a high first coulomb efficiency (86.4%) and a high reversible capacity (365.8 mAh g -1 ), the platform capacity below 0.1V is 242mAh·g -1 .
[0054] This embodiment also provides a low-temperature sodium ion battery with the coal-based dense hard carbon as the negative electrode material. The electrochemical test results of the sodium ion battery at low temperature are as follows: the reversible capacity of the sodium ion battery at 0°C is 327.4 mAh·g -1 , the reversible capacity is 267.5 mAh g at -30 °C -1 .
[0055] Example 2
[0056] The one-step pressure-induced preparation method of coal-based dense hard carbon negative electrode comprises the following steps: weighing 10g of deashed anthracite, crushing it and passing it through a 200-mesh sieve, pressing it into blocks by a powder press, pressing it at a pressure of 5MPa for 10 minutes, placing it in an alumina crucible, placing it in a tubular furnace for high-temperature carbonization, passing argon protective gas, and heating it at 5℃min -1 The heating rate was increased to 1500°C and kept warm for 3 hours. After crushing, the product was pickled to obtain a coal-based dense hard carbon material.
[0057] The coal-based dense hard carbon negative electrode material obtained in this example is in powder form, and its tap density is 0.96 g·cm -3 , ID / IG value is 1.06, specific surface area is 2.2m 2 ·g -1 .
[0058] This embodiment also provides a sodium ion battery using the coal-based dense hard carbon as the negative electrode material. The electrochemical test results of the sodium ion battery are as follows: the sodium ion battery has a high first coulomb efficiency (91.5%), a high reversible capacity (322.5 mAh·g -1 ), the platform capacity below 0.1V is 212mAh·g -1 The reversible capacity of sodium ion battery at 0°C is 291.4 mAh g -1 The reversible capacity is 244.6 mAh g at -30 °C. -1 .
[0059] Example 3
[0060] The one-step pressure-induced preparation method of coal-based dense hard carbon sodium negative electrode comprises the following steps: weighing 10g of deashed bituminous coal, crushing it and passing it through a 200-mesh sieve, pressing it into blocks by a powder press, the pressing pressure is 5MPa, and the pressing time is 10 minutes. Put it into an alumina crucible, place it in a tubular furnace for high-temperature carbonization, pass argon protective gas, and heat it at 5℃min -1 The heating rate was increased to 1500°C and kept warm for 3 hours. After crushing, the product was pickled to obtain a coal-based dense hard carbon material.
[0061] The coal-based dense hard carbon negative electrode material obtained in this example has a powdery morphology and a tap density of 0.86 g·cm -3 , ID / IG value is 1.08, specific surface area is 2.4m 2 ·g -1 .
[0062] This embodiment also provides a sodium ion battery using the coal-based dense hard carbon as the negative electrode material. The electrochemical test results of the sodium ion battery are as follows: the sodium ion battery has a high first coulomb efficiency (90.2%), a high reversible capacity (355.3 mAh·g-1 ), the platform capacity below 0.1V is 224mAh·g -1 The reversible capacity of sodium ion battery at 0°C is 325.6 mAh g -1 The reversible capacity is 259.3 mAh g at -30 °C. -1 .
[0063] Example 4
[0064] The difference between this embodiment and embodiment 1 is that the pressing pressure of the crushed lignite in step (1) is 2 MPa.
[0065] The coal-based dense hard carbon negative electrode material obtained in this example has a powdery morphology and a tap density of 0.78 g·cm -3 , ID / IG value is 1.05, specific surface area is 3.4m 2 ·g -1 .
[0066] Figure 5 The transmission electron microscope image of the coal-based dense hard carbon negative electrode material obtained in this embodiment is shown. It can be seen from the image that the coal-based dense hard carbon obtained in this embodiment has a small amount of short-range microcrystals stacked in a staggered manner, and the proportion of disordered regions is high.
[0067] Figure 6 (b) shows the cyclic voltammetry curve of the coal-based dense hard carbon negative electrode material obtained in this embodiment. It can be seen from the figure that the coal-based dense hard carbon obtained in this embodiment has good redox reversibility and cycle stability, and the irreversible capacity of the first cycle is small;
[0068] Figure 7 The charge-discharge curve of the coal-based dense hard carbon negative electrode material prepared in this embodiment is shown. It can be seen from the figure that the coal-based hard carbon presents a typical charge-discharge curve. The discharge curve consists of a high-voltage slope segment and a low-voltage platform segment. The first charge-discharge capacity is 304.5 mAh g -1 The first coulombic efficiency is 77.7%, and the platform capacity below 0.1V is 172mAh·g -1 .
[0069] Example 5
[0070] The difference between this embodiment and embodiment 1 is that the pressing pressure of the crushed lignite in step (1) is 15 MPa.
[0071] The rest of the preparation methods and parameters were the same as those in Example 1.
[0072] This embodiment also provides a coal-based dense hard carbon negative electrode material for sodium electricity. The coal-based dense hard carbon has a powdery morphology and a tap density of 0.89 g cm -3, ID / IG value is 1.08, specific surface area is 4.2m 2 ·g -1 .
[0073] Figure 5 The transmission electron microscope image of the coal-based dense hard carbon negative electrode material obtained in this embodiment is shown. It can be seen from the image that the coal-based dense hard carbon obtained in this embodiment has a large number of closed-pore structures formed by stacking microcrystals.
[0074] This embodiment also provides a sodium ion battery using the coal-based dense hard carbon as the negative electrode material. The electrochemical test results of the sodium ion battery are as follows: the sodium ion battery has a high first coulomb efficiency (82.4%), a high reversible capacity (344.2 mAh·g -1 ), the platform capacity below 0.1V is 202mAh·g -1 .
[0075] Example 6
[0076] The difference between this embodiment and embodiment 1 is that the pressing pressure of the crushed lignite in step (1) is 25 MPa.
[0077] The rest of the preparation methods and parameters were the same as those in Example 1.
[0078] This embodiment also provides a coal-based dense hard carbon negative electrode material for sodium electricity. The coal-based dense hard carbon has a powdery morphology and a tap density of 0.91 g cm -3 , ID / IG value is 1.02, specific surface area is 5.9m 2 ·g -1 .
[0079] Figure 5 The transmission electron microscope image of the coal-based dense hard carbon negative electrode material obtained in this embodiment is shown. It can be seen from the image that the coal-based dense hard carbon obtained in this embodiment has more long-range ordered graphite-like crystallites and fewer closed-pore structures formed by short-range crystallite stacking.
[0080] Figure 6 (c) shows the cyclic voltammetry curve of the coal-based dense hard carbon negative electrode material obtained in this embodiment. It can be seen from the figure that the coal-based dense hard carbon obtained in this embodiment has good redox reversibility and cycle stability, and the irreversible capacity of the first cycle is small;
[0081] Figure 7 The charge and discharge curve of the coal-based dense hard carbon negative electrode material prepared in this embodiment is shown. It can be seen from the figure that the coal-based hard carbon presents a typical charge and discharge curve. The discharge curve consists of a high-voltage slope section and a low-voltage platform section. The first coulomb efficiency is 79.5%, and the first-cycle reversible specific capacity is 332.5 mAh g -1 , the platform capacity below 0.1V is 164mAh·g-1 .
[0082] Example 7
[0083] The difference between this embodiment and embodiment 1 is that the pressing pressure of the crushed lignite in step (1) is 50 MPa.
[0084] The rest of the preparation methods and parameters were the same as those in Example 1.
[0085] Example 8
[0086] The difference between this embodiment and embodiment 1 is that the pressing pressure of the crushed lignite in step (1) is 5 MPa and the pressing time is 1 min.
[0087] The rest of the preparation methods and parameters were the same as those in Example 1.
[0088] Example 9
[0089] The difference between this embodiment and embodiment 1 is that the pressing pressure of the crushed lignite in step (1) is 5 MPa and the pressing time is 30 min.
[0090] The rest of the preparation methods and parameters were the same as those in Example 1.
[0091] Example 10
[0092] The difference between this embodiment and embodiment 1 is that the carbonization treatment in step (2) is: -1 The heating rate was increased to 1200°C and kept at this temperature for 3 hours.
[0093] The rest of the preparation methods and parameters were the same as those in Example 1.
[0094] Embodiment 11
[0095] The difference between this embodiment and embodiment 1 is that the carbonization treatment in step (2) is: -1 The heating rate was increased to 1800°C and kept at this temperature for 3 h.
[0096] The rest of the preparation methods and parameters were the same as those in Example 1.
[0097] Comparative Example 1
[0098] The difference between this comparative example and Example 1 is that no pressure induction is performed, but the sieved coal-based precursor powder is directly carbonized.
[0099] The rest of the preparation methods and parameters were the same as those in Example 1.
[0100] Comparative Example 2
[0101] The difference between this comparative example and Example 1 is that the pressing pressure of the lignite after crushing and screening is 0.1 MPa.
[0102] The rest of the preparation methods and parameters were the same as those in Example 1.
[0103] Comparative Example 3
[0104] The difference between this comparative example and Example 1 is that no crushing and screening processes are performed.
[0105] The rest of the preparation methods and parameters were the same as those in Example 1.
[0106] The electrochemical performance test of the sodium ion battery prepared above is carried out, including:
[0107] Cyclic voltammetry: voltage range 0-2.5 V, scan rate 0.1 mV s -1 , scan 3 times.
[0108] Charge and discharge test: The voltage range is 0-2.5V, and the charge and discharge test is carried out at a current density of 20mA / g to obtain the charge and discharge specific capacity and the first efficiency.
[0109] Low temperature performance test: The test temperature is 0, -10, -20, -30, -40℃, the voltage range is 0-2.5V, and the charge and discharge test is carried out at a current density of 20mA / g.
[0110] The above test results are shown in Table 1.
[0111] Table 1 Test results
[0112]
[0113]
[0114] It can be seen from the above embodiments that the present invention provides a one-step pressure-induced coal-based dense hard carbon negative electrode material and its preparation method and a low-temperature sodium ion battery. It can be seen from the above table data that the method provided by the present invention avoids the high degree of order formed by direct carbonization of coal, but in the process of pressure induction, uses physical pressure to increase the degree of crosslinking between molecules, regulates the spatial distribution density of precursor molecules, controls the development space of carbon sheets, and adjusts the closed-pore structure of the dense hard carbon negative electrode, thereby forming a closed-pore configuration of stacked microcrystals in hard carbon and a suitable carbon layer spacing, effectively enhancing the high-capacity storage of sodium ions in coal-based dense hard carbon, showing excellent low-potential capacity and volume energy density, and meeting the current demand for sodium ion batteries in the energy storage field.
[0115] It can be seen from Examples 1 and 2 to 3 that the process method described in the present invention is not only limited to lignite as raw material, but also has excellent modification effects on other coal precursors such as anthracite and bituminous coal, that is, the general principle of the present invention is universal for different coal precursors.
[0116] It can be seen from Examples 1 and 4 to 7 that if the pressure in the pressing process is too small, the degree of induction of intermolecular cross-linking will be insufficient, while if the pressure is too large, the carbon sheet layers will lack sufficient development space, resulting in excessive ordering of the carbon structure, and the maximum capacity and initial efficiency of the sodium ion battery provided by the present invention cannot be achieved.
[0117] It can be seen from Example 1 and Examples 8 to 9 that if the pressing process is too short, the degree of cross-linking established between molecules will be too low, the induction effect will not be obvious, and the density of the coal-based hard carbon will be low, and the reversible capacity and first efficiency will be low; while excessively extending the induction time will not produce a better modification effect, but will increase the time cost.
[0118] It can be seen from Example 1 and Examples 10 to 11 that the dense coal precursor after pressure induction is carbonized at a relatively low temperature, and the precursor cannot be fully pyrolyzed, and the resulting hard carbon leads to a lower tap density and a higher degree of disorder; too high a carbonization temperature will lead to excessive development of carbon crystallites and the formation of an overly ordered structure, both of which will lead to lower first efficiency and reversible capacity.
[0119] It can be seen from Example 1 and Comparative Examples 1-2 that if pressure induction is not performed before carbonization or the applied pressure is too low, the polycyclic aromatic hydrocarbon molecules in the coal will tend to be ordered, forming over-ordered hard carbon.
[0120] It can be seen from Example 1 and Comparative Example 3 that if crushing and screening are not carried out before pressure induction, the larger coal precursor particles will not be in close contact, the degree of pressure-induced molecular cross-linking will not be obvious, and the formed coal-based hard carbon will have high order, poor density, and low capacity and initial efficiency.
[0121] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A one-step pressure-induced method for preparing a coal-based dense hard carbon negative electrode material, characterized in that: The following steps are involved: (1) crushing the deashed coal precursor and physically pressing it into a dense body; (2) carbonizing the dense body under protective gas, and then crushing and acid washing to obtain a coal-based hard carbon negative electrode material; The carbonization treatment is a one-step heat treatment, and the temperature of the one-step heat treatment is 1000-2200°C.
2. The preparation method according to claim 1, characterized in that: The deashed coal precursor comprises one or more of lignite, bituminous coal, anthracite, coal tar, petroleum tar, coal coke and petroleum coke.
3. The preparation method according to claim 1 or 2, characterized in that: The crushed particle size is ≤200 meshes.
4. The preparation method according to claim 3, characterized in that: The pressure of the physical pressing is 0.5-50 MPa, and the time of the physical pressing is 1-30 min.
5. The preparation method according to claim 1, characterized in that: The protective gas includes an inert gas or a vacuum environment.
6. The preparation method according to claim 1, 2, 4 or 5, characterized in that: The time of the one-step heat treatment is 1 to 8 hours, and the heating rate is 0.5 to 10° C. / min.
7. The coal-based dense hard carbon negative electrode material prepared by the preparation method according to any one of claims 1 to 6.
8. A low-temperature sodium ion battery, characterized in that: It is assembled from the negative electrode sheet, the counter electrode and the GF / D glass fiber separator; The negative electrode sheet is obtained by coating a mixture of the coal-based dense hard carbon negative electrode material according to claim 7, acetylene black and sodium carboxymethyl cellulose on a copper foil; the counter electrode is a sodium sheet.
Citation Information
Patent Citations
Hard carbon material, preparation method thereof, and sodium ion battery
CN112397715A
Method for preparing hard carbon negative electrode material for sodium ion battery by adopting porous material
CN114477130A
Hard carbon material with high initial coulombic efficiency for negative electrode of sodium-ion battery and preparation method of hard carbon material
CN117842966A
Coal-based hard carbon negative electrode material of sodium ion battery and preparation method of coal-based hard carbon negative electrode material
CN117894982A
Method for preparing hard carbon material by compounding coal / biomass / asphalt, hard carbon material and application
CN118419903A
Cited By
Carbon material with regulated holes as well as regulation method and application of carbon material
CN119409166A
Biomass-based hard carbon negative electrode material with high specific capacity and high magnification as well as preparation method and application of biomass-based hard carbon negative electrode material
CN120191915A
A high specific capacity, high rate biomass-based hard carbon negative electrode material and a preparation method and application thereof
CN120191915B