Vertical graphene film and preparation method thereof
The vertical structure graphene membrane is prepared by gradually widening the channels and wet spinning technology, which solves the problem of insufficient longitudinal thermal conductivity of traditional graphene membranes, achieves efficient thermal conductivity improvement, and is feasible and economical for industrial preparation. sex.
Patent Information
- Application Number
- CN202410766673.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-01
AI Technical Summary
In traditional graphene films, graphene sheets are densely stacked in the horizontal direction, resulting in insufficient longitudinal thermal conductivity, which limits its application in the field of thermal management.
Vertical structure graphene membranes are prepared using stepwise channel widening and wet spinning technology. The external shear force is used to guide graphene oxide to flip from the horizontal direction to the vertical direction. Wet spinning technology is used to achieve industrialized and continuous preparation.
It significantly improves the longitudinal thermal conductivity of the graphene film and solves the problem of low thermal conductivity of the traditional graphene film. The preparation process is easy to industrialize, the cost is low, and it has good market application prospects.
Smart Images

Figure CN118723981A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of graphene film preparation, and relates to a method for regulating the structural orientation of a graphene film, and in particular to a vertical graphene film and a preparation method thereof. Background Art
[0002] In recent years, with the rapid rise of electronic products, thin and light designs require devices to have higher heat dissipation performance. 2 The covalent bond connection allows for rapid phonon conduction, resulting in ultra-high thermal conductivity. For example, the in-plane thermal conductivity of a single-layer graphene obtained by mechanical exfoliation can reach 5300 W·m -1 ·K -1 . Graphene membranes can be easily obtained by stacking graphene layers by coating or filtering. Usually, the graphene sheets in this traditional graphene membrane are arranged in parallel along the horizontal direction of the membrane. Thanks to the rapid conduction ability of phonons in the graphene surface, this layered graphene membrane also exhibits good in-plane thermal conductivity. However, phonons are difficult to conduct in the normal direction of the graphene sheets, resulting in low thermal conductivity of traditional layered graphene membranes in the thickness direction, which greatly limits its application in the field of thermal management. In contrast, the vertically structured graphene membrane provides a smoother phonon vibration transmission channel in the thickness direction by flipping the originally horizontally arranged graphene sheets into a vertical arrangement, thereby greatly improving the longitudinal thermal conductivity of the graphene membrane. For example, in patent CN 113697800 A "Directedly arranged graphene thermally conductive foam, graphene thermally conductive film, preparation method thereof and electronic product", a directedly arranged graphene thermally conductive foam is obtained by using a grid array of a specific structure to groove-shape graphene oxide, and combining freeze-drying. The graphene thermally conductive material not only has a high in-plane thermal conductivity, but also has a high longitudinal thermal conductivity. However, the method not only has a complicated preparation process, but also has difficulty in large-scale continuous preparation of graphene membranes. In view of this, the present invention proposes a method for preparing a vertical graphene membrane based on step-by-step channel widening, including the design and preparation of step-by-step channel amplification and the preparation of a vertical structured graphene membrane using wet spinning technology. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a vertically structured graphene film and a preparation method thereof in view of the problem that the graphene sheets in the graphene film material in the prior art are densely stacked in the horizontal direction, resulting in insufficient longitudinal thermal conductivity.
[0004] Invention idea: The preparation mechanism of the present invention is based on the liquid crystal phenomenon of graphene oxide. The behavior of graphene oxide liquid crystals that spontaneously orient along the direction of the force when subjected to external shear force is utilized to research and develop a step-by-step widening channel as a membrane spinning nozzle. When the fluid flows through the step-by-step widening channel, it will present an inverted flow, thereby guiding the graphene oxide in the flow field to flip from the horizontal direction to the vertical direction. Not only that, the step-by-step widening channel can cause the vertical graphene oxide to gradually increase in width, and finally form a vertical graphene film through steps such as drying and reduction.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0006] The present invention discloses a method for preparing a vertical graphene film, comprising the following steps:
[0007] (1) preparing a graphene oxide solution;
[0008] (2) mixing a metal salt with a first solvent to obtain a mixed metal salt solution; adding the mixed metal salt solution to the graphene oxide solution prepared in step (1), mixing, and centrifuging to obtain a graphene oxide spinning solution;
[0009] (3) pumping the graphene oxide spinning solution obtained in step (2) into a stepwise widening channel in a coagulation bath, and standing and coagulating in the coagulation bath after wet spinning to obtain a gel vertical graphene oxide membrane;
[0010] (4) taking the gel vertical graphene oxide film obtained in step (3) out of the coagulation bath, performing a first washing, and obtaining a vertical graphene oxide film after freeze-drying; reducing the vertical graphene oxide film, performing a second washing after the reduction is completed, and obtaining a vertical graphene film after freeze-drying;
[0011] The step-by-step widening channel is a coaxial step-by-step widening channel or a plurality of coaxial step-by-step widening channels arranged in parallel.
[0012] In some embodiments, in step (1), in the graphene oxide solution, the solute is graphene oxide, the concentration of graphene oxide is 5.0 to 15.0 mg / mL, and the solvent in the solution is preferably water.
[0013] In some embodiments, preferably, in step (1), in the graphene oxide solution, the solute is graphene oxide, the concentration of graphene oxide is 7.5-15.0 mg / mL, and the solvent in the solution is preferably water.
[0014] Wherein, in step (1), the graphene oxide can be purchased commercially or prepared according to the prior art; the prior art is preferably prepared by the Hummers method.
[0015] In some embodiments, in step (2), the metal salt is a combination of any two of ferric nitrate, nickel nitrate, ferric chloride, sodium chloride and calcium chloride; the first solvent is preferably water; and the mass concentration of the metal salt in the mixed metal salt solution is 0.1% to 1.0%.
[0016] In some embodiments, in step (2), preferably, the metal salt is a mixture of ferric nitrate and nickel nitrate in any mass ratio, and further preferably, the metal salt is a mixture of ferric nitrate and nickel nitrate in a mass ratio of 3:2; in the mixed metal salt solution, the mass concentration of the metal salt is 0.1% to 0.5%, and further preferably is 0.2%.
[0017] Among them, in step (2), the metal salt can increase the concentration and viscosity of the graphene oxide spinning solution, which is beneficial to the flipping orientation of the graphene oxide sheet during the spinning process.
[0018] In some embodiments, in step (2), the mass ratio of graphene oxide in the graphene oxide solution to the metal salt in the mixed metal salt solution is 10:1-6; the centrifugation speed is 5000-20000 rpm, and the centrifugation time is 0.5-4h.
[0019] In some embodiments, in step (2), preferably, the mass ratio of graphene oxide in the graphene oxide solution to the metal salt in the mixed metal salt solution is 10:3-6, and more preferably 10:5; the centrifugal speed is 8000-15000 rpm, and the centrifugal time is 0.5-2 h, and more preferably, the centrifugal speed is 10000 rpm, and the centrifugal time is 1 h.
[0020] In some embodiments, in step (3), the graphene oxide membrane spinning stock solution is pumped into the stepwise widening channel at a flow rate of 0.1 to 1.0 mL / min; the wet spinning is carried out at room temperature; and the standing time is 2 h to 24 h.
[0021] In some embodiments, in step (3), preferably, the flow rate of the graphene oxide membrane stock solution pumped into the step-by-step widening channel is 0.2-0.6 mL / min, and more preferably 0.4 mL / min; the standing time is 8 h to 16 h, and more preferably 12 h.
[0022] In some embodiments, in step (3), the coagulation bath contains a solute and a solvent; the solute is any one or a combination of cetyltrimethylammonium bromide, sodium chloride and calcium chloride; the solvent is a combination of water and other substances, or anhydrous ethanol; the other substance is ethanol or glycerol; the volume concentration of other substances in the solvent is 30% to 50%; the concentration of the solute in the coagulation bath is 0.1 to 10 g / L.
[0023] In some embodiments, in step (3), preferably, the coagulation bath contains a solute and a solvent; the solute is hexadecyltrimethylammonium bromide; the solvent is a composition of water and other substances; the other substance is propylene glycol; the volume concentration of the other substance in the solvent is 30% to 40%, more preferably 30%; the concentration of the solute in the coagulation bath is 0.2 to 4 g / L, more preferably 2 g / L.
[0024] In some embodiments, the coaxial step-by-step widening channel has n levels; the coaxial step-by-step widening channel includes an entrance channel, a first-level widening rectangular channel, a second-level widening rectangular channel, ... an n-1th-level widening rectangular channel and an nth-level widening rectangular channel; the corresponding side lengths of the cross sections of the rectangular channels of different levels are parallel to each other, and n is greater than or equal to 2;
[0025] The coaxial step-by-step widening channel, from the first-step widening rectangular channel to the n-step widening rectangular channel, has corresponding lengths of rectangular cross sections that increase step by step, and corresponding widths of rectangular cross sections that are all equal;
[0026] The cross section of the inlet channel is circular or rectangular; when the cross section of the inlet channel is circular, the diameter of the cross section of the inlet channel is smaller than the length of the cross section of the first-stage widened rectangular channel; when the cross section of the inlet channel is rectangular, the length of the cross section of the inlet channel is smaller than the length of the cross section of the first-stage widened rectangular channel;
[0027] The graphene oxide spinning stock solution flows in from the inlet channel, flows through the first-stage widened rectangular channel, the second-stage widened rectangular channel, ... the n-1-stage widened rectangular channel in sequence, and flows out from the n-stage widened rectangular channel.
[0028] The material of the coaxial step-by-step widening channel is not limited, as long as the material does not react with the graphene oxide membrane spinning stock solution.
[0029] The coaxial step-by-step widening channel has n stages, where n is greater than or equal to 2, preferably 2≤n≤10, further preferably 2≤n≤6, further preferably 3≤n≤6, and most preferably n=4.
[0030] Wherein, the coaxial step-by-step widening channel is engraved by a micro-mechanical engraving machine.
[0031] Among them, the entrance channel, the first-level widened rectangular channel, the second-level widened rectangular channel...the n-1-level widened rectangular channel and the n-level widened rectangular channel are connected through; the entrance channel, the first-level widened rectangular channel, the second-level widened rectangular channel...the n-1-level widened rectangular channel and the n-level widened rectangular channel are all straight pipe channels; the cross section of the entrance channel is parallel to the cross section of the first-level widened rectangular channel.
[0032] Among them, the pipe lengths of the entrance channel, the first-level widened rectangular channel, the second-level widened rectangular channel, ... the n-1-level widened rectangular channel and the n-level widened rectangular channel are the same or different.
[0033] Among them, from the first-level widened rectangular channel to the n-level widened rectangular channel, the corresponding lengths of the rectangular cross-sections thereof increase step by step. The ratio between the corresponding lengths of the rectangular cross-sections of the first-level widened rectangular channel, the second-level widened rectangular channel...the n-1-level widened rectangular channel and the n-level widened rectangular channel is preferably 1~2:2~3:3~4:...:n~(n+1).
[0034] The coaxial step-wise widening channel is horizontally immersed in a coagulation bath to ensure that the graphene oxide membrane spinning stock solution fills the entire coaxial step-wise widening channel, and then flows out from the outlet of the coaxial step-wise widening channel to contact the coagulation bath and solidify into a gel vertical graphene oxide membrane.
[0035] Among them, it is further preferred that the coaxial step-by-step widening channel has four stages, and the coaxial step-by-step widening channel includes an entrance channel, a first-stage widened rectangular channel, a second-stage widened rectangular channel, a third-stage widened rectangular channel and a fourth-stage widened rectangular channel; from the first-stage widened rectangular channel to the fourth-stage widened rectangular channel, the corresponding lengths of their rectangular cross-sections increase step by step, and the corresponding widths of their rectangular cross-sections are all equal; the cross-section of the entrance channel is rectangular, and the length of the cross-section of the entrance channel is smaller than the length of the cross-section of the first-stage widened rectangular channel; the graphene oxide spinning stock solution flows into the entrance channel, flows through the first-stage widened rectangular channel, the second-stage widened rectangular channel, the third-stage widened rectangular channel in sequence, and flows out of the fourth-stage widened rectangular channel; the entrance channel, the first-stage widened rectangular channel The widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel and the fourth-level widened rectangular channel are interconnected; the entrance channel, the first-level widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel and the fourth-level widened rectangular channel are all straight pipe channels; the cross section of the entrance channel is parallel to the cross section of the first-level widened rectangular channel; the entrance channel, the first-level widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel and the fourth-level widened rectangular channel have the same pipe length; the ratio between the corresponding lengths of the rectangular cross sections of the first-level widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel and the fourth-level widened rectangular channel is preferably 1-2:2-3:3-4:4-5, preferably 2:3:4:5. Among them, the pipe length of the entrance channel is preferably 5-20 mm, and further preferably 10 mm. The length and width of the rectangular cross-section of the entrance channel are both 2.5-3 mm, and preferably 2.8 mm; the length of the rectangular cross-section of the first-level widened rectangular channel is 4-6 mm, and preferably 6 mm; the corresponding widths of the rectangular cross-sections of the first-level widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel and the fourth-level widened rectangular channel are all equal, and are preferably 0.3-1.2 mm, and further preferably 1 mm; the pipe lengths of the first-level widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel and the fourth-level widened rectangular channel are all the same, and are preferably 5-20 mm, and further preferably 10 mm.
[0036] Among them, the design of coaxially widening the channel step by step and expanding the capacity section by section has the characteristics of stable molding and uniform force on the edge of the graphene membrane, ensuring that the spun vertical structure graphene membrane has a good vertical structure.
[0037] In some embodiments, the plurality of parallel arranged coaxial progressively widening channels are composed of m parallel arranged coaxial progressively widening channels; m is greater than or equal to 2;
[0038] The directions of the m parallel arranged coaxial progressively widening channels from the entrance channel to the nth widening rectangular channel are the same;
[0039] The n-number of coaxial progressively widening channels arranged in parallel may be different or the same, the cross-sectional areas of the corresponding progressively widened rectangular channels may be the same or different, the length of the rectangular cross-section of the last-level widened rectangular channel may be on the same vertical plane and the width may be the same; the last-level widened rectangular channels of multiple coaxial progressively widened channels arranged in parallel may be interconnected.
[0040] Therein, the material of the m parallel arranged coaxial step-by-step widening channels is not limited, as long as the material does not react with the graphene oxide membrane spinning stock solution.
[0041] Herein, m is greater than or equal to 2, preferably 2≤m≤100, more preferably 2≤m≤50, further preferably 2≤m≤10, and most preferably m=2.
[0042] Among them, multiple parallel arranged coaxial step-by-step widening channels are engraved by a micro-mechanical engraving machine.
[0043] Among them, between the parallel arranged coaxial step-by-step widening channels, the rectangular cross-sections of the outlets of the last step widening rectangular channels are on the same horizontal plane, ensuring that the parallel arranged coaxial step-by-step widening channels simultaneously discharge the graphene oxide spinning stock solution, thereby successfully preparing a wider gel vertical graphene oxide membrane.
[0044] Among them, the last-level widening rectangular channels of the multiple parallel-arranged coaxial step-by-step widening channels are interconnected, and between adjacent parallel-arranged coaxial step-by-step widening channels, the parts near the outlet ends are interconnected, while the parts near the inlet ends are not connected and have gaps; or, between adjacent parallel-arranged coaxial step-by-step widening channels, the last-level widening rectangular channels are all connected.
[0045] Among them, the multiple parallel arranged coaxial step-by-step widening channels are horizontally immersed in the coagulation bath to ensure that the graphene oxide membrane spinning stock solution fills the entire widened channel, and then flows out from the outlet of the last step widening rectangular channel of the parallel arranged coaxial step-by-step widening channels to contact the coagulation bath and solidify into a gel vertical graphene oxide film.
[0046] In some embodiments, preferably, the n-number of coaxial progressively widened channels arranged in parallel are the same, the cross-sectional areas of the corresponding widened rectangular channels are the same, and the length of the rectangular cross-section of the last widened rectangular channel is on the same vertical plane and has the same width.
[0047] Among them, it is further preferred that the coaxial step-by-step widening channel has four stages, and the coaxial step-by-step widening channel includes an entrance channel, a first-stage widened rectangular channel, a second-stage widened rectangular channel, a third-stage widened rectangular channel and a fourth-stage widened rectangular channel; from the first-stage widened rectangular channel to the fourth-stage widened rectangular channel, the corresponding lengths of their rectangular cross-sections increase step by step, and the corresponding widths of their rectangular cross-sections are all equal; the cross-section of the entrance channel is rectangular, and the length of the cross-section of the entrance channel is smaller than the length of the cross-section of the first-stage widened rectangular channel; the graphene oxide spinning stock solution flows into the entrance channel, flows through the first-stage widened rectangular channel, the second-stage widened rectangular channel, the third-stage widened rectangular channel in sequence, and flows out of the fourth-stage widened rectangular channel; the entrance channel, the first-stage widened rectangular channel The widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel and the fourth-level widened rectangular channel are interconnected; the entrance channel, the first-level widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel and the fourth-level widened rectangular channel are all straight pipe channels; the cross section of the entrance channel is parallel to the cross section of the first-level widened rectangular channel; the entrance channel, the first-level widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel and the fourth-level widened rectangular channel have the same pipe length; the ratio between the corresponding lengths of the rectangular cross sections of the first-level widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel and the fourth-level widened rectangular channel is preferably 1-2:2-3:3-4:4-5, preferably 2:3:4:5. Among them, the pipe length of the entrance channel is preferably 5-20mm, and further preferably 10mm. The length and width of the rectangular cross-section of the entrance channel are both 2.5-3mm, and preferably 2.8mm; the length of the rectangular cross-section of the first-level widened rectangular channel is 4-6mm, and preferably 6mm; the corresponding widths of the rectangular cross-sections of the first-level widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel and the fourth-level widened rectangular channel are all equal, and are preferably 0.3-1.2mm, and further preferably 1mm; the pipe lengths of the first-level widened rectangular channel, the second-level widened rectangular channel and the third-level widened rectangular channel are all the same, and are preferably 5-20mm, and further preferably 10mm; the pipe length of the fourth-level widened rectangular channel is preferably 5-20mm, and further preferably 13mm.A plurality of parallel coaxial step-by-step widening channels are composed of two of the above coaxial step-by-step widening channels arranged in parallel, and the directions of the two parallel coaxial step-by-step widening channels from the entrance channel to the fourth-stage widening rectangular channel are the same; the n-levels of the parallel coaxial step-by-step widening channels are the same, both being 4, and the cross-sectional areas of the corresponding stage widening rectangular channels are the same, the lengths of the rectangular cross-sections of the last-stage widening rectangular channels are on the same vertical plane and the widths are the same, and the rectangular cross-sections of the outlets of the last-stage widening rectangular channels are on the same horizontal plane, ensuring that the parallel coaxial step-by-step widening channels simultaneously discharge graphene oxide spinning stock solution, and successfully preparing a wider gel vertical graphene oxide membrane; the last-stage widening rectangular channels of the two parallel coaxial step-by-step widening channels are interconnected, and the 10mm pipe lengths near the outlet end are interconnected, and the 3mm pipe lengths near the inlet end are not connected and are spaced 1mm apart.
[0048] Among them, the design of coaxially widening the channel step by step and expanding the capacity section by section has the characteristics of stable molding and uniform force on the edge of the graphene membrane, ensuring that the spun vertical structure graphene membrane has a good vertical structure.
[0049] In some embodiments, in step (4), the first washing, the detergent used is any one or a combination of hydrochloric acid aqueous solution, ether, ethyl acetate and water; the reduction method is high temperature reduction, hydroiodic acid reduction or hydrazine hydrate reduction; the hydroiodic acid reduction, the reduction temperature is 60-80°C, and the reduction time is 6-8h; the second washing, the detergent used is any one or a combination of ethanol and water.
[0050] In some embodiments, in step (4), preferably, in the first washing, the detergents used are aqueous hydrochloric acid solution and water; the reduction method is hydroiodic acid reduction; the hydroiodic acid reduction has a reduction temperature of 60°C and a reduction time of 8 hours; and the second washing has anhydrous ethanol and water.
[0051] Wherein, the concentration of the hydrochloric acid aqueous solution is preferably 1M.
[0052] In the process of the hydroiodic acid reduction, a hydroiodic acid aqueous solution is used as a reducing agent, and the amount of the hydroiodic acid aqueous solution used is excessive; the concentration of the hydroiodic acid aqueous solution is preferably 40 to 65 wt%, and more preferably 47 wt%.
[0053] The vertical graphene film prepared by the above preparation method is also within the protection scope of the present invention.
[0054] The application of the vertical graphene film in the preparation of thermal conductive materials is also within the protection scope of the present invention.
[0055] Beneficial effects:
[0056] (1) The graphene film with a vertical structure prepared by the present invention can be used in the field of thermal management. Compared with traditional layered graphene, the vertically arranged graphene is conducive to the rapid transmission of phonons in the longitudinal direction, thereby improving its longitudinal thermal conductivity.
[0057] (2) In order to precisely control the orientation of graphene sheets, the present invention proposes to use a step-by-step widening channel as a spinning nozzle. In the widened portion of the pipeline, the fluid boundary layer separates, and the flow field flips from being parallel to the central axis of the pipeline to being perpendicular to the central axis of the pipeline. This flow field flipping causes the graphene oxide therein to deflect, so that the graphene sheets are oriented vertically along the fiber axis. More importantly, the use of a step-by-step widening structure avoids the situation where the orientation of the graphene sheets changes during the spinning process of the wide film. In addition, by connecting multiple step-by-step widening channels in parallel, the width of the graphene film can be effectively increased.
[0058] (3) The present invention utilizes a step-by-step channel widening method to prepare a wide-basin expansion flow, causing the graphene sheets in the membrane spinning solution to flip from a horizontal direction to a vertical direction, thereby preparing a vertically structured graphene membrane.
[0059] (4) The present invention is based on wet spinning technology, and forms wet spinning membrane technology by adjusting the viscosity of the spinning solution, selecting a suitable coagulation bath, adding additives and other technical improvements. This technology has the advantages of wet spinning being easy to scale up industrially, easy to prepare continuously, high reliability and low cost, and has good market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.
[0061] Figure 1 Flow chart of the preparation of a vertically structured graphene film in an embodiment of the present invention.
[0062] Figure 2 The structure diagram and structure cross-section diagram of the 4-stage coaxial step-by-step widening channel used in the embodiment of the present invention; wherein, Figure 2 A is the structural cross-section of the coaxial step-by-step widening channel. Figure 2 B is the structural diagram of the coaxial step-by-step channel widening.
[0063] Figure 3 It is a top-view dimension diagram, a top-view schematic diagram and a perspective diagram of a 4-stage coaxial step-by-step widening channel used in an embodiment of the present invention; wherein, Figure 3 A is the top view of the coaxial step-by-step widening channel. Figure 3 B is a top view of the actual object of the coaxial step-by-step widening channel. Figure 3 C is a perspective view of the coaxial step-by-step widening channel.
[0064] Figure 4 This is a scanning electron microscope (SEM) image of the vertical structure graphene film of the product of Example 1.
[0065] Figure 5 This is a scanning electron microscope (SEM) image of the graphene film prepared in Example 2.
[0066] Figure 6 This is a schematic diagram of the top-down dimensions of the structure of two parallel-arranged four-stage coaxial progressively widened channels used in an embodiment of the present invention.
[0067] Figure 7 The figure is a top view and a perspective view of two parallel arranged four-stage coaxial progressively widened channels used in the embodiment of the present invention; wherein: Figure 7 A is a top view of the object. Figure 7 B is a perspective view of two parallel arranged four-stage coaxial progressively widening channels.
[0068] Figure 8 This is a scanning electron microscope (SEM) image of the vertical structure graphene film of the product of Example 3.
[0069] Fig. 9 This is a scanning electron microscope (SEM) image of the ordinary graphene film product of Comparative Example 1. DETAILED DESCRIPTION
[0070] The present invention can be better understood with reference to the following examples.
[0071] The preparation flow chart of the vertically structured graphene film of the present invention is as follows: Figure 1 As shown, a graphene oxide membrane spinning stock solution is loaded into a syringe, and bubbles in the syringe are removed. After a silicone hose is put on the injection head of the syringe, the other end of the silicone hose is connected and assembled with the inlet end of the coaxial step-by-step widening channel, and the graphene oxide membrane spinning stock solution is pumped into the coaxial step-by-step widening channel located in a coagulation bath (the coaxial step-by-step widening channel is horizontally immersed in the coagulation bath) by a syringe pump, and a vertical graphene oxide membrane is prepared by wet spinning, and then the vertical graphene oxide membrane is reduced by hydroiodic acid to obtain a graphene membrane, and then freeze-dried to obtain a vertical graphene membrane.
[0072] The graphene oxide used in the embodiments of the present invention can be purchased commercially or prepared by the Hummers method. The specific preparation method can refer to the prior art Chemical Engineering Science 176 (2018) 319-328.
[0073] Example 1: Wet spinning membrane using a single coaxial step-by-step channel widening
[0074] Micro-mechanical engraving machine engraves 4 levels of coaxial and gradually widens the channel:
[0075] The structure diagram of the coaxial step-by-step widening channel used in the embodiment of the present invention is as follows Figure 2 As shown, it is engraved by a micromechanical engraving machine, and the coaxial step-by-step widening channel has 4 levels. The coaxial step-by-step widening channel includes an entrance channel a, a first-level widening rectangular channel b, a second-level widening rectangular channel c, a third-level widening rectangular channel d and a fourth-level widening rectangular channel e; from the first-level widening rectangular channel to the fourth-level widening rectangular channel, the corresponding lengths of the rectangular cross-sections thereof increase step by step, and the corresponding widths of the rectangular cross-sections thereof are all equal; wherein, see Figure 2 B or Figure 3 The rectangular cross-section channel opening of the fourth-level widened rectangular channel of the coaxial step-by-step widening channel in C, L is the length of the rectangular cross-section, W is the width of the rectangular cross-section, and the corresponding long side of the rectangular cross-section of the other levels of widened rectangular channels is the length, and the corresponding short side of the rectangular cross-section is the width; the cross-section of the inlet channel is a square, and the length of the cross-section of the inlet channel is less than the length of the cross-section of the first-level widened rectangular channel. The graphene oxide spinning stock solution flows in from the inlet channel a, flows through the first-level widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel in sequence, and flows out from the fourth-level widened rectangular channel; the inlet channel, the first-level widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel and the fourth-level widened rectangular channel are connected through; the inlet channel, the first-level widened rectangular channel, the second-level widened rectangular channel, the third-level widened rectangular channel and the fourth-level widened rectangular channel are all straight tube channels; the cross-section of the inlet channel is parallel to the cross-section of the first-level widened rectangular channel. The top view dimension diagram, the top view schematic diagram and the perspective view of the 4-stage coaxial step-by-step widening channel used in this embodiment are shown in Figure 3, where the length of the pipes of the entrance channel, the first-level widening rectangular channel, the second-level widening rectangular channel, the third-level widening rectangular channel and the fourth-level widening rectangular channel are the same, all 10mm; the corresponding length ratios of the rectangular cross sections of the first-level widening rectangular channel, the second-level widening rectangular channel, the third-level widening rectangular channel and the fourth-level widening rectangular channel are 2:3:4:5. Wherein, the pipe length of the entrance channel is 10mm, and the length and width of the rectangular cross section are both 2.8mm; the pipe length of the first-level widening rectangular channel is 10mm, and the length and width of the rectangular cross section are 6mm and 1mm; the pipe length of the second-level widening rectangular channel is 10mm, and the length and width of the rectangular cross section are 9mm and 1mm; the pipe length of the third-level widening rectangular channel is 10mm, and the length and width of the rectangular cross section are 12mm and 1mm; the pipe length of the fourth-level widening rectangular channel is 10mm, and the length and width of the rectangular cross section are 15mm and 1mm. The inlet channel of the 4-stage coaxial step-by-step widening channel is connected to the syringe using a silicone tube with an inner diameter of 2 mm and an outer diameter of 3 mm. The injection head of the syringe is inserted into one end, and the inlet end of the inlet channel a is inserted into the other end. The wall thickness of the 4-stage coaxial step-by-step widening channel is not 0, and there is no special limitation, as long as the inlet channel a can be adaptively connected to the silicone tube.
[0076] Preparation of vertical graphene membrane:
[0077] (1) A 10 mg / mL graphene oxide aqueous solution was prepared by the Hummers method, and the graphene oxide aqueous solution was further centrifuged and concentrated to obtain a graphene oxide aqueous solution with a concentration of about 15 mg / mL.
[0078] (2) Take 10 mL of graphene oxide aqueous solution (concentration of about 15 mg / mL, prepared in step (1), a total of 150 mg of graphene oxide), add deionized water to dilute to 20 mL, and stir evenly. At the same time, weigh 45 mg of ferric nitrate and 30 mg of nickel nitrate in a mass ratio of 10:3:2 for graphene oxide, ferric nitrate, and nickel nitrate to prepare a mixed metal salt solution, mix the ferric nitrate and nickel nitrate, add deionized water to prepare 40 mL of a mixed metal salt solution, stir evenly, use a burette to drop into the diluted 20 mL of graphene oxide solution at a rate of one drop per 7 seconds, and stir continuously to prevent local agglomeration of graphene oxide. After mixing evenly, continue to stir at high speed for 30 minutes until completely mixed, and then centrifuge at 10000 r / min for 1 hour to obtain a graphene oxide spinning solution.
[0079] (3) At room temperature, a syringe is used to absorb the graphene oxide spinning stock solution prepared in step (2), and bubbles in the syringe are removed. After the injection head of the syringe is covered with a silicone hose, the other end of the silicone hose is connected and assembled with the inlet channel of the coaxial step-by-step widening channel (the inlet channel is inserted into the other end of the silicone hose), and the coaxial step-by-step widening channel is horizontally placed in a coagulation bath, and its outlet is located in a mixed coagulation bath consisting of glycerol and water containing hexadecyltrimethylammonium bromide (CTAB) (the volume concentration of glycerol in the mixed coagulation bath is 30%, and the concentration of hexadecyltrimethylammonium bromide in the coagulation bath is 2 g / L). During wet spinning, the injection rate of the syringe is 0.4 mL / min. After the spinning is completed, the gel obtained continues to stand in a glycerol coagulation bath containing CTAB for 12 hours to obtain a gel vertical graphene oxide membrane.
[0080] (4) The gel vertical graphene oxide film obtained in step (3) is washed three times with a 1M hydrochloric acid aqueous solution, each time for 30 minutes, and then washed three times with deionized water, each time for 30 minutes, and then the washed gel vertical graphene oxide film is freeze-dried for 24 hours to obtain a vertical graphene oxide film. The vertical graphene oxide film and hydroiodic acid aqueous solution (the concentration of hydroiodic acid is 47wt%) are further added to a sealed container, heated to 60°C and kept warm for 8 hours to fully reduce, and then washed with anhydrous ethanol for 3 times after the reduction is completed, each time for 30 minutes, and then washed with deionized water until the solution is colorless and odorless, and freeze-dried for 24 hours to obtain a vertical reduced graphene oxide film, i.e., a vertical graphene film.
[0081] Figure 4 For the vertical graphene film prepared in this embodiment, it can be seen that the graphene sheets are arranged vertically along the horizontal direction of the graphene film, thereby constructing a good heat conduction channel.
[0082] Example 2: No metal salt added
[0083] The number and size of the coaxial step-by-step widening channels used in this embodiment are the same as those of the coaxial step-by-step widening channels used in Example 1.
[0084] (1) A 10 mg / mL graphene oxide aqueous solution was prepared by the Hummers method. The graphene oxide aqueous solution was further centrifuged and concentrated to obtain a graphene oxide aqueous solution with a concentration of about 15 mg / mL. The solution was then centrifuged at 10,000 r / min for 1 h to obtain a graphene oxide membrane spinning stock solution.
[0085] (2) At room temperature, a syringe is used to absorb the graphene oxide spinning stock solution prepared in step (1), and bubbles in the syringe are removed. After the injection head of the syringe is covered with a silicone hose, the other end of the silicone hose is connected and assembled with the inlet channel of the coaxial step-by-step widening channel (the inlet channel is inserted into the other end of the silicone hose), and the coaxial step-by-step widening channel is horizontally placed in a coagulation bath, and its outlet is located in a mixed coagulation bath consisting of glycerol and water containing hexadecyltrimethylammonium bromide (CTAB) (the volume concentration of glycerol in the mixed coagulation bath is 30%, and the concentration of hexadecyltrimethylammonium bromide in the coagulation bath is 2 g / L). During wet spinning, the injection rate of the syringe is 0.4 mL / min. After the spinning is completed, the gel obtained continues to stand in a glycerol coagulation bath containing CTAB for 12 hours to obtain a gel graphene oxide membrane.
[0086] (3) The gel graphene oxide film obtained in step (2) is washed three times with a 1M hydrochloric acid aqueous solution, each time for 30 minutes, and then washed three times with deionized water, each time for 30 minutes, and then the washed gel graphene oxide film is freeze-dried for 24 hours to obtain a graphene oxide film. The graphene oxide film and a hydroiodic acid aqueous solution (the concentration of hydroiodic acid is 47wt%) are further added to a sealed container, heated to 60°C and kept warm for 8 hours to fully reduce, and after the reduction is completed, it is washed three times with anhydrous ethanol, each time for 30 minutes, and then washed with deionized water until the solution is colorless and odorless, and freeze-dried for 24 hours to obtain a reduced graphene oxide film, i.e., a graphene film.
[0087] Figure 5 From the graphene film prepared in this embodiment, it can be seen that the graphene sheets are arranged in a disordered manner and no good heat conduction channel is formed.
[0088] Example 3: Wet spinning membrane using two parallel coaxial progressively widened channels
[0089] The micro-mechanical engraving machine engraves two parallel arranged 4-level coaxial and step-by-step widening channels:
[0090] The top view of the structure of the four-stage coaxial progressively widened channel arranged in parallel in the embodiment of the present invention is as follows: Figure 6 As shown, the actual top view and perspective view of two parallel arranged four-stage coaxial step-by-step widening channels are as follows Figure 7As shown. Among them, the number and size of a single coaxial step-by-step widening channel are the same as the number and size of a single 4-stage coaxial step-by-step widening channel used in Example 1, except that the pipe length of the 4th stage widening rectangular channel is 13 mm. In this embodiment, the above two identical 4-stage coaxial step-by-step widening channels are arranged in parallel, and the directions from the entrance channel to the 4th stage widening rectangular channel between the two parallel arranged 4-stage coaxial step-by-step widening channels are the same, and the cross-sectional areas of the corresponding stages of widened rectangular channels between the parallel arranged coaxial step-by-step widening channels are the same, the length of the rectangular cross section of the last stage widening rectangular channel is on the same vertical plane and the same width, and the rectangular cross section of the outlet of the last stage widening rectangular channel is on the same horizontal plane, ensuring that the parallel arranged coaxial step-by-step widening channels can simultaneously discharge oxide. The graphene spinning stock solution was used to successfully prepare a wider gel vertical graphene oxide membrane; the last-stage widening rectangular channels of the 2 parallel coaxial step-by-step widening channels were interconnected, and the 10mm pipe length near the outlet was interconnected, and the 3mm pipe length near the inlet was not connected. The partition at the merged part was 3mm long and 0.1mm wide, that is, the unconnected part was separated by 0.1mm, and the length of the rectangular cross-section of the last stage channel of the 2 parallel 4-stage coaxial step-by-step widening channels was L (L was 30.1mm), and the width of the rectangular cross-section was W (W was 1mm).
[0091] Use two silicone tubes to connect the two inlet channels of the two parallel arranged four-stage coaxial progressively widening channels to two syringes respectively. The silicone tubes used have an inner diameter of 2 mm and an outer diameter of 3 mm. One end is inserted into the injection head of the syringe, and the other end is inserted into the inlet end of the inlet channel a. Among them, the tube wall thickness of the coaxial progressively widening channel is not 0, and there is no special limitation, as long as the inlet channel a can be adaptively connected to the silicone tube.
[0092] Preparation of vertical graphene membrane:
[0093] (1) A 10 mg / mL graphene oxide aqueous solution was prepared by the Hummers method, and the graphene oxide aqueous solution was further centrifuged and concentrated to obtain a graphene oxide aqueous solution with a concentration of about 15 mg / mL.
[0094] (2) Take 10 mL of graphene oxide aqueous solution (concentration of about 15 mg / mL, prepared in step (1), a total of 150 mg of graphene oxide), add deionized water to dilute to 20 mL, and stir evenly. At the same time, weigh 45 mg of ferric nitrate and 30 mg of nickel nitrate in a mass ratio of 10:3:2 for graphene oxide, ferric nitrate, and nickel nitrate to prepare a mixed metal salt solution, mix the ferric nitrate and nickel nitrate, add deionized water to prepare 40 mL of a mixed metal salt solution, stir evenly, use a burette to drop into the diluted 20 mL of graphene oxide solution at a rate of one drop per 7 seconds, and stir continuously to prevent local agglomeration of graphene oxide. After mixing evenly, continue to stir at high speed for 30 minutes until completely mixed, and then centrifuge at 10000 r / min for 1 hour to obtain a graphene oxide spinning solution.
[0095] (3) At room temperature, two syringes are used to draw an equal amount of the graphene oxide spinning solution prepared in step (2), and bubbles in the syringes are removed. The injection ports of the two syringes are respectively covered with silicone hoses and then respectively connected to the inlet channels a of two parallel coaxial step-by-step widening channels (the two inlet channels are respectively covered with the other ends of the two silicone hoses). The two syringes simultaneously pump the graphene oxide spinning solution into the coaxial step-by-step widening channels. The two parallel coaxial step-by-step widening channels are horizontally placed in a coagulation bath. The outlet is located in a mixed coagulation bath consisting of glycerol and water containing cetyltrimethylammonium bromide (CTAB) (the volume concentration of glycerol in the mixed coagulation bath is 30%, and the concentration of cetyltrimethylammonium bromide in the coagulation bath is 2 g / L). The injection rate of the syringe during wet spinning is 0.4 mL / min, and finally the membrane width is 30.1 mm after the parallel arrangement of channels. After the spinning is completed, the gel obtained continues to stand in a glycerol coagulation bath containing CTAB for 12 hours to obtain a gel vertical structure graphene oxide membrane.
[0096] (4) The gel vertical structure graphene oxide film obtained in step (3) is washed three times with a 1M hydrochloric acid aqueous solution, each time for 30 minutes, and then washed three times with deionized water, each time for 30 minutes, and then the washed gel vertical graphene oxide film is freeze-dried for 24 hours to obtain a vertical graphene oxide film. The vertical graphene oxide film and hydroiodic acid aqueous solution (the concentration of hydroiodic acid is 47wt%) are further added to a sealed container, heated to 60°C and kept warm for 8 hours to fully reduce, and then washed with anhydrous ethanol for 3 times after the reduction is completed, each time for 30 minutes, and then washed with deionized water until the solution is colorless and odorless, and freeze-dried for 24 hours to obtain a vertical reduced graphene oxide film, i.e., a vertical graphene film.
[0097] Figure 8For the vertical graphene film prepared in this embodiment, it can be seen that the graphene sheets are arranged vertically along the horizontal direction of the graphene film, thereby constructing a good heat conduction channel.
[0098] Comparative Example 1: Wet Spinning Membrane Using Flat Rectangular Channels
[0099] The flat channel used in this embodiment is a straight rectangular channel with a length of 15 mm and a rectangular cross section with a length of 10 mm and a width of 1 mm. The flat channel is placed horizontally in the coagulation bath.
[0100] (1) A 10 mg / mL graphene oxide aqueous solution was prepared by the Hummers method. The graphene oxide aqueous solution was further centrifuged and concentrated to obtain a graphene oxide aqueous solution with a concentration of about 15 mg / mL. The solution was then centrifuged at 10,000 r / min for 1 h to obtain a graphene oxide membrane spinning stock solution.
[0101] (2) At room temperature, use a syringe to absorb the graphene oxide spinning solution prepared in step (1), remove bubbles in the syringe, connect the injection head of the syringe to the inlet of the Luer connector, connect the outlet of the Luer connector to the flat channel interface, place the flat channel horizontally in a coagulation bath, and its outlet is located in an anhydrous ethanol coagulation bath. During wet spinning, the injection rate of the syringe is 0.4 mL / min. After the spinning is completed, stand in an anhydrous ethanol coagulation bath for 12 hours to fix the shape, and then wash with deionized water for multiple times, each washing time lasting 30 minutes, until the solution is colorless and odorless. Then freeze-dry the washed membrane for 24 hours to obtain a graphene oxide membrane. Further, graphene oxide film and hydroiodic acid aqueous solution (the concentration of hydroiodic acid is 47wt%) are added to a sealed container, heated to 60°C and kept warm for 8h for sufficient reduction. After the reduction is completed, it is washed with anhydrous ethanol for 3 times, each washing time lasting 30min, and then washed with deionized water until the solution is colorless and odorless. After freeze-drying for 24h, a reduced graphene oxide film, i.e., a graphene film, is obtained.
[0102] Fig. 9 For the graphene film prepared in this comparative example, it can be seen that the graphene sheets are arranged along the horizontal direction of the graphene film and no vertical heat conduction channel is formed.
[0103] Example 4: Thermal conductivity test
[0104] For the graphene films provided in Examples 1, 2, 3 and Comparative Example 1, the thermal conductivity perpendicular to the film axis was characterized by the laser scattering method (DB32 / T 3596-2019). The test results are as follows:
[0105] Table 1 Thermal conductivity of different graphene films in the vertical direction
[0106] Thermal conductivity W / (m·K) Example 1 512 Example 2 120 Example 3 420 Comparative Example 1 5
[0107] It can be seen from Table 1 that the vertical graphene film prepared by the preparation method provided by the present invention (prepared in Example 1 and Example 3) has a higher thermal conductivity in the vertical direction, and has significant advantages over the traditional horizontally oriented graphene film. The main reasons are as follows:
[0108] (1) A step-by-step widening channel was developed as a spinning nozzle to avoid changes in the vertical orientation of graphene sheets during the spinning process of wide membranes.
[0109] (2) The step-by-step widening channel has good scalability. By connecting multiple step-by-step widening channels in parallel, the width of the graphene membrane can be effectively increased.
[0110] (3) The present invention is based on wet spinning technology, and forms wet spinning membrane technology by adjusting the viscosity of the spinning solution, selecting a suitable coagulation bath, adding additives and other technical improvements. This technology has the advantages of wet spinning being easy to scale up industrially, easy to prepare continuously, high reliability and low cost, and has good market application prospects.
[0111] Embodiment 5:
[0112] Wet spinning membranes using a single coaxial, step-by-step widening channel:
[0113] The preparation method is the same as that in Example 1, except that ferric nitrate and nickel nitrate are replaced by sodium chloride and calcium chloride, respectively, to prepare a vertical graphene film.
[0114] Wet spinning membranes using two parallel coaxial progressively widened channels:
[0115] The preparation method is the same as that in Example 3, except that ferric nitrate and nickel nitrate are replaced by ferric chloride and calcium chloride, respectively, to prepare a vertical graphene film.
[0116] Embodiment 6:
[0117] Wet spinning membranes using a single coaxial, step-by-step widening channel:
[0118] (1) The preparation method is the same as that in Example 1, except that the mass ratio of graphene oxide in the graphene oxide solution to the metal salt in the mixed metal salt solution is 10:3, the amount of graphene oxide used remains unchanged, and the mass ratio of iron nitrate to nickel nitrate remains unchanged, and a vertical graphene film is prepared.
[0119] (2) The preparation method is the same as that in Example 1, except that the mass ratio of graphene oxide in the graphene oxide solution to the metal salt in the mixed metal salt solution is 10:6, the amount of graphene oxide used remains unchanged, and the mass ratio of iron nitrate to nickel nitrate remains unchanged, and a vertical graphene film is prepared.
[0120] Wet spinning membranes using two parallel coaxial progressively widened channels:
[0121] (1) The preparation method is the same as that in Example 3, except that the mass ratio of graphene oxide in the graphene oxide solution to the metal salt in the mixed metal salt solution is 10:3, the amount of graphene oxide used remains unchanged, and the mass ratio of iron nitrate to nickel nitrate remains unchanged, and a vertical graphene film is prepared.
[0122] (2) The preparation method is the same as that in Example 3, except that the mass ratio of graphene oxide in the graphene oxide solution to the metal salt in the mixed metal salt solution is 10:6, the amount of graphene oxide used remains unchanged, and the mass ratio of iron nitrate to nickel nitrate remains unchanged, and a vertical graphene film is prepared.
[0123] The present invention provides a vertical graphene film and a method for preparing the same. There are many methods and approaches to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention. All components not specified in this embodiment can be implemented by existing technologies.
Claims
1. A method for preparing a vertical graphene film, It is characterized in that The steps include: (1) preparing a graphene oxide solution; (2) mixing a metal salt with a first solvent to obtain a mixed metal salt solution; adding the mixed metal salt solution to the graphene oxide solution prepared in step (1), mixing, and centrifuging to obtain a graphene oxide spinning solution; (3) pumping the graphene oxide spinning solution obtained in step (2) into a stepwise widening channel in a coagulation bath, and standing and coagulating in the coagulation bath after wet spinning to obtain a gel vertical graphene oxide membrane; (4) taking the gel vertical graphene oxide film obtained in step (3) out of the coagulation bath, performing a first washing, and obtaining a vertical graphene oxide film after freeze-drying; reducing the vertical graphene oxide film, performing a second washing after the reduction is completed, and obtaining a vertical graphene film after freeze-drying; The step-by-step widening channel is a coaxial step-by-step widening channel or a plurality of coaxial step-by-step widening channels arranged in parallel.
2. The preparation method according to claim 1, It is characterized in that In step (1), in the graphene oxide solution, the solute is graphene oxide, the concentration of graphene oxide is 5.0 to 15.0 mg / mL, and the solvent in the solution is preferably water.
3. The preparation method according to claim 1, It is characterized in that In step (2), the metal salt is a combination of any two of ferric nitrate, nickel nitrate, ferric chloride, sodium chloride and calcium chloride; the first solvent is preferably water; and the mass concentration of the metal salt in the mixed metal salt solution is 0.1% to 1.0%.
4. The preparation method according to claim 1, It is characterized in that In step (2), the mass ratio of graphene oxide in the graphene oxide solution to the metal salt in the mixed metal salt solution is 10:1-6; the centrifugation speed is 5000-20000 rpm, and the centrifugation time is 0.5-4h.
5. The preparation method according to claim 1, It is characterized in that In step (3), the graphene oxide membrane spinning stock solution is pumped into the stepwise widening channel at a flow rate of 0.1 to 1.0 mL / min; the wet spinning is carried out at room temperature; and the standing time is 2 h to 24 h.
6. The preparation method according to claim 1, It is characterized in that In step (3), the coagulation bath contains a solute and a solvent; the solute is any one or a combination of cetyltrimethylammonium bromide, sodium chloride and calcium chloride; the solvent is a combination of water and other substances, or anhydrous ethanol; the other substance is ethanol or glycerol; the volume concentration of the other substance in the solvent is 30% to 50%; the concentration of the solute in the coagulation bath is 0.1 to 10 g / L.
7. The preparation method according to claim 1, It is characterized in that The coaxial step-by-step widening channel has n levels; the coaxial step-by-step widening channel includes an entrance channel, a first-level widening rectangular channel, a second-level widening rectangular channel, ... an n-1th-level widening rectangular channel and an nth-level widening rectangular channel; the corresponding side lengths of the cross sections of the rectangular channels of different levels are parallel to each other, and n is greater than or equal to 2; The coaxial step-by-step widening channel, from the first-step widening rectangular channel to the n-step widening rectangular channel, has corresponding lengths of rectangular cross sections that increase step by step, and corresponding widths of rectangular cross sections that are all equal; The cross section of the inlet channel is circular or rectangular; when the cross section of the inlet channel is circular, the diameter of the cross section of the inlet channel is smaller than the length of the cross section of the first-stage widened rectangular channel; when the cross section of the inlet channel is rectangular, the length of the cross section of the inlet channel is smaller than the length of the cross section of the first-stage widened rectangular channel; The graphene oxide spinning stock solution flows in from the inlet channel, flows through the first-stage widened rectangular channel, the second-stage widened rectangular channel, ... the n-1-stage widened rectangular channel in sequence, and flows out from the n-stage widened rectangular channel.
8. The preparation method according to claim 1 or claim 7, It is characterized in that The plurality of parallel arranged coaxial progressively widening channels are composed of m parallel arranged coaxial progressively widening channels; m is greater than or equal to 2; The directions of the m parallel arranged coaxial progressively widening channels from the entrance channel to the nth widening rectangular channel are the same; The n-number of coaxial progressively widening channels arranged in parallel may be different or the same, the cross-sectional areas of the corresponding progressively widened rectangular channels may be the same or different, the length of the rectangular cross-section of the last-level widened rectangular channel may be on the same vertical plane and the width may be the same; the last-level widened rectangular channels of multiple coaxial progressively widened channels arranged in parallel may be interconnected.
9. The preparation method according to claim 1, It is characterized in that In step (4), in the first washing, the detergent used is any one or a combination of hydrochloric acid aqueous solution, ether, ethyl acetate and water; the reduction method is high temperature reduction, hydroiodic acid reduction or hydrazine hydrate reduction; the hydroiodic acid reduction has a reduction temperature of 60 to 80° C. and a reduction time of 6 to 8 hours; and in the second washing, the detergent used is any one or a combination of ethanol and water.
10. The vertical graphene film prepared by the preparation method according to any one of claims 1 to 9.
11. Use of the vertical graphene film according to claim 10 in preparing a thermal conductive material.
Citation Information
Patent Citations
Oxidized graphene dry-jetting and wet-spinning method
CN106894113A
Preparation method of graphene heat dissipating fin
CN110255538A
Preparation method of graphene film
CN112125297A
Graphene / graphene quantum dot vertical fiber as well as preparation method and application thereof
CN114411285A
Graphene assembly fiber as well as preparation method and application thereof
CN114990734A
Cited By
Graphene-based electrothermal film, preparation method thereof and application of graphene-based electrothermal film in heating chassis of chef machine
CN119854985A
High-strength and high-elasticity graphene metamaterial-based stress sensor and application thereof
CN119958735A
High-strength high-elasticity graphene metamaterial-based stress sensor and application thereof
CN119958735B
Vertically-oriented continuous graphene film material as well as preparation method and application thereof
CN122145191A