Composite flux and method for X fluorescence detection of 11 elements of ferrosilicon alloy by direct oxidative melting sample preparation
By using a composite flux composed of 99.50% Li2B4O7-0.50% LiI, 99.0% Li2B4O7-1.0% LiBr and Li2B4O7 for direct oxidation melting sample preparation, combined with an X-ray fluorescence spectrometer, the problems of low detection efficiency and safety risks in the existing technology are solved. It achieves rapid and accurate detection of 11 elements in ferrosilicon alloys, reduces costs and improves safety.
Patent Information
- Application Number
- CN202410708866.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-03
AI Technical Summary
Existing detection methods cannot effectively and simultaneously detect 11 elements other than carbon and sulfur in ferrosilicon alloys, and there are problems such as low detection efficiency, high cost and safety risks.
A composite flux composed of 99.50% Li2B4O7-0.50% LiI, 99.0% Li2B4O7-1.0% LiBr and Li2B4O7 was used to prepare the sample through direct oxidation and melting, and the X-ray fluorescence spectrometer was used to detect Si, Fe, Mn, Cr, P, Al, Ca, Ti , V, Ni, Cu and other 11 elements, the oxidant and heating parameters are designed to achieve rapid and accurate detection.
It achieves efficient detection of 11 elements in ferrosilicon alloys, shortens detection time, reduces costs, is simple to operate, has high detection accuracy and precision, avoids environmental pollution from acid gas and waste acid, and improves detection safety.
Smart Images

Figure CN118724007A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of alloy detection, and specifically relates to a composite flux and a method for directly oxidizing and melting a sample to detect 11 elements of a ferrosilicon alloy by X-ray fluorescence. Background Art
[0002] Ferrosilicon alloys are widely and massively used in steel smelting, mainly for deoxidation and silicon supplementation. As a major element and an important regulating element for the quality and performance of steel, silicon can significantly improve the strength, hardness and elasticity of steel, increase the magnetic permeability of steel, and reduce the hysteresis loss of transformer steel. In GB2272-2020 "Ferrosilicon", ferrosilicon alloys are mainly divided into four categories: high silicon ferrosilicon, ordinary ferrosilicon, low aluminum ferrosilicon, and high purity ferrosilicon. With the improvement of the quality requirements of ferrosilicon in steel smelting, high purity ferrosilicon is further subdivided into other varieties such as low carbon, low titanium, high purity ferrosilicon, etc.
[0003] Nowadays, with the rapid development of new energy, the role of ferrosilicon alloys in increasing steel smelting varieties and improving steel quality has become more diverse and specific, which also requires strict control of the internal components of ferrosilicon alloys, and the elements that need to be tested are also increasing. The elements that need to be tested today are Si, Fe, Mn, Cr, C, P, S, Al, Ca, Ti, V, Ni, Cu, etc., reaching more than thirteen.
[0004] There are eleven methods for detecting the content of alloy elements in ferrosilicon. The detection of carbon and sulfur elements in ferrosilicon adopts GB / T4333.10-2019 "Determination of carbon content in ferrosilicon by infrared absorption method" and GB / T4333.7-2019 "Determination of sulfur content in ferrosilicon by infrared absorption method and chromatographic separation barium sulfate weight method". These two methods can achieve synchronous detection and are relatively convenient to use. There is no single method for synchronous detection of the other eleven elements.
[0005] The existing detection method GB / T24194-2009 "Determination of aluminum, calcium, manganese, chromium, titanium, copper, phosphorus and nickel content in ferrosilicon by inductively coupled plasma atomic emission spectrometry" can only detect 8 trace elements in ferrosilicon. It uses a quaternary acid dissolution system of nitric acid, hydrofluoric acid, hydrochloric acid and perchloric acid. The operation process is complicated, the detection of a single sample takes more than 3 hours, and the detection efficiency is low. In addition, an expensive inductively coupled plasma atomic emission spectrometer is required. The equipment that meets the requirements of trace detection costs more than 700,000 yuan. Argon excitation cooling is required during detection. A variety of chemical reagents and glassware are used during sample dissolution. A high-power electric hot plate is used for sample dissolution, and a high-power fume hood is used for ventilation. Therefore, the laboratory configuration facilities are required to be more, and the detection cost is high. In addition, perchloric acid smoke dissolution is used. Since anhydrous perchloric acid is easy to accumulate in the air duct under the fume hood, if it is not cleaned in time, it is very easy to cause explosion safety accidents. There have been many reports in China, so there are great safety risks in the detection. In addition, the large amount of acid gas and waste acid residue generated during the dissolution process cannot be discharged directly into the air and surface water. Environmental protection facilities must be added for disposal, which increases the cost of equipment procurement and environmental protection treatment. If the treatment does not meet the standards, it is easy to cause social complaints and government penalties.
[0006] The prior art also has the detection method GB / T4333.5-2016 "Determination of silicon, manganese, aluminum, chromium and iron content of ferrosilicon by wavelength dispersive X-ray fluorescence spectrometry (molten glass sheet method)", which can detect two major elements of silicon and iron, as well as three trace elements of manganese, aluminum and chromium, but can only detect 5 elements, which cannot meet the requirements of detecting more than 11 elements. In addition, two steps must be completed when preparing the molten glass sheet, one step is the pre-oxidation of the sample, and the other step is the melting of the sample. In the pre-oxidation process of the sample, three steps must be performed. The first step is to use lithium tetraborate to melt and make a cup, followed by weighing and mixing the sample for a long time of high-temperature oxidation, and the third step is to weigh and add potassium iodide after taking out the pre-oxidized sample. The whole operation process is complicated and the experiment fails if there is a slight mistake. In the analysis and detection, the operator has been melting, making cups, placing samples, taking samples, clamping platinum crucibles and other repeated operations in front of the high-temperature furnace, which is labor-intensive and high temperature can easily cause human discomfort. Due to the shortcomings of this method, there are not many domestic applications and promotions.
[0007] In summary, the existing detection methods can detect a total of twelve types of elements in ferrosilicon, but none of them covers vanadium. Analysts are persistently researching and inventing a method to simultaneously detect all elements except carbon and sulfur, in order to achieve efficient and low-cost detection.
[0008] For example, the patent "A method for quickly determining the content of multiple elements in ferrosilicon" with publication number CN113960016A published on January 21, 2022, the patent "A method for determining the content of manganese, phosphorus, aluminum, chromium, nickel, vanadium and titanium in high-purity ferrosilicon" with publication number CN115078339A published on September 20, 2022, and the patent "A method for X-ray fluorescence spectrometry analysis of the content of main elements in low-silicon ferrosilicon" with publication number CN111650231A published on September 11, 2020, and other existing technologies, some of which have improved the quaternary acid solution system, but there are still problems of multiple positions coexisting and environmental protection treatment of acid gas and acid liquid; some use the tablet pressing method for detection, and the accuracy and precision of the results cannot meet the high quality control requirements; some detected elements still do not meet the expected requirements of more than 11 kinds.
[0009] The patent "Method for determining the content of elements in ferroalloys and pretreatment method of samples thereof" with publication number CN 104502169 A published on April 8, 2015 adopts a tabletting method for detection. The ferroalloy is first melted with an alkaline mixed flux to form balls, followed by grinding, tabletting and detection. However, its operation process is relatively complicated and the detection accuracy cannot meet the requirements. Summary of the invention
[0010] The object of the present invention is to provide a composite flux, using 99.50% Li2B4O7-0.50% LiI,
[0011] 99.0% Li2B4O7-1.0% LiBr and Li2B4O7 are used as the base composite flux. First, 99.50% Li2B4O7-0.50% LiI is laid on the bottom layer, then 99.0% Li2B4O7-1.0% LiBr is laid, and finally Li2B4O7 is laid. By utilizing the large repose angle of the last laid Li2B4O7, a hemispherical concave cavity can be dug out to hold the sample and the oxidant, and then covered with Li2B4O7 for oxidation melting sample preparation, which can not only completely oxidize the sample, participate in sample melting, and form a glass melt, but also does not affect the accuracy of the test results; at the same time, it avoids contact and corrosion with the platinum crucible.
[0012] Another object of the present invention is to provide a method for X-ray fluorescence detection of 11 elements of ferrosilicon alloys by direct oxidation melting sample preparation, using the above-mentioned composite flux as a primer composite flux, using Li2CO3 and LiOH as oxidants, designing oxidation melting heating parameters, being able to directly oxidize melting and make slices, conveniently and accurately using an X-ray fluorescence spectrometer for detection, and realizing the detection of 11 elements including Si, Fe, Mn, Cr, P, Al, Ca, Ti, V, Ni, and Cu in ferrosilicon alloys, and detecting the 11 elements in a wide range, from high to low different contents, from the lowest to ppm level, and the highest to constant level. Using the method of the present invention, the detection time of a single sample is less than 120 minutes, the detection cost is lower than the national standard method, the detection process is simple, and the detection accuracy and precision are high.
[0013] The specific technical solutions of the present invention are as follows:
[0014] A composite flux comprising 99.50% Li2B4O7-0.50% LiI, 99.0% Li2B4O7-1.0% LiBr and Li2B4O7;
[0015] The mass ratio of 99.50% Li2B4O7-0.50% LiI, 99.0% Li2B4O7-1.0% LiBr and Li2B4O7 is: 4:1:3;
[0016] The 99.50% Li2B4O7-0.50% LiI is laid on the bottom layer of the crucible, followed by 99.0% Li2B4O7-1.0% LiBr, and the top layer is Li2B4O7;
[0017] The 99.50% Li2B4O7-0.50% LiI refers to a mixture of 99.50% Li2B4O7 by mass and 0.50% LiI by mass; its impurity content is ≤100ppm, it is a 0.5mm bead, and its repose angle is 15°; the reagent does not powder or get damp in the air, its water absorption rate is less than 0.1% in 2 hours, and its uniformity reaches more than 99.9%, which indicates the uniformity of distribution of each element in the reagent. Because this reagent is a mixed reagent of Li2B4O7 and LiI, it is required to be very uniform when mixing and balling. A certain amount of reagent is randomly weighed, and the content of I is required to be close to 99.9%.
[0018] The 99.0% Li2B4O7-1.0% LiBr refers to a mixture of 99.0% Li2B4O7 by mass and 1.0% LiBr by mass, with an impurity content of ≤100ppm, a 0.5mm bead, and a repose angle of 15°; the reagent does not powder or become damp in the air, has a water absorption rate of less than 0.1% in 2 hours, and a uniformity of more than 99.9%, which indicates the uniformity of the distribution of each element in the reagent. Because the reagent is a mixed reagent of Li2B4O7 and LiBr, it is required to be very uniform when mixing and balling. A certain amount of reagent is randomly weighed, and the Br content is required to be close to 99.9%.
[0019] The coarse particles of Li2B4O7 are of high quality and purity, with a particle size of 0.5 to 3.5 mm, and are in an irregular state with many edges and corners, and a repose angle of 47°.
[0020] The present invention provides a method for X-ray fluorescence detection of 11 elements in ferrosilicon alloys by direct oxidation melting sample preparation, using the composite flux, and the specific method comprises the following steps:
[0021] 1) In the center of the crucible, first lay 99.50% Li2B4O7-0.50% LiI on the bottom layer of the crucible, then lay
[0022] 99.0% Li2B4O7-1.0% LiBr, lay Li2B4O7 on the top, use the Li2B4O7 on the top to dig out a hemispherical cavity, pour the sample and oxidant into the cavity, and then cover it with Li2B4O7;
[0023] 2) heating the platinum crucible to perform oxidation melting;
[0024] 3) A glass melt is made and tested by an X-ray fluorescence spectrometer.
[0025] In step 1), a hemispherical concave cavity is dug out using the uppermost layer of Li2B4O7, so that the center of the hemispherical concave cavity is at the center of the crucible, and the thickness of the walls of the hemispherical concave cavity is the same or substantially the same, so that the sample and the oxidant in the concave cavity are at the same or substantially the same distance from the crucible surface. This ensures the uniformity of the melt oxidation process. The flux is in direct contact with the crucible, and the sample and the oxidant are placed in the flux concave cavity, and the sample and the oxidant do not contact the crucible.
[0026] The crucible is selected from a platinum crucible, and the composition is 95wt% Pt+5wt% Au;
[0027] In step 1), the mass ratio of the total mass of 99.50% Li2B4O7-0.50% LiI, 99.0% Li2B4O7-1.0% LiBr and Li2B4O7, the sample and the oxidant is: 45:1:6;
[0028] In step 1), the mass ratio of the uppermost layer of Li2B4O7 and the covering layer of Li2B4O7 is 3:1;
[0029] In step 1), the sample is a standard sample of ferrosilicon alloy or a sample to be tested of ferrosilicon alloy;
[0030] In step 1), the oxidant is a mixture of lithium carbonate and lithium hydroxide;
[0031] The mass ratio of lithium carbonate to lithium hydroxide is 7:5;
[0032] In step 2), the platinum crucible is heated, specifically: first at 450°C for 2.5 minutes, then heated to 500°C for 2 minutes, heated at 500°C for 5 minutes, then heated to 850°C for 50 minutes, heated at 850°C for 5 minutes, then heated to 1050°C for 5 minutes, heated at 1050°C for 5 minutes, the swing angle of this process is 20°, and finally heated at 1050°C for 8 minutes, the swing angle of this process is 35°. First control the swing angle of 20°, the sample and reagent have not completely melted into a viscous liquid, and there is some scattered flux. If the swing angle is too large, the reagent and sample will be thrown out. Then control the swing angle of 35°, the sample and reagent have completely melted into a viscous liquid, and the large swing angle can be mixed more evenly.
[0033] In step 3), an X-ray fluorescence spectrometer is used for detection. First, a standard ferrosilicon alloy is used as a sample to obtain a working curve of each element Si, Fe, Mn, Cr, P, Al, Ca, Ti, V, Ni, and Cu; then the ferrosilicon alloy sample to be detected is detected, and the content of each element Si, Fe, Mn, Cr, P, Al, Ca, Ti, V, Ni, and Cu in the ferrosilicon alloy sample to be detected is obtained using the working curve of each element.
[0034] In step 3), an X-ray fluorescence spectrometer is used for detection, and the parameters are set as follows:
[0035] Detect Si element, voltage 40KV, current 70mA, PHD 5-115, channel angle 108.88, measurement time 40.00 seconds;
[0036] Detection of Fe element, voltage 40KV, current 70mA, PHD 5-145, channel angle 57.52, measurement time 40.00 seconds;
[0037] Detection of Mn element, voltage 40KV, current 70mA, PHD 15-125, channel angle 62.97, measurement time 40.00 seconds;
[0038] Detection of Cr element, voltage 40KV, current 70mA, PHD 20-155, channel angle 69.36, measurement time 40.00 seconds;
[0039] Detect P element, voltage 40KV, current 70mA, PHD 10-90, channel angle 141.03, measurement time 40.00 seconds;
[0040] Detect Al element, voltage 40KV, current 70mA, PHD 10-105, channel angle 144.58, measurement time 40.00 seconds;
[0041] Detection of Ca element, voltage 40KV, current 70mA, PHD 30-140, channel angle 113.09, measurement time 40.00 seconds;
[0042] Detection of Ti element, voltage 40KV, current 70mA, PHD 10-130, channel angle 86.14, measurement time 40.00 seconds;
[0043] Detect V element, voltage 40KV, current 70mA, PHD 20-120, channel angle 76.94, measurement time 40.00 seconds;
[0044] Detection of Ni element, voltage 40KV, current 70mA, PHD 15-100, channel angle 48.67, measurement time 40.00 seconds;
[0045] Detect Cu element, voltage 40KV, current 70mA, PHD 15-105, channel angle 45.03, measurement time 40.00 seconds.
[0046] The invention provides a method for detecting 11 elements of ferrosilicon alloy by X-ray fluorescence through direct oxidation melting sampling, which is used for detecting 11 elements including Si, Fe, Mn, Cr, P, Al, Ca, Ti, V, Ni and Cu, and the detection range is as follows: Si 45.0-80.0%, Fe 5.0-55.0%, Mn 0.010-0.70%, Cr 0.001-0.50%, P 0.003-0.10%, Al 0.02-3.0%, Ca 0.002-4.00%, Ti 0.005-0.300%, V 0.001-0.05%, Ni 0.002-0.50% and Cu 0.005-0.40%.
[0047] Although there are many detection methods in the existing technology, large-scale instrument detection includes X-ray fluorescence spectrometry and inductively coupled plasma atomic emission spectrometry. Sample decomposition includes high-temperature melting and tetrabasic acid dissolution. However, many reagents are used, the detection efficiency is low, and the detection risk is high.
[0048] The design ideas of the present invention are as follows:
[0049] First, a direct oxidation melting system is constructed, in which the oxidant and sample mixture is wrapped in the center of the entire melt, with the composite flux designed by the present invention as a base and the Li2B4O7 flux as a cover. On the one hand, the designed composite flux and oxidant can achieve complete oxidation, and on the other hand, the contact with the platinum crucible is avoided, thereby preventing the corrosion of the platinum crucible by the reducing element.
[0050] The single element silicon and iron, especially the single element iron, present in the ferrosilicon alloy easily form a solid solution with platinum at high temperature, resulting in corrosion to the platinum crucible. The bottom of the platinum crucible is covered with a thick layer of primer composite flux, which can prevent the single element metal in the alloy from directly contacting the crucible on the one hand, and can participate in the melting of the sample to form a glass melt after the alloy is oxidized, on the other hand. The repose angle of the uppermost Li2B4O7 in the primer composite flux designed by the present invention is relatively large, and a hemispherical concave cavity can be dug out, which can be completely filled with a mixture of the sample and the oxidant, and the mixture is 100% oxidized into oxides in the cavity. On the other hand, due to the hemispherical wrapping of the composite flux, the contact and corrosion of the single element metal on the surrounding of the platinum crucible are cut off. The pure Li2B4O7 flux covering the sample and the oxidant mixture prevents the splashing of the ferrosilicon alloy during the oxidation process, ensures that the sample is not lost, and on the other hand, prevents the splashing single element metal from corroding the platinum crucible.
[0051] In the present invention, the composite flux is required to form hemispherical small nests, and the composite flux is required to prevent slipping and sinking when the composite flux is dug from the center point of the platinum crucible to the inner and outer peripheries of the crucible, which requires that the static and stable stacking angle of the reagent is large enough. The amount and stacking order of the base composite flux are determined by measuring the angle of repose, and 4 grams of 99.50% Li2B4O7-0.50% LiI+1 gram of 99.0% Li2B4O7-1.0% LiBr in beads are successively laid in the crucible, and 3 grams of Li2B4O7 are weighed and laid thereon. Since the uppermost layer of Li2B4O7 reagent particles are coarse and irregular, they are not easy to slip, and hemispherical downwardly concave small nests can be conveniently dug out. In addition, considering that the 11 types of elements in silicon alloys are very susceptible to X-ray fluorescence spectrum interference caused by elements introduced by external reagents, the present invention designs a unique ratio composite flux of "4 grams of 99.50% Li2B4O7-0.50% LiI + 1 gram of 99.0% Li2B4O7-1.0% LiBr + 3 grams of Li2B4O7" to minimize the influence of the introduced elements. Compared with the blank test of other different single fluxes, considering the influence of each demoulding element on Ti and Al elements, and the superposition influence of residual elements in the reagent on the detection results, only the composite flux with a specific ratio designed by the present invention has the best effect and the least interference.
[0052] The principles for determining the types and proportions of the sample and oxidant mixture of the present invention are as follows:
[0053] Elemental silicon is a non-metal, and it undergoes the following reactions in a strong alkaline solution at room temperature:
[0054] Si+2NaOH+H2O=Na2SiO3+2H2↑
[0055] X-ray fluorescence detection is to melt at high temperature to form glass sheets before detection. Aqueous solution is not allowed at high temperature, so a low melting point strong alkali reagent must be selected. In a dry state, it is melted by heating to form a liquid state. The elemental silicon and iron elements melt and fuse with the mobile ions in the liquid state to complete oxidation. According to the principle of X-ray fluorescence formation, the selection of strong alkali reagents of light elements can reduce spectral interference. According to the reagent characteristics, the melting point of LiOH is 462℃ and the melting point of Li2CO3 is 720℃. These two types of reagents are selected for oxidation at high temperature. The specific reaction formula is as follows:
[0056]
[0057] The direction of a chemical reaction is determined by the Gibbs free energy, and its formula is: ΔG=ΔH-TΔS, where ΔG is the reaction free energy. When it is a negative value, the reaction proceeds to the right, and when it is a positive value, the reaction proceeds to the left. ΔH is the enthalpy change, ΔS is the entropy change, and T is the reaction temperature.
[0058] ΔH=1216.04+2×484.93-1649.33-2×598.93-2×110.54-241.84=92.23;
[0059] ΔS=80.33+2×37.91+2×197.90+188.74-18.83-2×90.17-2×42.80=455.92;
[0060] ΔG=ΔH-TΔS=92.23-298.15×0.45592=-43.7;
[0061] After calculation, it is found that the reaction can proceed to the right at room temperature. Since there are not many negative values, it means that the reaction speed is slow. When the temperature rises to the point where LiOH begins to melt, the reaction speed increases and elemental silicon can be gradually oxidized into lithium silicate.
[0062] LiOH and Li2CO3 are low melting point reagents, Li2CO3 is an oxidant to oxidize silicon and iron, and LiOH is a strong alkaline reagent to neutralize silicic acid. The present invention determines the starting temperature of the oxidation reaction according to the Gibbs free energy formula. In addition, in order to speed up the reaction speed, the molar number of the reactant must be greater than the reactant. After conditional testing, the ratio of the sample and the oxidant mixture is finally determined to be: 0.7000 grams of lithium carbonate + 0.5000 grams of lithium hydroxide + 0.2000 grams of sample. At this time, the oxidation effect is the best, and the melted glass sheet is transparent without spots and impurities.
[0063] NO3 should not be used for oxidation of ferrosilicon alloys - Salt and BaO-based substances are oxidized at high temperature. Due to the violent oxidation reaction, the alloy is very easy to splash, causing sample loss and damage to the platinum crucible.
[0064] The present invention is based on the direct oxidation melting temperature program curve of the oxidant characteristics, analyzes the uniformity of each element component in the glass melt by X-ray fluorescence diffractometer, and realizes the complete oxidation of the single element according to the temperature program set by the melting and boiling points of each oxidizing agent. The single element is evenly distributed in the glass sheet. Through the comparison and verification of standard substances and different national standard methods, the extreme values of silicon and iron are 0.51% and 0.21%, which are lower than the wet method detection error. Due to the complete oxidation of the single element, the damage rate of the platinum crucible caused by chemical reagent corrosion is reduced to zero.
[0065] In addition, if the content of I and Br double release agents is high, it will interfere with Ti and Al elements. However, if the sublimation volatilization reaches too low a concentration, the glass melt cannot be molded out, and even if it is molded out, it is easy to crack during the cooling stage. According to the design of the present invention, the constant temperature of 1050℃ for 5 minutes (swing angle 20°) → 1050℃ constant temperature for 8 minutes (swing angle 35°), the concentration of I and Br double release agents is about 10ppm, and the blank effects on Ti and Al are 0.015% and 0.02%. The effects can be eliminated by blank correction, and the mold forming rate of the glass melt reaches more than 99%.
[0066] Compared with the prior art, the present invention can dig out hemispherical concave holes to hold reagents and oxidants through the bottom composite flux and the ratio design, and can reduce the influence of the flux on element detection; through the selection of the oxidant, the temperature rise parameters and the swing angle setting, it can realize the one-step direct oxidation melting glass sheet making method, and obtain the X-ray fluorescence detection method of 11 elements of ferrosilicon alloy by direct oxidation melting sample preparation. The process is short, the operation is simple, the cost is saved, and it is more environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] Figure 1 is the working curve of silicon element;
[0068] Figure 2 Working curve for iron element;
[0069] Figure 3 is the working curve of manganese element;
[0070] Figure 4 This is the working curve of chromium element;
[0071] Figure 5 is the working curve of phosphorus element;
[0072] Figure 6 is the working curve of aluminum element;
[0073] Figure 7 This is the working curve of calcium element;
[0074] Figure 8 is the working curve of titanium element;
[0075] Fig. 9 is the working curve of vanadium element;
[0076] Fig.10 This is the working curve for nickel element;
[0077] Fig.11 This is the working curve for copper element;
[0078] Fig.12 Comparison of test spectra at different melting temperatures;
[0079] Fig.13 Comparison of test spectra with different melting times. DETAILED DESCRIPTION
[0080] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0081] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0082] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0083] The reagent used in the present invention is as follows:
[0084] 99.50% Li2B4O7-0.50% LiI, with an impurity content of ≤100ppm, in the form of 0.5mm beads and a repose angle of 15°; the reagent does not powder or become damp in the air, has a water absorption rate of less than 0.1% in 2 hours, and has a uniformity of more than 99.9%.
[0085] 99% Li2B4O7-1% LiBr, impurity content ≤100ppm, 0.5mm beads, repose angle of 15°; the reagent does not powder or get damp in the air, the water absorption rate is less than 0.1% in 2 hours, and the uniformity reaches more than 99.9%.
[0086] Li2B4O7, fine particles, impurity content ≤100ppm, beads, particle size ≤0.5mm;
[0087] Li2B4O7, coarse particles, high quality and pure, particle size is 0.5 ~ 3.5mm, and it is irregular, with many edges and corners, and the angle of repose is 47°.
[0088] KI, Luoyang Tenai, high quality pure;
[0089] Li2CO3, Luoyang Tenai, high quality pure;
[0090] LiOH, Xilong Chemical, analytical grade.
[0091] The equipment used in the present invention:
[0092] Platinum crucible: component Au 5wt% + Pt 95wt%, volume 30mL, referred to as "platinum crucible";
[0093] Electronic balance: Model AB204-S, Mettler Toledo, Switzerland;
[0094] Fully automatic electric melting furnace: Model FE0000-2D, CLAISSE, Canada;
[0095] Field emission scanning electron microscope: model Sigma 300, Zeiss, Germany;
[0096] X-ray fluorescence spectrometer: Model MXF-2400, Shimadzu Corporation, Japan, power 3600W, 75μm beryllium window X-ray tube, tube voltage 40kV, tube current 70mA.
[0097] The present invention is further described with reference to the following examples and comparative examples:
[0098] Example 1
[0099] A composite flux comprising 99.50% Li2B4O7-0.50% LiI, 99.0% Li2B4O7-1.0% LiBr and Li2B4O7;
[0100] The mass ratio of 99.50% Li2B4O7-0.50% LiI, 99.0% Li2B4O7-1.0% LiBr and Li2B4O7 is: 4:1:3;
[0101] The 99.50% Li2B4O7-0.50% LiI is laid on the bottom layer of the crucible, followed by 99.0% Li2B4O7-1.0% LiBr, and the top layer is Li2B4O7;
[0102] The 99.50% Li2B4O7-0.50% LiI refers to a mixture of 99.50% Li2B4O7 by mass and 0.50% LiI by mass; its impurity content is ≤100ppm, it is a 0.5mm bead, and its repose angle is 15°; the reagent does not powder or become damp in the air, its water absorption rate in 2 hours is less than 0.1%, and its uniformity reaches more than 99.9%.
[0103] The 99.0% Li2B4O7-1.0% LiBr refers to a mixture of 99.0% Li2B4O7 by mass and 1.0% LiBr by mass, with an impurity content of ≤100ppm, a 0.5mm bead, and a repose angle of 15°; the reagent does not powder or become damp in the air, has a water absorption rate of less than 0.1% in 2 hours, and has a uniformity of more than 99.9%.
[0104] The Li2B4O7 is coarse-grained, high-quality and pure, with a particle size of 0.5 to 3.5 mm, and is in an irregular state with many edges and corners, and a repose angle of 47°.
[0105] Example 2
[0106] A method for X-ray fluorescence detection of 11 elements in ferrosilicon alloy by direct oxidation melting sampling, using the composite flux of the above embodiment 1, and the specific method comprises the following steps:
[0107] 1) In the center of a 30mL platinum crucible, first weigh 4 grams of 99.50% Li2B4O7-0.50% LiI and lay it on the bottom layer, then weigh 1 gram of 99.0% Li2B4O7-1.0% LiBr and lay it on the middle layer, and finally weigh 3 grams of high-purity Li2B4O7 and lay it on the top layer, and use the Li2B4O7 on the top layer to dig out a hemispherical concave cavity. Take another 100mL glass cup, accurately weigh 0.7000 grams of Li2CO3 and 0.5000 grams of LiOH, and then weigh 0.2000 grams of sample, stir evenly with a glass rod, and slowly pour it into the concave cavity in the platinum crucible; then weigh 1 gram of high-purity Li2B4O7 to cover the mixture of sample and oxidant;
[0108] When digging out a hemispherical concave cavity in step 1), only the top layer of pure Li2B4O7 is used as much as possible. 4 grams of 99.50% Li2B4O7-0.50% LiI are laid on the bottom layer, and 1 gram of 99.0% Li2B4O7-1.0% LiBr is laid on the middle layer. Since it is a bead, it is easy to roll. If it is hit during digging, it will not affect the test result. The crucible cannot be exposed to avoid corrosion. The diameter of the hemispherical concave cavity is 25mm and the depth is 20mm, then tanɑ=25÷2÷20=0.625; check the inverse tangent function, the ɑ angle is 32°, and theoretically reaching 32° can achieve the goal of digging out a hemispherical concave cavity. The present invention adopts the above-mentioned composite flux, and the repose angle of a hemispherical concave cavity dug out is 36°, so it meets the requirements of digging a hemispherical cavity.
[0109] 2) Heat the platinum crucible for oxidation melting, specifically: place the platinum crucible into a fully automatic electric melting furnace with a set "oxidation melting heating program curve" for oxidation melting. The specific program heating curve is: 450°C constant temperature for 2.5 minutes → 2 minutes to 500°C → 500°C constant temperature for 5 minutes → 50 minutes to 850°C → 850°C constant temperature for 5 minutes → 5 minutes to 1050°C → 1050°C constant temperature for 5 minutes (swing angle 20°) → 1050°C constant temperature for 8 minutes (swing angle 35°).
[0110] 3) Making glass frits and testing them with an X-ray fluorescence spectrometer, specifically: selecting 15 types of ferrosilicon alloy standard samples in Table 1, making fused glass frits under the determined melting conditions, testing the sample glass frits with the X-ray fluorescence spectrometer parameters determined in Table 2, and drawing the working curves of the 11 types of elements as shown in FIG. Figure 1-Figure 11 .
[0111] Working curves of each element:
[0112] C i =1.343262Is i +3.349853, R=1.0000;
[0113] Fe C Fe =0.093162I Fe +0.276461, R=1.0000;
[0114] C Mn =0.242528I Mn -0.196580, R=0.9990;
[0115] Cr C Cr =0.381123I Cr -0.207739, R=0.9988;
[0116] PC P =0.474716I P -0.019685, R=0.9987;
[0117] Al C Al =1.816258I Al -0.302500, R=0.9998;
[0118] Ca C Ca =0.572386I Ca -0.173503, R=0.9999;
[0119] Ti C Ti =0.300195I Ti -0.268099, R=0.9980;
[0120] VC V =0.237989I V -0.209158, R=0.9973;
[0121] C Ni =0.071869I Ni -0.452069, R=0.9981;
[0122] C Cu =0.064273I Cu -0.514199, R=0.9986;
[0123] Cs i is the concentration of Si element, Is i is the fluorescence intensity of Si element, and so on for other elements.
[0124] Table 1 Element composition of 15 types of ferrosilicon alloys
[0125]
[0126] Table 2X Fluorometer Detection Parameters
[0127]
[0128] The analysis spectra of each element are shown in Table 3 below.
[0129] Table 3 Spectral line energy and spectroscopic crystal
[0130] Element Name Si Fe Mn Cr P Al Ca Ti V Ni Cu Ka Energy 1.74 6.40 5.90 5.41 2.01 1.49 3.69 4.51 4.95 7.48 8.05 Analyze spectral lines Kα <![CDATA[K α / K β ]]> Kα Kα Kα Kα Kα Kα Kα Kα Kα Spectroscopic crystal PET LIF LIF LIF GE PET LIF LIF LIF LIF LIF
[0131] Using the working curves of the 11 elements that have been drawn, two other standard samples and 6 samples were randomly selected and tested in the same manner as in Example 2. The test results are shown in Table 4. From the comparative analysis of the tests, it is found that the allowable difference range specified in the national testing standards for ferrosilicon alloys is fully met.
[0132] Table 4 Comparison of test results of Example 2X fluorescence method detection
[0133]
[0134]
[0135] The X-ray fluorescence detection method for 11 types of elements in Example 2 was successfully used in January 2024 and has been applied to daily detection. Eight samples were randomly checked on March 12, 2024. From the comparative data analysis in Table 3, the results of the X-ray fluorescence method provided by the present invention (the extreme difference of 8 samples) and the national standard method (X-ray fluorescence + ICP) were all within the allowable error range.
[0136] Note: There is no standard value range for Ni and Ti of standard sample GT-07. This data is not counted when calculating the range.
[0137] Comparative Example 1
[0138] In order to compare the interference of different fluxes on the detection results, a blank test comparison was carried out. The specific process was as follows: accurately weigh the composite flux composed of different raw materials, add 0.7000 g of lithium carbonate and 0.5000 g of lithium hydroxide, stir evenly in a 100 ml glass cup with a glass rod, and slowly pour into a platinum crucible; melt at 1050°C in an alloy melting furnace for 25 minutes, and mold the glass frit into a glass frit, which was used to detect 11 types of elements.
[0139] The selection of composite fluxes with different raw material compositions is as follows:
[0140] 1. Blank test of pure Li2B4O7 with high-quality coarse particles, particle size of 0.5-3.5mm, irregular shape, many edges and corners, and repose angle of 47°: Since pure Li2B4O7 cannot be demolded after melting, the selected weighing ratio is 9 grams of high-quality pure Li2B4O7 + 1 gram of KI mixed melting, 6 parts of the same ratio of flux are weighed, and glass frits are obtained under the determined experimental process. X-fluorescence spectrometer is used for detection under the experimental parameters formulated in Tables 2 and 3. The content range of 11 elements is shown in Table 5.
[0141] Table 5 Blank test data of 9g high-purity Li2B4O7+1g KI mixed melting
[0142]
[0143]
[0144] As can be seen from Table 3, among the 11 elements, the blanks of 7 elements, such as Mn, Cr, P, Al, V, Ni, and Cu, are zero, and the effect is good; but there are blanks in Si, Fe, Ca, and Ti. The contents of Si and Fe themselves are about 80% and 20%, so the blank impact is not large, but the contents of Ca and Ti themselves are about 0.10%, especially for Ti, the blank detection value is more than 5 times the sample content, so it is not suitable for the analysis of 11 elements.
[0145] 2. Blank test of fine-particle high-quality pure Li2B4O7: Since pure Li2B4O7 cannot be demolded after melting, the weighing ratio selected is 9 grams of Li2B4O7 + 1 gram of KI mixed and melted. 6 parts of the same ratio of reagents are weighed, and glass flakes are obtained under the determined experimental process. X-ray fluorescence spectrometer is used for detection under the same parameters. The analysis results of 11 elements are shown in Table 6.
[0146] Table 6 Blank test data of 9g Li2B4O7+1g KI mixed melting
[0147]
[0148] It can be seen from Table 6 that for the 11 elements, the blank value of the fine-particle Li2B4O7 used this time is smaller than that of the above-mentioned coarse-particle Li2B4O7. The blank values of 8 elements including Mn, Cr, P, Al, Ca, V, Ni and Cu are zero, which shows a good effect. However, there are still blank values for Si, Fe and Ti. The contents of Si and Fe are about 80% and 20% respectively, and the blank value has little effect. However, the Ti content is about 0.10%, and the blank detection value still reaches more than 5 times the sample content. Therefore, it is still not suitable for the analysis of 11 elements.
[0149] 3. Impurity content ≤100ppm, in the form of 0.5mm beads, with an angle of repose of 15°; the reagent does not powder or become damp in the air, has a water absorption rate of less than 0.1% in 2 hours, and a uniformity of more than 99.9%. 99.50% Li2B4O7-0.50% LiI flux blank test: Since the reagent is a mixed flux with its own LiI release agent, no other release agent is needed. 10 grams of the melt is directly weighed to obtain a glass frit, and the X-fluorescence spectrometer is used for detection under the same parameters. The analysis results of 11 elements are shown in Table 7.
[0150] Table 7 99.50%Li2B4O7-0.50%LiI blank test data
[0151]
[0152]
[0153] It can be seen from Table 7 that for the 11 elements, the 99.50% Li2B4O7-0.50% LiI mixed flux has a better effect than the Li2B4O7+KI combined flux. Although the blank contents of 10 elements, including Si, Mn, Cr, P, Al, Ca, Ti, V, Ni and Cu, were detected, the results were generally low, especially the blank content of Ti element was significantly reduced, accounting for only about 10% of the sample content. However, due to the obvious increase in Ni and Cu contents, reaching 5 to 10 times the sample content, and the large volatility of the blank detection results of elements such as Al and Ca, it is still not suitable for the analysis of 11 elements in ferrosilicon alloys.
[0154] 4. Impurity content ≤100ppm, in the form of 0.5mm beads, with an angle of repose of 15°; the reagent does not powder or become damp in the air, has a water absorption rate of less than 0.1% in 2 hours, and a uniformity of more than 99.9%. 99.0% Li2B4O7-1.0% LiBr blank test: Since the reagent is also a mixed flux and has its own LiBr release agent, no other release agents need to be added. 10 grams of the melt is directly weighed to obtain a glass melt, and the X-fluorescence spectrometer is used for detection under the same parameters. The analysis results of 11 elements are shown in Table 8.
[0155] Table 8 99.0%Li2B4O7-1.0%LiBr blank test data
[0156]
[0157] It can be seen from Table 8 that the blank test results of 11 elements, 99.0% Li2B4O7-1.0% LiBr mixed flux has its unique feature, that is, the detection value of Ti element is zero; the contents of other 10 elements such as Si and Fe are all detected, the results of 9 elements are low, and the result of Al element is high, with an average value of 1.0972%, which is more than 10 times the sample content; therefore, a single flux is not suitable for the analysis of 11 elements.
[0158] Comparing the four single or mixed fluxes, the obvious characteristics are that if the flux contains iodine release agent, the blank detection value of Ti element is high, and it increases with the increase of I element content; if the flux contains Br release agent, the blank detection value of Al element is high, and it increases with the increase of Br element content.
[0159] 5. Blank test of the above-mentioned 99.50% Li2B4O7-0.50% LiI + 99.0% Li2B4O7-1.0% LiBr + coarse-grained Li2B4O7 composite flux: Based on the blank influence brought by various reagents, the present invention provides a composite flux with a unique ratio of I and Br double demolding, the specific ratio is 4 grams of 99.50% Li2B4O7-0.50% LiI + 1 gram of 99.0% Li2B4O7-1.0% LiBr + 3 grams of coarse-grained Li2B4O7, 6 parts of the composite flux are weighed, melted to obtain glass frits, and detected by X-ray fluorescence spectrometer under the same parameters. The analysis of 11 elements is shown in Table 9.
[0160] Table 9 Blank test data of composite flux of the present invention
[0161]
[0162] As can be seen from Table 9, the I and Br double demolding composite fluxes of the present invention are generally low in the blank test. Although the data of Si, Fe, Ni, and Cu are higher, the content of the comparative sample itself is low. From the blank value precision analysis, the extreme values of the 11 types of elements are all below 0.03, which fully meets the sample detection primer requirements. In addition, the composite flux itself contains ultra-low content of I and Br double demolding agents, and no release agent needs to be added, which avoids the influence of the incompletely sublimated release agent on elements such as Al, Ti, Cr, and Ni. The composite flux provided by the present invention is a composite primer flux with the characteristics of each element for melting, and the blank detection values of 11 types of elements are relatively low, which can achieve synchronous detection of 11 types of elements.
[0163] Comparative Example 2
[0164] In order to prevent the unoxidized ferrosilicon alloy from contacting the platinum crucible, the sample mixed with the oxidant needs to be wrapped in a composite flux. The present invention is designed to dig out a hemispherical recess in the composite flux. The thickness of the recess wall at each location of the hemispherical recess is the same or substantially the same, so that the sample and the oxidant in the recess are at the same or substantially the same distance from the crucible surface. This ensures the uniformity of the melting oxidation process. The flux is in direct contact with the crucible, and the sample and the oxidant are placed in the flux recess, and the sample and the oxidant do not contact the crucible. The evenly stirred oxidant and sample mixture is poured into the recess, and oxidation is completed in the recess. Shaking and melting afterwards will not damage the platinum crucible.
[0165] The composite flux designed in the present invention digs a hemispherical concave cavity, and a slope of more than 35° must be accumulated from the inner and outer peripheries of the crucible to the center point, with the outer periphery being higher and the center point being lower. The angle at which the reagents are accumulated in a static state is called the angle of repose, which refers to the maximum angle at which the bulk materials can maintain natural stability when stacked.
[0166] The repose angle test was carried out on each flux, and the results are shown in Table 10:
[0167] Table 10 Comparison of repose angles of four types of fluxes
[0168]
[0169] As can be seen from Table 10, the three types of fluxes, Li2B4O7-0.50%LiI, Li2B4O7-1.0%LiBr and fine-grained Li2B4O7, are all 0.5 mm beads, which are particularly easy to slide and have a repose angle of 15°. The coarse-grained Li2B4O7 has a particle size of 0.5-3.5 mm and is irregular with many edges and corners, and a repose angle of 47°. Therefore, the ternary composite flux system of Li2B4O7 (coarse particles) + Li2B4O7-0.50%LiI + Li2B4O7-1.0%LiBr designed by the present invention can achieve a repose angle of more than 35°, which meets the requirements of the nesting, and also reduces the melting cost.
[0170] Comparative Example 3
[0171] The same method as in Example 2 was used, except that the highest constant temperature in step 2) was changed from the highest constant temperature of 1050°C in Example 2 to two different constant temperatures of 950°C and 1000°C. The molten glass sheet was subjected to a microscopic analysis of the oxidation state of the sample and the melting state of the flux using a field emission scanning electron microscope. The specific analysis is shown in Fig.12 From left to right, the highest constant temperatures are 950℃, 1000℃, and 1050℃. From the analysis of the microscopic spectrum magnified 50 times, the unmelted foreign matter in the spectrum is gradually decreasing, and at 1050℃, the melting effect is generally good.
[0172] Comparative Example 4
[0173] The same method as in Example 2 was used except that the constant temperature time of 35° swing in step 2) was changed. The melting effects were compared for 3, 5, and 8 minutes, respectively. The comparative analysis results are shown in FIG. Fig.13 .
[0174] from Fig.13 The comparison chart shows that when the swing melting of Example 2 of the present invention reaches 8 minutes, the quality of the melt can meet the analysis requirements of X-ray fluorescence, but it cannot meet the analysis requirements at other times. Moreover, 35° is the maximum swing angle of the present invention. If the angle is larger, the molten reagent will be thrown out, and it is found that the molten material around the platinum crucible is stuck to the crucible.
[0175] Comparative Example 5
[0176] The experiment was carried out according to Example 2, except that the composite flux formula was changed, as follows:
[0177] Weigh 6.5000g of 99.5% fine particles of Li2B4O7+0.5% LiI and spread them in the crucible first, then weigh 1.0000g of coarse particles of Li2B4O7 and spread them as the base composite flux into the platinum crucible, dig a hemispherical concave cavity on the 1g coarse particles of Li2B4O7 flux, inevitably dig into the lower layer of 99.5% fine particles of Li2B4O7+0.5% LiI, dig a certain depth slightly The degree of the crucible should be small, and the platinum crucible should not be dug out, otherwise it will corrode easily; weigh 0.7000g of lithium carbonate, 0.5000g of lithium hydroxide, and 0.2000g of sample in a glass cup, mix them with a glass rod and slowly pour them into the hemispherical cavity of the platinum crucible; weigh 1.5000g of 99.5% fine particles Li2B4O7+0.5%LiI to cover the sample; select two standard samples and four samples for comparison by different methods, and the results are shown in Table 11.
[0178] Table 11 Comparative Example 5 Test Results
[0179]
[0180] It can be seen from Table 11 that when fine particles 99.50% Li2B4O7-0.50% LiI + coarse particles Li2B4O7 are used as base composite flux, the analysis results of titanium element are basically close to the standard value of the high content, but the fluctuation of the titanium content ≤0.020% is far beyond the national standard range; in addition, some glass melts showed crystallization.
[0181] Comparative Example 6
[0182] The experiment was carried out according to Example 2, except that the composite flux formula was changed, as follows:
[0183] Weigh 5.000 g of 99.5% Li2B4O+0.5% LiI, 2.0000 g of 99% Li2B4O+1% LiBr, and 1.0000 g of coarse-grained Li2B4O, and dig a hemispherical socket in the same manner as in Example 2 for use; weigh 0.7000 g of lithium carbonate, 0.5000 g of lithium hydroxide, and 0.2000 g of sample in a glass cup, mix them with a glass rod, and slowly pour them into the hemispherical socket; weigh 1.0000 g of coarse-grained 100% Li2B4O to cover the sample; continue to select a standard sample and five samples for comparison by different methods, and the results are shown in Table 12.
[0184] Table 12 Comparative Example 6 Test Results
[0185]
[0186] As can be seen from Table 12, by adding 2 grams of 99.0% Li2B4O7-1.0% LiBr, the low-content Ti element detection results were improved, and were close to the results of the two methods in Example 2; however, the aluminum element results fluctuated greatly, and the results of the two methods were quite different; in addition, cracks appeared in some glass frits.
[0187] The excellent performance of the composite primer flux provided by the present invention is further demonstrated by the tests of Comparative Examples 5 and 6, two different primer composite fluxes with unique ratios from the present invention. By comparing Example 2 with Comparative Examples 5 and 6, it can be seen that the accuracy and precision of the results obtained by using primer composite fluxes with different ratios under the same melting conditions and X-ray fluorescence spectrometer analysis conditions cannot meet the national standard requirements.
[0188] Compared with the prior art, the present invention has the following outstanding effects:
[0189] 1. The present invention adopts the designed composite flux to carry out direct oxidation melting method, and the detection speed is increased by 45.45%. In the past, the three elements Si, Fe and P in the 11 elements of silicon-iron alloy were reported by X-ray fluorescence detection, and the time for a single sample was 120 minutes. The remaining 8 elements were reported by acid-dissolved samples through inductively coupled plasma (ICP) spectrometer, and the reporting time for a single sample was 100 minutes. The direct oxidation melting X-ray fluorescence detection provided by the present invention can report 11 element components simultaneously, and no longer needs ICP spectrum detection after acid dissolution. The detection time is reduced by 100 minutes, and the speed is increased by 45.45%.
[0190] Second, the direct oxidation melting method adopted by the present invention saves 30% of the reagent detection cost. In the past, the three elements Si, Fe, and P of ferrosilicon alloys were all detected by reagent oxidation melting, and the price of each element was 3.46 yuan. The remaining 8 elements were detected by ICP spectrometer, and the price of each element was 2.89 yuan. The direct oxidation melting X-ray fluorescence detection of the present invention increases the cost of a single melting sample because the base composite flux part uses high-quality reagents. However, since a melting sample can simultaneously analyze 11 elements, the cost per element is 2.14 yuan, and the total cost is reduced by about 30%. If the composite flux is mass-produced in the later stage, the detection cost will be further reduced.
[0191] 3. The direct oxidation melting method of the present invention improves the detection efficiency by 50%. In the past, 11 elements required two methods to detect and two detection posts to be configured. Now only one method is required and only one detection post is configured, which improves the detection efficiency by more than 50%.
[0192] Fourth, the direct oxidation melting method adopted by the present invention completely solves the environmental pollution problem of waste acid gas and waste acid water. X-ray fluorescence detection is a high-temperature melting glass sheet method, which does not require any acid or alkali reagents. It also completely solidifies the carbon in the reagents and samples without external discharge, meeting the carbon reduction requirements. After the acid dissolution ICP spectroscopy method is stopped, the large amount of HF, HCl, HNO3, and HCLO4 used in the acid dissolution, the acid gas generated by the dissolution and the external acid water are achieved zero discharge.
[0193] Fifth, the present invention adopts direct oxidation melting method, and the safety of the detection method is improved. Since there is no need to use HCLO4 to dissolve the sample, the possibility of HCLO4 volatilizing, remaining, accumulating at high temperature, and exploding with organic matter after heating is completely eliminated.
[0194] 6. The present invention can achieve accurate detection of 11 elements, and the detection range of each element is shown in Table 13.
[0195] Table 13 Detection content range of 11 elements of the present invention
[0196]
[0197] The present invention can directly oxidize and melt to form sheets, and the X-ray fluorescence spectrometer can conveniently and accurately detect 11 elements in the ferrosilicon alloy, and the detection cost is lower than that of the national standard method.
[0198] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A composite flux, characterized in that: The composite flux includes 99.50% Li2B4O7-0.50% LiI, 99.0% Li2B4O7-1.0% LiBr and Li2B4O7.
2. The composite flux according to claim 1, characterized in that: Said The mass ratio of 99.50% Li2B4O7-0.50% LiI, 99.0% Li2B4O7-1.0% LiBr and Li2B4O7 is: 4:1:
3.
3. The composite flux according to claim 1 or 2, characterized in that: The coarse particles of Li2B4O7 are of high quality and purity, with a particle size of 0.5 to 3.5 mm, and are in an irregular state with a repose angle of 47°.
4. A method for X-ray fluorescence detection of 11 elements in ferrosilicon alloys by direct oxidation melting sampling, characterized in that: The method uses the composite flux according to any one of claims 1 to 3, and the specific method comprises the following steps: 1) In the center of the crucible, first lay 99.50% Li2B4O7-0.50% LiI on the bottom layer of the crucible, then lay 99.0% Li2B4O7-1.0% LiBr, and lay Li2B4O7 on the top layer. Use the top layer of Li2B4O7 to dig out a hemispherical concave cavity, pour the sample and oxidant into the cavity, and then cover it with Li2B4O7; 2) heating the platinum crucible to perform oxidation melting; 3) A glass melt is made and tested by an X-ray fluorescence spectrometer.
5. The method according to claim 4, characterized in that The mass ratio of the total mass of 99.50% Li2B4O7-0.50% LiI, 99.0% Li2B4O7-1.0% LiBr and Li2B4O7, the sample and the oxidant is 45:1:6; the mass ratio of the top layer Li2B4O7 and the covering Li2B4O7 is 3:
1.
6. The method according to claim 4 or 5, characterized in that: In step 1), the oxidant is a mixture of lithium carbonate and lithium hydroxide.
7. The method according to claim 6, characterized in that The mass ratio of the lithium carbonate to lithium hydroxide is 7:
5.
8. The method according to claim 4, characterized in that In step 2), the platinum crucible is heated, specifically as follows: first, the temperature is kept constant at 450°C for 2.5 minutes, then the temperature is increased to 500°C for 2 minutes, the temperature is kept constant at 500°C for 5 minutes, then the temperature is increased to 850°C for 50 minutes, the temperature is kept constant at 850°C for 5 minutes, then the temperature is increased to 1050°C for 5 minutes, the temperature is kept constant at 1050°C for 5 minutes, the swing angle is 20° during this process, and finally the temperature is kept constant at 1050°C for 8 minutes, the swing angle is 35° during this process.
9. The method according to claim 4, characterized in that An X-ray fluorescence spectrometer is used for detection. First, a ferrosilicon alloy standard sample is used as a sample to obtain a working curve of each element Si, Fe, Mn, Cr, P, Al, Ca, Ti, V, Ni, and Cu. The working curve is used to obtain the concentration of each element Si, Fe, Mn, Cr, P, Al, Ca, Ti, V, Ni, and Cu in the ferrosilicon alloy sample to be tested.
10. The method according to claim 4, characterized in that X-ray fluorescence spectrometer was used for detection, and the parameters were set as follows: Detect Si element, voltage 40KV, current 70mA, PHD 5-115, channel angle 108.88, measurement time 40.00 seconds; Detection of Fe element, voltage 40KV, current 70mA, PHD 5-145, channel angle 57.52, measurement time 40.00 seconds; Detection of Mn element, voltage 40KV, current 70mA, PHD 15-125, channel angle 62.97, measurement time 40.00 seconds; Detection of Cr element, voltage 40KV, current 70mA, PHD 20-155, channel angle 69.36, measurement time 40.00 seconds; Detect P element, voltage 40KV, current 70mA, PHD 10-90, channel angle 141.03, measurement time 40.00 seconds; Detect Al element, voltage 40KV, current 70mA, PHD 10-105, channel angle 144.58, measurement time 40.00 seconds; Detection of Ca element, voltage 40KV, current 70mA, PHD 30-140, channel angle 113.09, measurement time 40.00 seconds; Detection of Ti element, voltage 40KV, current 70mA, PHD 10-130, channel angle 86.14, measurement time 40.00 seconds; Detect V element, voltage 40KV, current 70mA, PHD 20-120, channel angle 76.94, measurement time 40.00 seconds; Detection of Ni element, voltage 40KV, current 70mA, PHD 15-100, channel angle 48.67, measurement time 40.00 seconds; Detect Cu element, voltage 40KV, current 70mA, PHD 15-105, channel angle 45.03, measurement time 40.00 seconds.
Citation Information
Patent Citations
Method for detecting contents of alloying elements in ferrotitanium and ferrovanadium by X-fluorescence fusion method
CN101592571A
Sample preparation method of titanium-iron alloy melt sample for spectral analysis
CN110596169A
Fuse piece sample preparation method for measuring element content in silicon oxide through X-ray fluorescence spectrum
CN117214213A
Melting sample preparation method for determining main components of ferrosilicon alloy by using X-ray fluorescence spectrum
CN117420164A
Process for producing a lithium borate thermoluminescent and fluorescent substance
US4290909A