A conductive MOF modified gas-sensitive material and its preparation method and application
By modifying the conductive metal organic frame material on the upper surface of the graphene-based material, the conductive MOF modified graphene gas-sensitive material is formed, which solves the problem of insufficient sensitivity of a single MOF material in trace gas detection, and achieves high-sensitivity gas detection at room temperature , suitable for gas identification and health management in complex environments.
Patent Information
- Application Number
- CN202210420150.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-04-20
AI Technical Summary
It is difficult to construct chemical resistance gas sensors for existing single three-dimensional insulated MOF materials, and a single conductive MOF material is usually detected at a ppm level when detecting gas, making it difficult to achieve rapid trace detection and analysis.
Conductive MOF is used to modify graphene gas-sensitive materials, and by modifying conductive metal organic frame materials on the upper surface of graphene-based materials, forming composite materials, increasing specific surface area and pores, improving gas adsorption, diffusion and desorption capabilities, and achieving trace amounts at room temperature Selective detection of organic and inorganic volatile gases.
It realizes high sensitivity detection of various gases at room temperature, reduces the impact of humidity on gas detection, meets the gas detection requirements in complex environments, and is suitable for the identification and health management of trace gases.
Smart Images

Figure HDA0003605436740000011 
Figure HDA0003605436740000012 
Figure HDA0003605436740000021
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of sensor material preparation, and specifically relates to a conductive MOF-modified gas-sensitive material and a preparation method and application thereof. Background Art
[0002] Metal-organic frameworks (MOFs) are a new type of nanoporous crystalline materials formed by the coordination of metal cations and organic linkers. This type of material has a large internal porosity, specific surface area, and excellent reversible adsorption properties. The variable pore size and surface environment can provide advantages for the selectivity and sensitivity of gas sensing. Due to the presence of polar metal centers and non-polar organic connecting parts in the MOFs structure, it is guaranteed to have the ability to selectively adsorb inorganic and organic volatile gas molecules. However, most three-dimensional metal-organic framework materials are insulating materials. Due to their insulating properties, it is difficult to construct commonly used chemical resistance gas sensors.
[0003] Nowadays, insulating MOFs are used for gas sensing in surface acoustic wave (SAW) sensors, quartz crystal microbalances (QCM), impedance sensors, and capacitive gas sensors (Sensors and Actuators B: Chemical, 2019, 278: 153-164.). A few two-dimensional MOF materials have good conductivity, such as M-HHTP and M-HITP metal organic framework materials prepared with HHTP (2,3,6,7,10,11-hexahydroxytriphenylene) and HATP·6HCl (triphenylene-2,3,6,7,10,11-hexaamine hexahydrochloride) as organic ligands (Chem. Commun., 2018, 54, 7873--7891). Due to their special electrical properties, this type of 2D MOF material can be directly prepared into chemiresistive gas sensors or sensor arrays (J.Am.Chem.Soc.2015, 137, 13780-13783; Sensors 2017, 17, 2192).
[0004] However, the reported gas sensors composed of single MOF materials are basically in the range of ppm (10 -6 ) levels to detect different gases (Chem. Commun., 2018, 54, 7873--7891), which hinders their gas detection requirements at lower levels required in practical applications. Ming-ShuiYao et al. used Cu 3 (HHTP) 2 NH was detected at 100 ppm 3, and its response and recovery times are 1.36 min and 9.11 min (Angew. Chem. 2017, 129, 16737-16741), which shows that a single conductive MOF material may be difficult to achieve the goal of rapid trace detection and analysis of gases. Summary of the invention
[0005] In view of this, the present application provides a conductive MOF-modified gas-sensitive material and a preparation method and application thereof, wherein the gas-sensitive material can realize the selective detection of trace organic and inorganic volatile compounds at room temperature.
[0006] The present invention provides a conductive MOF-modified gas-sensitive material, which can be used to reduce the influence of humidity in the gas detection process. The conductive MOF-modified gas-sensitive material includes a graphene assembly material and a conductive metal organic framework material modified on the surface thereof;
[0007] The graphene assembly material has a two-dimensional layered structure and is assembled from a polycation electrolyte and negatively charged graphene oxide.
[0008] The present invention provides a method for preparing the conductive MOF modified gas-sensitive material as described above, comprising the following steps:
[0009] In the liquid phase, a polycationic electrolyte such as polydiallyldimethylammonium chloride is initially assembled with negatively charged graphene oxide, and then a conductive metal organic framework material is introduced to perform surface modification to obtain a conductive MOF-modified gas-sensitive material.
[0010] In an embodiment of the present invention, the molecular weight of the polydiallyldimethylammonium chloride is 200-350 KDa; preferably, 10-60 μL of a 1 wt% polydiallyldimethylammonium chloride solution is added to 0.5 mL of a graphene oxide solution for initial assembly.
[0011] In an embodiment of the present invention, after the initial assembly, a conductive metal organic framework material suspension having an equal volume to the graphene oxide solution is added, and surface modification is achieved by oscillation; the conductive metal organic framework material includes but is not limited to Co 3 (HITP) 2 、Ni 3 (HITP) 2 , Cu 3 (HITP) 2 、Co 3 (HHTP) 2 Cu 3 (HHTP) 2 .
[0012] The present invention provides a gas sensor chip, which is prepared by combining the conductive MOF modified gas sensitive material mentioned above with an electrode.
[0013] In an embodiment of the present invention, the substrate of the electrode is a flexible substrate or a hard substrate, and the flexible substrate is preferably a PET film, a PEN film, a PI film or a PC film; the hard substrate is preferably silicon, glass, ceramic or a PCB board.
[0014] The present invention provides a method for preparing the gas sensor chip as described above, comprising the following steps:
[0015] Step 1, preparing the conductive MOF modified gas-sensitive material self-assembly suspension described above;
[0016] Step 2: Use a PDMS film to confine the ITO-PET interdigital electrode and treat the electrode with oxygen plasma. Then, take the conductive MOF modified gas-sensitive material self-assembled suspension prepared in step 1 and drop it into the electrode confinement area and dry it at room temperature; place the dried electrode in a reducing vapor atmosphere for reduction to obtain the gas sensor chip.
[0017] The present invention provides application of the above-mentioned gas sensor chip in gas detection.
[0018] In an embodiment of the present invention, the gas detection is the detection and identification of different organic / inorganic gases and human exhaled breath.
[0019] In an embodiment of the present invention, in the gas detection, the carrier gas used is the background gas of the sample gas; the sample gas is an organic or inorganic volatile gas, including but not limited to nitric oxide, nitrogen dioxide, hydrogen sulfide, ammonia, acetone, isoprene or water vapor.
[0020] In an embodiment of the present invention, the gas detection conditions satisfy at least one of the following: gas concentration of 0.1-10 ppm, room temperature, and different humidity of 0%-98%.
[0021] In the embodiment of the present invention, Co 3 (HITP) 2 Surface modified gas-sensitive materials are used to detect nitric oxide and nitrogen dioxide.
[0022] Single 3D insulating MOFs cannot construct chemiresistive gas sensors, while single conductive MOFs usually detect gases at ppm levels, such as Cu 3 (HHTP) 2 The detection is carried out at 1ppm-100ppm.
[0023] Compared with the prior art, the present invention provides a conductive MOF-modified gas-sensitive material, which is a surface-modified graphene gas sensing material, mainly composed of a graphene assembly material and a conductive metal organic framework material modified on its surface, wherein the graphene assembly material has a two-dimensional layered structure and is assembled from a polycation electrolyte and a negatively charged graphene oxide. The embodiment of the present invention uses a polycation electrolyte PDDA to intercalate a negatively charged two-dimensional material graphene, and realizes the initial assembly of PDDA and graphene through electrostatic self-assembly, which can not only overcome the problem of easy self-aggregation of graphene in solution, but also introduce a conductive metal organic framework material (MOF) on this basis to further modify its surface, so as to realize the stable assembly of the material in the liquid phase. That is, the present invention uses a conductive MOF to modify graphene to obtain a gas-sensitive material, further increases the specific surface area and pores of graphene, is conducive to gas adsorption, diffusion and desorption, improves the detection sensitivity of multiple gases, and realizes the selective detection of trace organic and inorganic volatile gases at room temperature.
[0024] Furthermore, the present invention uses a conductive MOF containing hydrophobic aromatic groups to modify graphene gas-sensitive materials, which are gas-sensitive materials that introduce hydrophobic aromatic groups. This can reduce the influence of humidity factors on gas detection and provide a basis for the subsequent practical application of gas-sensitive materials.
[0025] Furthermore, the present invention uses two-dimensional conductive MOF to modify graphene gas-sensitive materials, because three-dimensional conductive MOF cannot be well dispersed in the aqueous solution required by the experimental scheme, while two-dimensional conductive MOF can achieve this.
[0026] Reducing the impact of humidity on gas detection is also crucial in the development of gas sensors. At present, many reports have pointed out that indium selenide, indium oxide, tungsten oxide, etc. can be used as gas-sensitive materials (most of which are MO or composite / doped materials containing MO) to produce effective moisture-resistant photoelectric gas sensors, resistive gas sensors, etc. (Anal. Chem. 2020, 92, 11277-11287; IEEE SENSORS JOURNAL, VOL. 21, NO. 8, APRIL 15, 2021; Sensors and Actuators: B. Chemical 350 (2022) 130884). When they detect gases within the humidity fluctuation range, they are only slightly affected, but their detection often requires exposure to light (such as UV or infrared) or high temperature (such as 275°C), which hinders them from realizing gas sensing without light assistance and at room temperature.
[0027] The present invention can also solve such a problem by modifying MOF on the surface of graphene-based gas-sensitive materials. The composite gas-sensitive material provided by the present invention can obtain a relatively stable response value and a high sensitivity for gases in a wide humidity range of 0-98% at room temperature and without other auxiliary conditions, thereby realizing the selective detection of trace (ppb level) organic / inorganic volatile compounds, meeting complex breath detection requirements, and can be further applied to gas detection devices to realize breath-related disease identification and health management. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The graphene oxide / PDDA / Co described in Example 2 3 (HITP) 2 Scanning electron micrograph of a gas sensing material; Co with a hydrophobic aromatic group is attached 3 (HITP) 2 The structure diagram of
[0029] Figure 2 The graphene oxide / PDDA / Co described in Example 2 3 (HITP) 2 C1s spectrum of gas sensing materials;
[0030] Figure 3 The graphene oxide / PDDA / Co described in Example 2 3 (HITP) 2 N1s spectrum of gas sensing materials;
[0031] Figure 4 The graphene oxide / PDDA / Co in Example 3 3 (HITP) 2 The response kinetic curves of gas-sensitive materials to different gases under concentration gradient;
[0032] Figure 5 The graphene oxide / PDDA / Co in Example 3 3 (HITP) 2 Comparison of the response results of gas-sensitive materials to six different gases at 1ppm or 2ppm concentration; the gases include: 1ppm (NO, NO 2 , H 2 S. NH 3 , Ace), 2ppm(Iso);
[0033] Figure 6 The graphene oxide / PDDA / Co described in Example 4 3 (HITP) 2Comparison of the response kinetics of gas-sensitive materials to nitric oxide and nitrogen dioxide at a concentration gradient of 0.1-1ppm; the comparison materials include graphene oxide, graphene oxide / Co 3 (HITP) 2 , graphene oxide / PDDA materials;
[0034] Figure 7 The graphene oxide / PDDA / Co in Example 5 3 (HITP) 2 Comparison of the response results of the gas-sensitive material to nitric oxide gas at a concentration of 200ppb at different humidity levels;
[0035] Figure 8 for Figure 7 The relative response change value of
[0036] Fig. 9 This is a schematic diagram of the exhaled gas and ambient gas collection device described in Example 6;
[0037] Fig.10 The graphene oxide / PDDA / Co 3 (HITP) 2 Diagram of detection and identification results of exhaled gas by gas-sensitive materials at room temperature. DETAILED DESCRIPTION
[0038] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0039] The present application provides a conductive MOF-modified gas-sensitive material, which includes a graphene assembly material and a conductive metal-organic framework material modified on its surface; the graphene assembly material has a two-dimensional layered structure, which is assembled from a polycationic electrolyte and negatively charged graphene oxide, and the conductive MOF-modified gas-sensitive material can be used to reduce the influence of humidity in the gas detection process.
[0040] The gas-sensitive material provided by the present invention has the characteristics of good pore structure, etc., which is conducive to gas adsorption, diffusion and desorption, improves the detection sensitivity of various gases, and can realize the selective detection of trace organic and inorganic volatile compounds at room temperature.
[0041] It is known that graphene materials have the characteristics of high specific surface area, strong electron transport ability, adjustable energy band, high flexibility while maintaining a certain mechanical strength, so they have great advantages in gas sensing. Graphene-based composite gas-sensitive materials can be used in ppb (10-9 ) level to detect gases. However, the commonly used graphene oxide is unstable in the liquid phase and is prone to self-aggregation, which reduces the sensitivity of the sensing material.
[0042] It has been reported that compounding negatively charged graphene oxide with some polycationic electrolytes (PDDA, PAH, PEI, etc.) can prevent the occurrence of agglomeration and improve gas accessibility. Lin Wang et al. and Ping Ni et al. assembled graphene oxide with polycationic electrolyte PDDA to maintain the graphene oxide layered system (Separation and Purification Technology 160 (2016) 123-131, Carbon 48 (2010) 2100-2105). There are also reports confirming that MOF materials can be compounded with graphene to obtain good gas sensing materials, most of which are three-dimensional insulating MOFs, such as Cu-BTC and Zn-MOF (Materials Research Bulletin 99 (2018) 152-160, Journal of Alloys and Compounds 816 (2020) 152509), etc., while there are few reports on compounding with two-dimensional conductive MOF for gas sensing. In the liquid phase, conductive MOF materials and graphene oxide are difficult to assemble stably, and the sensitivity is low when detecting trace gases.
[0043] The conductive MOF modified gas-sensitive material provided by the present invention is a novel multi-component composite material obtained by compounding a conductive MOF material with graphene and other gas sensing materials.
[0044] In the composite gas-sensitive material described in the embodiment of the present invention, the main body is a graphene assembly material with a two-dimensional layered structure, which is formed by electrostatic self-assembly of negatively charged graphene oxide intercalated with a polycationic electrolyte PDDA; the polycationic electrolyte is preferably polydiallyldimethylammonium chloride (PDDA), which is beneficial to the stable assembly of the material in the liquid phase and the detection of trace gases at room temperature (especially beneficial to improving sensitivity).
[0045] In a preferred embodiment of the present invention, the molecular weight of the polydiallyldimethylammonium chloride is 200-350KDa. In the embodiment of the present invention, 10-60 μL of a 1wt% polydiallyldimethylammonium chloride solution is preferably added to 0.5 mL of a graphene oxide solution for initial assembly; the amount of PDDA solution is preferably 15-50 μL, more preferably 20-40 μL.
[0046] The surface of the graphene assembly material of the present invention is modified with a conductive MOF material; the metal of the modified conductive MOF material can be cobalt (Co), nickel (Ni), copper (Cu), including but not limited to Co3 (HITP) 2 、Ni 3 (HITP) 2 , Cu 3 (HITP) 2 、Co 3 (HHTP) 2 or Cu 3 (HHTP) 2 Etc. For example, Co 3 (HHTP) 2 :Co-HHTP metal organic framework material prepared with HHTP (2,3,6,7,10,11-hexahydroxytriphenylene) as organic ligand. Due to the excellent conductivity of conductive MOF itself, it has great advantages in the preparation of chemical resistance gas sensors.
[0047] The gas-sensitive material of the conductive MOF-modified graphene described in the embodiment of the present invention can be recorded as graphene oxide / PDDA / MOF composite material, etc., which further increases the specific surface area and pores of graphene, is beneficial to gas adsorption, diffusion and desorption, improves the detection sensitivity to various gases, and realizes the selective detection of trace organic and inorganic volatile gases at room temperature.
[0048] In some embodiments of the present invention, the composite material has wrinkles on the surface, has an interlaced mesh structure, and has a conductive MOF material attached to the surface (carbon-metal bonds, etc.). The gas-sensitive material described in some embodiments of the present invention has a hydrophobic aromatic group, which can reduce the influence of humidity factors on gas detection, and provide a basis for the subsequent practical application of gas-sensitive materials.
[0049] The embodiment of the present invention provides a method for preparing the conductive MOF modified gas-sensitive material as described above, comprising the following steps:
[0050] In the liquid phase, a polycationic electrolyte such as polydiallyldimethylammonium chloride is initially assembled with negatively charged graphene oxide, and then a conductive metal organic framework material is introduced to perform surface modification to obtain a conductive MOF-modified gas-sensitive material.
[0051] Furthermore, the present invention provides a gas sensor chip, which is prepared by combining the conductive MOF-modified gas-sensitive material described above with electrodes.
[0052] The embodiment of the present invention uses a step-by-step assembly strategy to initially assemble the polycationic electrolyte PDDA and negatively charged graphene oxide in the liquid phase, and then introduces a conductive metal organic framework material to further modify its surface; the present invention can stably assemble in the liquid phase to prepare a gas-sensitive material suspension. The present invention overcomes the problem of liquid phase assembly of a single MOF material and graphene oxide through a step-by-step assembly strategy, realizes the stable assembly of materials in the liquid phase and the selective detection of trace organic and inorganic volatile compounds at room temperature.
[0053] The present invention provides a method for preparing a conductive MOF-modified gas-sensitive material and a gas sensor chip, which is as follows:
[0054] Step 1: Preparation of graphene oxide / PDDA / MOF self-assembly suspension:
[0055] A trace amount of PDDA is added to a certain amount of graphene oxide solution, and after oscillation, an equal volume of MOF suspension is preferably added to the graphene oxide solution, and oscillated on an oscillator overnight. After that, it can be washed by centrifugation with deionized water for 3 times and re-dispersed with an equal volume of deionized water.
[0056] The present invention adopts a step-by-step assembly of sensing materials, and assembles conductive MOF materials and graphene oxide in a liquid phase with the assistance of PDDA, thereby overcoming the self-aggregation problem of graphene oxide and the assembly problem of a single MOF material and graphene oxide, and realizing the stable assembly of materials in a liquid phase.
[0057] Preferably, the molecular weight Mw of the PDDA is 200-350KDa. In the embodiment of the present invention, 10-60 μL of a 1wt% polydiallyldimethylammonium chloride solution is added to 0.25-0.75 mL of a graphene oxide solution for initial assembly, preferably 0.5 mL; the amount of PDDA solution is preferably 15-50 μL, more preferably 20-40 μL, and further preferably 20 μL. In addition, the concentration of the graphene oxide solution can be 0.25-1.0 mg / mL, preferably 0.5 mg / mL.
[0058] Specifically, the MOF suspension is a suspension obtained by ultrasonically dispersing a conductive MOF material in deionized water, and the conductive MOF material includes but is not limited to Co 3 (HITP) 2 , Ni 3 (HITP) 2 , Cu 3 (HITP) 2 ,Co 3 (HHTP) 2 , Cu 3 (HHTP) 2 wait.
[0059] Step 2: Preparation of graphene oxide / PDDA / MOF material gas sensor chip:
[0060] The ITO-PET interdigitated electrodes can be confined using a PDMS membrane (PDMS membrane is also called polydimethylsiloxane film), and the electrodes can be treated with oxygen plasma;
[0061] Then, the suspension of PDDA-assisted graphene oxide and metal organic framework material self-assembly (graphene oxide / PDDA / MOF self-assembly suspension) prepared in step 1 is added dropwise into the electrode limit domain, the addition amount is 5 μL-10 μL, preferably 10 μL, preferably dried at room temperature, and then the electrode is placed in a gas atmosphere of reducing steam at 70 to 120° C. for reduction. After 15 to 30 minutes, the graphene oxide / PDDA / MOF material gas sensor chip (gas sensor chip) is obtained.
[0062] In some embodiments of the present invention, the substrate can be of appropriate thickness and can be a flexible substrate such as PET (polyethylene terephthalate) film, PEN (polyethylene naphthalate) film, PI (polyimide) film, PC (polycarbonate) film, or a hard substrate such as silicon, glass, ceramic, PCB board (printed circuit board).
[0063] In addition, the reducing vapor includes but is not limited to hydrazine hydrate.
[0064] In the preparation of the conductive MOF modified gas-sensitive material, in step 1 of a certain embodiment, graphene oxide / PDDA / Co 3 (HITP) 2 The preparation process of the self-assembly suspension is preferably as follows:
[0065] 20 μL PDDA (Mw. 200-350 kDa, 1% Wt.) was added to 0.5 mL of graphene oxide solution (0.5 mg / mL), and after oscillation, 0.5 mL Co 3 (HITP) 2 The suspension was shaken overnight on a shaker, then washed three times by centrifugation with deionized water, and redispersed with an equal volume of deionized water to obtain graphene oxide / PDDA / Co 3 (HITP) 2 Self-assembled suspension.
[0066] In the preparation of the conductive MOF modified gas-sensitive material, in step 1 of a certain embodiment, graphene oxide / PDDA / Ni 3 (HITP) 2 The preparation process of the self-assembly suspension is preferably as follows:
[0067] 20 μL PDDA (Mw. 200-350 kDa, 1% Wt.) was added to 0.5 mL of graphene oxide solution (0.5 mg / mL), and after oscillation, 0.5 mL Ni 3 (HITP) 2 The suspension was shaken overnight on a shaker, then washed three times with deionized water by centrifugation, and redispersed with an equal volume of deionized water to obtain graphene oxide / PDDA / Ni 3 (HITP) 2 Self-assembled suspension.
[0068] In the preparation of the conductive MOF modified gas-sensitive material, in step 1 of a certain embodiment, graphene oxide / PDDA / Cu 3 (HITP) 2 The preparation process of the self-assembly suspension is as follows:
[0069] 20 μL PDDA (Mw. 200-350 kDa, 1% Wt.) was added to 0.5 mL of graphene oxide solution (0.5 mg / mL), and after oscillation, 0.5 mL Cu 3 (HITP) 2 The suspension was shaken overnight on a shaker, then washed three times by centrifugation with deionized water, and redispersed with an equal volume of deionized water to obtain graphene oxide / PDDA / Cu 3 (HITP) 2 Self-assembled suspension.
[0070] In the preparation of the conductive MOF modified gas-sensitive material, in step 1 of a certain embodiment, graphene oxide / PDDA / Co 3 (HHTP) 2 The preparation process of the self-assembly suspension is preferably as follows:
[0071] 20 μL PDDA (Mw. 200-350 kDa, 1% Wt.) was added to 0.5 mL of graphene oxide solution (0.5 mg / mL), and after oscillation, 0.5 mL Co 3 (HHTP) 2 The suspension was shaken overnight on a shaker, then washed three times by centrifugation with deionized water, and redispersed with an equal volume of deionized water to obtain graphene oxide / PDDA / Co 3 (HHTP) 2 Self-assembled suspension.
[0072] In the preparation of the conductive MOF modified gas-sensitive material, in step 1 of a certain embodiment, graphene oxide / PDDA / Cu3 (HHTP) 2 The preparation process of the self-assembly suspension is as follows:
[0073] 20 μL PDDA (Mw. 200-350 kDa, 1% Wt.) was added to 0.5 mL of graphene oxide solution (0.5 mg / mL), and after oscillation, 0.5 mL Cu 3 (HHTP) 2 The suspension was shaken overnight on a shaker, then washed three times by centrifugation with deionized water, and redispersed with an equal volume of deionized water to obtain graphene oxide / PDDA / Cu 3 (HHTP) 2 Self-assembled suspension.
[0074] At the same time, the present invention also provides the application of the gas sensor chip as described above in gas detection, and can provide a gas detection device, including the gas sensor chip, and a connected gas collection unit, a display unit, etc. In an embodiment of the present invention, the gas detection is the detection and identification of different organic / inorganic gases and human exhaled breath. Preferably, the conditions for gas detection in the present invention meet at least one of the following: gas concentration of 0.1-10ppm, room temperature, 0%-98% different humidity.
[0075] The conductive MOF modified gas-sensitive material described in the embodiment of the present invention can detect and identify gas at room temperature, and its application method is as follows:
[0076] The conductive MOF-modified graphene gas sensor chip is placed in a gas flow cell. During the test, the carrier gas is first introduced until the baseline tends to be stable, and then the sample gas is introduced at the same flow rate. Under a given voltage, the current value flowing through the gas-sensitive material is tested by a picoammeter to obtain data on the relationship between the current value and time, thereby obtaining the response image of the gas-sensitive material to different samples of gas;
[0077] The carrier gas is the background gas of the sample gas; the sample gas may be organic or inorganic volatile gas, including but not limited to nitric oxide (NO), nitrogen dioxide (NO 2 ), hydrogen sulfide (H 2 S), ammonia (NH 3 ), acetone, isoprene, water vapor (H 2 O) etc.
[0078] The response value can be defined as R% = [(II 0 ) / I 0 ]×100, where I is the current value measured in the sample gas atmosphere, I 0 It is the current value measured in a carrier gas atmosphere.
[0079] The conductive MOF modified gas-sensitive material described in the present invention can detect gas at different humidity levels, and its application method is as follows:
[0080] The conductive MOF-modified graphene gas sensor chip is placed in a gas flow cell. During the test, a carrier gas is first introduced until the baseline tends to be stable, and then a dry sample gas or a moist sample gas after being subjected to different saturated salt solutions is introduced at the same flow rate. Under a given voltage, the current value flowing through the gas-sensitive material is tested by a picoammeter to obtain data on the relationship between the current value and time, thereby obtaining a response image of the gas-sensitive material to the sample gas at different humidity levels;
[0081] The carrier gas is the background gas of the sample gas; the saturated salt solution includes but is not limited to saturated potassium acetate solution, saturated magnesium nitrate solution, saturated sodium chloride solution, saturated potassium sulfate solution, etc. The sample gas is an organic or inorganic volatile gas, including but not limited to nitric oxide, acetone, isoprene and other gases that are insoluble in water.
[0082] The response value can be defined as R% = [(II 0 ) / I 0 ]×100, where I is the current value measured in a dry or humid sample gas atmosphere, I 0 It is the current value measured in a carrier gas atmosphere.
[0083] The conductive MOF modified gas-sensitive material described in the present invention can detect and identify mixed gases (human exhaled breath) at room temperature, and its application method is as follows:
[0084] The conductive MOF-modified graphene gas sensor chip is placed in a gas flow cell. During the test, the pre-treated ambient gas is first introduced until the baseline tends to be stable, and then the pre-treated human exhaled gas is introduced at the same flow rate. Under a given voltage, the current value flowing through the gas-sensitive material is tested by a picoammeter to obtain data on the relationship between the current value and time. The difference in the response values when different mixed gases (human exhaled gas) are introduced can be used for gas identification.
[0085] The human exhaled gas is the exhaled gas of a healthy individual or the exhaled gas of a patient with a simulated airway inflammatory disease, wherein the airway inflammatory disease includes but is not limited to asthma, chronic obstructive pulmonary disease (COPD) and other airway inflammatory diseases; the exhaled gas of a patient with a simulated airway inflammatory disease is achieved by introducing a quantitative standard gas into the exhaled gas of a healthy individual.
[0086] In some embodiments of the present invention, the pretreatment method is to allow the gas to pass through a Teflon hard tube with an inner diameter of 4-8 mm and immersed in ice water for 20-40 cm.
[0087] The response value can be defined as R% = [(II 0 ) / I 0 ]×100, where I is the current value measured in the mixed gas atmosphere, I 0 It is the current value measured in ambient gas atmosphere.
[0088] In summary, the present invention provides a conductive MOF modified gas-sensitive material, a preparation method and application thereof, preferably PDDA and graphene oxide are initially assembled and then introduced into a conductive MOF material for modification, so as to realize the detection and identification of different organic / inorganic gases and human exhaled breath (such as exhaled breath of patients with airway inflammation diseases). The composite material provided by the present invention can realize the selective detection of trace (ppb level) organic / inorganic volatile compounds at room temperature with good sensitivity.
[0089] In order to better understand the technical content of the present invention, the following specific examples are provided to further illustrate the present invention. The present invention uses commercially available raw materials. The manufacturer of graphene oxide (10 mg / mL) is Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, and the MOF material is prepared by the reference method, and its specific surface area is large, such as Co 3 (HITP) 2 About 805.5m 2 / g、Ni 3 (HITP) 2 About 884.7m 2 / g. The reducing vapor is hydrazine hydrate.
[0090] Embodiment 1:
[0091] This example mainly provides graphene oxide / PDDA / Co with different PDDA contents 3 (HITP) 2 The preparation method of the gas-sensitive material and the selection of the optimal proportion of PDDA content are as follows:
[0092] Step 1: Preparation of graphene oxide / PDDA / Co 3 (HITP) 2 Self-assembly suspension: 10 μL, 20 μL, 30 μL, 40 μL, and 60 μL of PDDA (Mw. 200-350 kDa, 1% Wt.) were added to 0.5 mL of graphene oxide solution (0.5 mg / mL), and after oscillation, 0.5 mL of Co 3 (HITP) 2 The suspension was shaken overnight on a shaker, then washed three times with deionized water by centrifugation, and redispersed with an equal volume of deionized water to obtain graphene oxide / PDDA / Co 3(HITP) 2 Self-assembled suspension.
[0093] Step 2: Preparation of graphene oxide / PDDA / Co with different PDDA contents 3 (HITP) 2 Gas-sensing chip: Use PDMS film to confine the ITO-PET interdigital electrode, and treat the electrode with oxygen plasma (oxygen plasma treatment time is 30s), then take 10μL of the suspension of the five PDDA-assisted graphene oxide and MOF material self-assembly prepared in step 1, drop it into the electrode confinement, and dry it at room temperature. Place this electrode in a reducing vapor atmosphere at 70°C for 20 to 30 minutes to obtain the graphene oxide / PDDA / MOF gas sensor chip with different PDDA contents.
[0094] As an example, the five graphene oxide / PDDA / Co prepared above with different PDDA contents were 3 (HITP) 2 The gas sensor chip is used for the detection of nitric oxide. When the PDDA content is 20 μL, the graphene oxide / PDDA / Co 3 (HITP) 2 The sensitivity is best when detecting gases.
[0095] Embodiment 2:
[0096] This embodiment mainly provides a graphene oxide / PDDA / Co 3 (HITP) 2 The preparation method of the gas-sensitive material has the following specific steps:
[0097] Step 1: Preparation of graphene oxide / PDDA / Co 3 (HITP) 2 Self-assembly suspension: 20 μL PDDA (Mw. 200-350 kDa, 1% Wt.) was added to 0.5 mL of graphene oxide solution (0.5 mg / mL), and after oscillation, 0.5 mL Co 3 (HITP) 2 The suspension was shaken overnight on a shaker, then washed three times by centrifugation with deionized water, and redispersed with an equal volume of deionized water to obtain graphene oxide / PDDA / Co 3 (HITP) 2 Self-assembled suspension.
[0098] Step 2: Preparation of graphene oxide / PDDA / Co 3 (HITP) 2Gas sensor chip: The ITO-PET interdigital electrode was confined with a PDMS film, and the electrode was treated with oxygen plasma for 30 seconds, and then 10 μL of the PDDA-assisted graphene oxide and MOF material self-assembly suspension prepared in step 1 was dripped into the electrode confinement area and dried at room temperature. The electrode was placed in a reducing vapor atmosphere at 70°C for 20 minutes to obtain the graphene oxide / PDDA / MOF material gas sensor chip.
[0099] Among them, the PDDA content is 20μL of graphene oxide / PDDA / Co 3 (HITP) 2 The scanning electron microscope image of the gas-sensitive material is shown in Figure 1 , wrinkles, interlaced network structures and Co attached to the surface of the composite material can be observed. 3 (HITP) 2 , proving that the material has been composited and its structure is conducive to gas sensing. Graphene oxide / PDDA / Co with PDDA content of 20 μL 3 (HITP) 2 The X-ray photoelectron spectrum C1s and N1s spectra of gas-sensitive materials are shown in Figure 2 , Figure 3 The existence of C-Co bonds observed in the C1s spectrum of the composite material proves that the material has been composited, and the peaks of the N1s spectrum are consistent with the overall composition of the material.
[0100] In addition, the preparation methods of other MOF-modified composite materials are consistent with this embodiment and have no special steps.
[0101] Embodiment 3:
[0102] The following is the graphene oxide / PDDA / Co prepared in Example 2 3 (HITP) 2 Gas sensor chip, specifically describes the detection and identification of organic / inorganic volatile compounds at room temperature by conductive MOF-modified graphene gas-sensitive materials:
[0103] As an example, the graphene oxide / PDDA / Co prepared in Example 2 3 (HITP) 2 Gas sensor chip for the detection of nitric oxide / nitrogen dioxide / hydrogen sulfide / ammonia / isoprene / acetone: graphene oxide / PDDA / Co 3 (HITP) 2The gas sensor chip is placed in a gas flow cell. During the test, the carrier gas is first introduced until the baseline tends to be stable, and then different concentrations of nitric oxide, nitrogen dioxide, hydrogen sulfide, ammonia, isoprene, or acetone are introduced at the same flow rate. At a voltage of 1V, the current value flowing through the gas-sensitive material is tested by a picoammeter to obtain the data on the relationship between the current value and time. 3 (HITP) 2 The response value of gas-sensitive materials to different sample gases of different concentrations.
[0104] The kinetic curve of the detection of 0.1-1ppm nitric oxide standard gas is as follows: Figure 4 As shown in a, the kinetic curve for the detection of 0.1-1ppm nitrogen dioxide standard gas is as follows Figure 4 As shown in b, the kinetic curve for the detection of 0.1-1ppm hydrogen sulfide standard gas is as follows Figure 4 c shows the kinetic curve for the detection of 1-10ppm ammonia standard gas. Figure 4 d, the kinetic curve for the detection of 2-10 ppm isoprene standard gas is as shown in Figure 4 As shown in e, the kinetic curve for the detection of 1-10ppm acetone standard gas is as follows Figure 4 f. The basic trend of the above kinetic curve is that it shows linear growth at low concentrations and tends to saturation at high concentrations.
[0105] Graphene oxide / PDDA / Co 3 (HITP) 2 The detection results of gas-sensitive materials for six gases are as follows: Figure 5 As shown, under 1 ppm nitric oxide, or 1 ppm nitrogen dioxide, or 1 ppm hydrogen sulfide, or 1 ppm ammonia, or 2 ppm isoprene, or 1 ppm acetone gas, the graphene oxide / PDDA / Co 3 (HITP) 2 The gas-sensitive material is more sensitive to nitric oxide and nitrogen dioxide than the other four gases, indicating that the conductive MOF-modified graphene gas-sensitive material has a certain selectivity for different gases.
[0106] Embodiment 4:
[0107] The following is a study of single graphene oxide, graphene oxide / Co 3 (HITP) 2 Binary composite material chip, graphene oxide / PDDA binary composite material chip, graphene oxide / PDDA / Co prepared in the above Example 2 3 (HITP) 2The gas sensor chip was tested to specifically illustrate the advantages of the conductive MOF-modified graphene gas-sensitive material in detecting nitrogen oxides at room temperature compared with mono- and binary composite materials:
[0108] As an example, a single graphene oxide material, graphene oxide / Co 3 (HITP) 2 Binary composite materials, graphene oxide / PDDA binary composite materials, graphene oxide / PDDA / Co prepared in Example 2 3 (HITP) 2 Gas sensing materials, used for the detection of nitric oxide / nitrogen dioxide gas: single graphene oxide chip, graphene oxide / Co 3 (HITP) 2 Binary composite chip, graphene oxide / PDDA binary composite chip, graphene oxide / PDDA / Co 3 (HITP) 2 The gas sensor chip was placed in the gas flow cell in batches. During the test, the carrier gas was first introduced until the baseline became stable, and then different concentrations of nitric oxide or nitrogen dioxide were introduced at the same flow rate. At a voltage of 1V, the current value flowing through the gas-sensitive material was tested by a picoammeter to obtain the data on the relationship between the current value and time. 3 (HITP) 2 Binary composite materials, graphene oxide / PDDA binary composite materials, graphene oxide / PDDA / Co 3 (HITP) 2 The response value of gas-sensitive materials to different sample gases of different concentrations.
[0109] The kinetic curves of the four different materials for the detection of 0.1-1ppm nitric oxide standard gas are shown below: Figure 6 As shown in a, the kinetic curve for the detection of 0.1-1ppm nitrogen dioxide standard gas is as follows Figure 6 As shown in b, the graphene oxide / PDDA / Co 3 (HITP) 2 The sensitivity of the gas-sensitive material to nitric oxide and nitrogen dioxide is much higher than that of the other three mono- and binary materials, indicating that the conductive MOF-modified graphene gas-sensitive material has certain advantages in detecting nitrogen oxides compared with mono- and binary composite materials at room temperature.
[0110] The above-mentioned graphene oxide, graphene oxide / Co 3 (HITP) 2 , a method for preparing graphene oxide / PDDA material, the specific steps of which are as follows:
[0111] Step 1: The concentration of single graphene oxide is 0.5 mg / mL. 1.0 mL of graphene oxide solution is ultrasonically dispersed to obtain a single graphene oxide material.
[0112] Preparation of graphene oxide / Co 3 (HITP) 2 Binary materials: 0.5 mL Co 3 (HITP) 2 The suspension was added into 0.5 mL of graphene oxide solution (0.5 mg / mL) and shaken overnight on a shaker. After being shaken evenly, it was washed three times by centrifugation with deionized water and redispersed with an equal volume of deionized water to obtain graphene oxide / Co 3 (HITP) 2 Binary material suspension;
[0113] Preparation of graphene oxide / PDDA binary material: Add 20 μL PDDA (Mw. 200-350 kDa, 1% Wt.) to 1.0 mL of graphene oxide solution (0.5 mg / mL), shake on an oscillator overnight, wash by centrifugation with deionized water 3 times after shaking evenly, and redisperse with an equal volume of deionized water to obtain a graphene oxide / PDDA binary material suspension.
[0114] Step 2: Preparation of graphene oxide and graphene oxide / Co 3 (HITP) 2 2. Graphene oxide / PDDA sensor chip: Use PDMS film to confine the ITO-PET interdigital electrode, and treat the electrode with oxygen plasma for 30s, then take 10μL of the single graphene oxide prepared in step 1, graphene oxide / Co 3 (HITP) 2 The graphene oxide and graphene oxide / PDDA material suspensions are respectively added dropwise into the electrode limit range and dried at room temperature. The electrodes with different materials added are placed in a reducing steam atmosphere at 70°C for reduction for 10-30 minutes to obtain the graphene oxide and graphene oxide / Co 3 (HITP) 2 , graphene oxide / PDDA gas sensor chip.
[0115] Embodiment 5:
[0116] The following is the graphene oxide / PDDA / Co prepared in Example 2 3 (HITP) 2 , and two composite gas sensor chips of graphene oxide / PDDA (prepared in Example 4), and the detection of nitric oxide gas at different humidity by graphene gas-sensitive materials before and after conductive MOF modification is compared and specifically described:
[0117] As an example, the graphene oxide / PDDA / Co prepared in Example 2 3 (HITP) 2 , and graphene oxide / PDDA composite gas sensor chips are used for nitric oxide gas detection under different humidity conditions: graphene oxide / PDDA / Co 3 (HITP) 2 Or the graphene oxide / PDDA composite gas sensor chip is placed in a gas flow cell. During the test, the carrier gas is first introduced until the baseline tends to be stable, and then dry nitric oxide gas or wet nitric oxide gas after different saturated salt solutions is introduced at the same flow rate. At a voltage of 1V, the current value flowing through the gas-sensitive material is tested by a picoammeter to obtain the data of the relationship between the current value and time. It can be seen that the graphene oxide / PDDA / Co 3 (HITP) 2 And the response value of graphene oxide / PDDA composite gas-sensitive material to nitric oxide gas under different humidity.
[0118] Graphene oxide / PDDA and graphene oxide / PDDA / Co 3 (HITP) 2 The results of the 200ppb concentration of nitric oxide standard gas response test at 0%, 23%, 56%, 75%, and 98% humidity are as follows: Figure 7 a. Figure 7 b. Taking humidity 0% as the relative base, the relative response changes of the above two materials to nitric oxide gas at different humidity are shown as follows Figure 8 As shown, Co 3 (HITP) 2 After surface modification, its response value increased by nearly one-fold, but the ratio of the response value relative to 0% under different humidity was less than 1.2, which was lower than that of graphene oxide / PDDA material, indicating that graphene oxide / PDDA / Co 3 (HITP) 2 The material's response value to nitric oxide gas in a wide humidity range of 0%-98% is relatively stable.
[0119] The present invention adopts conductive MOF to modify graphene to prepare gas-sensitive materials, introduces hydrophobic aromatic groups, and verifies its ability to reduce the influence of humidity factors on gas detection by comparing with graphene oxide / PDDA binary composite materials without adding MOF materials, thus providing a basis for the subsequent practical application of gas-sensitive materials.
[0120] Embodiment 6:
[0121] The following is the graphene oxide / PDDA / Co prepared in Example 2 3 (HITP) 2Gas sensor chip, specifically describes the detection and identification of exhaled gas by conductive MOF-modified graphene gas-sensitive materials at room temperature:
[0122] As an example, the graphene oxide / PDDA / Co prepared in Example 2 3 (HITP) 2 The gas sensor chip is used for detecting and identifying exhaled gas at room temperature, simulating the identification of chronic obstructive pulmonary disease (COPD) patients and healthy individuals: first, the exhaled gas of healthy individuals who are fasting or have been fed for more than 2 hours is collected in a ventilation environment into a 2L perfluoroethylene propylene copolymer (FEP) sampling bag, wherein the exhaled gas of chronic obstructive pulmonary disease (COPD) patients is simulated by introducing 25ppb standard nitric oxide gas into the exhaled gas of healthy individuals, and at the same time, the local environmental gas is collected into a 10L perfluoroethylene propylene copolymer (FEP) sampling bag as a carrier gas; when collecting gas, the gas is first passed through a 30cm Teflon hard tube with an inner diameter of 4mm immersed in an ice water bath, and the environmental gas and exhaled gas collection device such as Fig. 9 shown.
[0123] Among them, (a) is a schematic diagram of the exhaled gas collection device, and (b) is a schematic diagram of the environmental gas collection device, wherein 1 is human exhaled gas, 2 is a vital capacity mouthpiece, 3 is an ice water bath, 4 is a gas pipeline, 5 is a 2L perfluoroethylene propylene copolymer (FEP) gas sampling bag, 6 is environmental gas, 7 is a micro pump, and 8 is a 10L perfluoroethylene propylene copolymer (FEP) gas sampling bag.
[0124] The graphene oxide / PDDA / Co 3 (HITP) 2 The gas sensor chip was placed in a gas flow cell. During the test, the pre-treated ambient gas was first introduced until the baseline became stable, and then the pre-treated human exhaled gas was introduced at the same flow rate. At a voltage of 1 V, the picoammeter was used to measure the flow through the graphene oxide / PDDA / Co 3 (HITP) 2 The current value of the gas sensor chip was tested to obtain the data of the relationship between the current value and time. The difference analysis of the response value when different mixed gases (human exhaled breath) were introduced can be used to identify different mixed gases. The detection and identification results of the exhaled gases of 15 simulated chronic obstructive pulmonary disease (COPD) patients and 15 healthy individuals are as follows: Fig.10 shown.
[0125] The results showed that there were significant differences in the responses between the exhaled breath of healthy people and the exhaled breath of simulated chronic obstructive pulmonary disease (COPD) patients, and the response values of the two types of gases showed an obvious clustering effect, indicating that the material can detect and identify mixed gases, providing a feasibility basis for the subsequent use of gas-sensitive materials in actual disease samples.
[0126] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
Claims
1. A method for preparing a conductive MOF-modified gas-sensitive material, characterized in that: The following steps are involved: In the liquid phase, a polycation electrolyte and a negatively charged graphene oxide solution are initially assembled. After the initial assembly, a conductive metal organic framework material suspension having an equal volume to the graphene oxide solution is added, and the conductive MOF surface is modified by oscillation. The conductive metal organic framework material is a two-dimensional conductive metal organic framework material, including Co3(HITP)2, Ni3(HITP)2, Cu3(HITP)2, Co3(HHTP)2 or Cu3(HHTP)2, to obtain a conductive MOF modified gas-sensitive material, which is used to reduce the influence of humidity in the gas detection process, and includes a two-dimensional layered graphene assembly material and a conductive metal organic framework material modified on its surface.
2. The preparation method according to claim 1, characterized in that: The polycation electrolyte is polydiallyldimethylammonium chloride.
3. The preparation method according to claim 2, characterized in that: The molecular weight of the polydiallyldimethylammonium chloride is 200-350 KDa.
4. The preparation method according to claim 3, characterized in that: The initial assembly in the liquid phase includes: adding 10-60 μL of a 1 wt% polydiallyldimethylammonium chloride solution to 0.5 mL of a graphene oxide solution for initial assembly.
5. A gas sensor chip, characterized in that: The conductive MOF modified gas-sensitive material obtained by the preparation method of claim 1 is combined with an electrode.
6. The gas sensor chip according to claim 5, characterized in that: The substrate of the electrode is a flexible substrate or a hard substrate, the flexible substrate is a PET film, a PEN film, a PI film or a PC film; the hard substrate is silicon, glass, ceramic or a PCB board.
7. The method for preparing the gas sensor chip according to claim 5 or 6, comprising the following steps: Step 1, preparing the conductive MOF modified gas-sensitive material self-assembly suspension obtained in claim 1; Step 2: Use a PDMS film to confine the ITO-PET interdigital electrode and treat the electrode with oxygen plasma. Then, take the conductive MOF modified gas-sensitive material self-assembled suspension prepared in step 1 and drop it into the electrode confinement area and dry it at room temperature; place the dried electrode in a reducing vapor atmosphere for reduction to obtain the gas sensor chip.
8. Use of the gas sensor chip as claimed in claim 5 or 6 in gas detection.
9. The use according to claim 8, characterized in that: The gas detection is the detection and identification of different organic / inorganic gases and human exhaled breath.
10. The use according to claim 9, characterized in that: In the gas detection, the carrier gas used is the background gas of the sample gas; the sample gas is an organic or inorganic volatile gas.
11. The use according to claim 10, characterized in that: The sample gas is nitric oxide, nitrogen dioxide, hydrogen sulfide, ammonia, acetone, isoprene or water vapor.
12. The use according to any one of claims 8 to 11, characterized in that: The gas detection conditions satisfy at least one of the following: gas concentration of 0.1-10 ppm, room temperature, and different humidity of 0%-98%.
13. The use according to any one of claims 8 to 11, characterized in that: Gas-sensitive materials modified with Co3(HITP)2 surface were used to detect nitric oxide and nitrogen dioxide.