Method for synthesizing SAPO-34 molecular sieve by using catalytic cracking catalyst glue residues
Through high-temperature steam activation and hydrothermal crystallization of catalytic cracking catalyst slag, the problem of slag resource utilization has been successfully solved, the synthesis cost of SAPO-34 molecular sieve has been reduced, its crystallinity has been improved, and the efficient utilization of resources has been achieved.
Patent Information
- Application Number
- CN202310321920.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-29
AI Technical Summary
It is difficult to effectively utilize the slag in the production of catalytic cracking catalysts with existing technology, resulting in a waste of Si and Al resources, and the synthesis cost of SAPO-34 molecular sieve is high.
By performing high-temperature steam activation and secondary hydrothermal activation of the catalytic cracking catalyst slag, adding inorganic acid and silicon source, aluminum source, phosphorus source and template agent, hydrothermal crystallization is performed to prepare high crystallinity SAPO-34 Molecular sieves.
The use of slag to synthesize SAPO-34 molecular sieve is realized, which reduces the cost of raw materials, improves the uniformity and crystallinity of crystallized materials, and reduces the emission of impurity ions.
Smart Images

Figure HDA0004152071110000011 
Figure HDA0004152071110000012 
Figure HDA0004152071110000021
Abstract
Description
Technical Field
[0001] The invention relates to a method for synthesizing SAPO-34 molecular sieve by utilizing slag. Background Art
[0002] The production of catalytic cracking catalysts includes the steps of synthesis and modification of Y-type molecular sieves, gelling with modified Y-type molecular sieves and matrix components, spray drying, washing, roasting, etc. The synthesis, modification, washing, etc. of molecular sieves will produce wastewater, and the gelling and washing of catalysts will also produce wastewater. After sedimentation, filtration, slag cutting and other operations, waste slag with Al2O3 and SiO2 as the main components is obtained, which is called slag. Directly discarding the slag will cause a waste of resources such as Si and Al. If it is utilized by adopting an industrially feasible and cost-effective technical route, it can not only reduce the environmental protection management pressure of the enterprise, but also help to reduce the production cost of the enterprise and improve the economic benefits. However, the silicon and aluminum in these slags are different from the commonly used silicon and aluminum raw materials, and it is difficult to obtain satisfactory results by direct use.
[0003] SAPO-34 molecular sieve has a typical CHA topological structure, and its skeleton is mainly composed of PO 2+ 、AlO 2- , SiO2 tetrahedrons are connected to each other, and these skeleton atoms are periodically arranged and combined into six-membered rings, four-membered rings and eight-membered rings, eventually forming an ellipsoidal CHA cage structure and a three-dimensional cross-channel structure. SAPO-34 is actually formed by Si atoms replacing AlPO4 skeleton atoms, because in the AlPO4 skeleton, PO 2+ and AlO 2- The tetrahedrons carry positive and negative charges respectively, and the number of the two is equal, so the entire framework appears to be electrically neutral and the surface acidity is very weak. However, after the Si atom is introduced into its framework, the original charge balance is destroyed, making the molecular sieve as a whole appear to be negatively charged. There are also L acid centers and B acid centers on the surface of SAPO-34. Therefore, SAPO-34 has excellent hydrothermal stability, suitable surface acidity and pore structure.
[0004] At present, there are four main methods for synthesizing SAPO-34: hydrothermal synthesis, vapor phase crystallization, microwave synthesis, and ultrasonic synthesis. Among them, hydrothermal synthesis is the most widely used and mature method. Its main raw materials are silicon source, aluminum source, phosphorus source, template and deionized water; commonly used silicon sources include silica sol, active SiO2 and orthosilicate; aluminum sources include active alumina, pseudo-boehmite and aluminum isopropoxide; templates can be tetraethylammonium hydroxide (TEAOH), triethylamine, diethylamine and morpholine, etc.; phosphorus sources generally use orthophosphoric acid. However, the above synthetic raw materials are expensive because they are all chemical reagents, resulting in a high cost for the synthesis of SAPO-34. A large amount of silicon and aluminum sources in the slag are low in cost. If the silicon and aluminum sources in the slag can be used to synthesize SAPO-34, it will be of great significance for the green emission reduction of catalyst plants and the reduction of the cost of molecular sieve synthesis. However, the slag cannot be directly used to synthesize SAPO-34 molecular sieves. At present, there is no method for synthesizing SAPO-34 molecular sieves with high crystallinity using slag. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for synthesizing SAPO-34 molecular sieve by utilizing waste silicon and aluminum in catalytic cracking catalyst slag.
[0006] The present invention provides a method for using the residue produced by catalytic cracking catalyst (referred to as catalytic cracking catalyst residue, referred to as residue) to produce SAPO-34 molecular sieve, comprising the following steps:
[0007] (1) catalytic cracking catalyst residue is activated once by high-temperature steam to obtain a residue after primary activation;
[0008] (2) adding inorganic acid and water to the rubber residue after the primary activation to perform secondary hydrothermal activation to obtain a rubber residue slurry after the secondary activation;
[0009] (3) adding an aluminum source, an optional silicon source, a phosphorus source and a template agent to the slurry after secondary activation to prepare a mixed solution;
[0010] (4) After the mixed solution is stirred and aged at room temperature, the temperature is raised for hydrothermal crystallization to obtain a crystallized solution;
[0011] (5) The crystallization liquid is cooled, washed, filtered and dried to obtain SAPO-34 molecular sieve.
[0012] The used slag can be the discarded slag obtained by sedimentation, filtration and slag cutting of wastewater generated in the production of catalytic cracking catalyst.
[0013] According to the present invention, based on the dry weight of the slag, the slag contains 0-9 wt % of Na2O, 20-60 wt % of Al2O3, 20-60 wt % of SiO2, and 0-15 wt % of RE2O3.
[0014] In one embodiment, the catalytic cracking catalyst residue is a residue produced by molecular sieve modification, wherein the molecular sieve modification generally comprises treating the molecular sieve with water vapor and / or treating with gaseous silicon tetrachloride, washing and optional exchange, and the molecular sieve modified by the molecular sieve is, for example, a Y-type molecular sieve.
[0015] In one embodiment, the slag produced by the molecular sieve modification is slag produced by the Y-type molecular sieve modification.
[0016] Preferably, the slag produced by the molecular sieve modification has a relative crystallinity of less than 10% and / or a micropore specific surface area of less than 100 m 2 / g. The adverse effect on crystallinity can be prevented, so that the synthesized SAPO molecular sieve has a higher crystallinity.
[0017] The temperature of the high-temperature steam for one activation is 500-700° C., the activation time is 2-4 hours, and the steam is preferably 100% by volume steam.
[0018] According to the present invention, the inorganic acid in step (2) is one or more of phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid.
[0019] According to the present invention, the pH value of the mixture formed by adding inorganic acid to the slag after the primary activation is preferably 0.1-2, such as 0.5-2.0, the temperature of the secondary activation is preferably 80-120°C, such as 85-99°C, and the time of the secondary activation is preferably 1-24h, such as 5-15h.
[0020] The solid content of the slurry after the secondary activation is preferably 5 to 25% by weight.
[0021] The rubber residue after the primary activation can be slurried with water to form a slurry, and then an inorganic acid is added to perform a secondary activation.
[0022] According to the present invention, the molar ratio of Al2O3, H3PO4, SiO2, template and H2O in the mixed solution of step (3) is 1.0:1.5~2.5:0~1.5:1~5:30~100; wherein Al2O3 is the molar number of the aluminum element in the mixed solution converted into Al2O3, H3PO4 is the molar number of the phosphorus element in the mixed solution converted into H3PO4, and SiO2 is the molar number of the silicon element in the mixed solution converted into SiO2.
[0023] Preferably, H3PO4:Al2O3 is 1.8-2.2:1, SiO2:Al2O3 is 0.6-1.0:1, template:Al2O3 is 1.5-3.5:1, H2O:Al2O3 is 40-60:1; the ratios are molar ratios.
[0024] Preferably, the silicon and aluminum introduced into the slag as oxides account for 1 to 30 weight % such as 5 to 25 weight % of the total amount of phosphorus, silicon and aluminum in the mixed solution, wherein silicon is calculated as SiO2, aluminum is calculated as Al2O3 and phosphorus is calculated as P2O5.
[0025] According to the present invention, the supplementary silicon source in step (3) is one or more of silica sol, silica gel, and water glass; the supplementary aluminum source is one or more of pseudo-boehmite, boehmite, alumina, aluminum hydroxide, aluminum sol or soluble aluminum salt, preferably pseudo-boehmite; the supplementary phosphorus source is at least one of phosphoric acid, ammonium phosphate, phosphite or soluble metal phosphate; the phosphoric acid is preferably phosphoric acid with a mass fraction of 75-85%, and the phosphorus source can be supplemented by adding concentrated phosphoric acid with a phosphoric acid concentration of 75-85%;
[0026] The template agent is, for example, one or more of tetraethylammonium hydroxide, triethylamine, diethylamine or morpholine, preferably triethylamine.
[0027] According to the present invention, in step (4), the aging time is 0 to 20 hours, for example, 0.5 to 20 hours; preferably 8 to 15 hours, and the room temperature is 10 to 30°C; after the aging is completed, the heating rate to the hydrothermal crystallization temperature is preferably 2 to 5°C / min.
[0028] According to one embodiment of the present invention, the pH value of the aged product in step (4) is preferably 2-9.
[0029] According to the present invention, in one embodiment, the hydrothermal crystallization temperature is 150-250° C., and the time is 16-48 hours; preferably, the hydrothermal crystallization temperature is 160-220° C., and the time is 24-48 hours.
[0030] According to the present invention, after the hydrothermal crystallization is completed, the obtained crystallization liquid (or mixed colloid) is cooled, filtered and washed to obtain SAPO-34 molecular sieve. In one embodiment, the washing is: washing with water until the pH value of the washed water is 7-8.
[0031] The present invention can synthesize SAPO-34 molecular sieve by using the above technical scheme. The SAPO-34 molecular sieve synthesized by the method of the present invention has high crystallinity.
[0032] The method provided by the present invention utilizes the slag as part of the silicon source and the aluminum source, and can reduce the raw material cost of SAPO-34 synthesis. In addition, the present invention can remove part of the anions in the slag while activating the silicon and aluminum sources in the slag through a high-temperature roasting hydrothermal treatment, and then use inorganic acid, especially phosphoric acid, for hydrothermal secondary activation, which can effectively activate the silicon and aluminum sources and also serve as a synthetic raw material, and can reduce the emission of impurity ions as much as possible while efficiently utilizing the silicon and aluminum in the slag, and can have a higher slag usage, and improve the uniformity of the crystallized material.
[0033] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 , XRD pattern of the product of Example 1
[0035] Figure 2 , SEM image of the product of Example 1
[0036] Figure 3 , SEM image of the product of comparative example 1
[0037] Figure 4 , XRD pattern of the product of comparative example 1 DETAILED DESCRIPTION
[0038] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.
[0039] The slag used in the embodiment is obtained by sedimentation, filtration and slag cutting of waste water generated in the production of catalytic cracking catalyst, wherein:
[0040] The solid content of the slag 1# is 80 wt%. Based on the dry weight of the slag, it contains 0.17 wt% Na2O, 49 wt% Al2O3, 43.9 wt% SiO2, and 3.18 wt% RE2O3; the relative crystallinity of the Y-type molecular sieve is 5%, and the micropore specific surface area is 47m 2 / g molecular sieve hydrothermal modification process residue provided by Sinopec Catalyst Co., Ltd. Qilu Branch;
[0041] The solid content of the slag 2# is 80 wt%. Based on the dry weight of the slag, it contains 2.7 wt% Na2O, 58.5 wt% Al2O3, 28.9 wt% SiO2, 6.71 wt% RE2O 3, The relative crystallinity of Y-type molecular sieve is 3%, and the micropore specific surface area is 26m 2 / g; molecular sieve hydrothermal modification process residue provided by Sinopec Catalyst Co., Ltd. Qilu Branch;
[0042] The solid content of the slag 3# is 80 wt%. Based on the dry weight of the slag, it contains 5.82 wt% Na2O, 31.6 wt% Al2O3, 54.7 wt% SiO2, 4.90 wt% RE2O 3, The relative crystallinity of Y-type molecular sieve is 8%, and the micropore specific surface area is 74m 2 / g; molecular sieve gas phase ultra-stable modification process slag provided by Sinopec Catalyst Co., Ltd. Qilu Branch.
[0043] Pseudo-boehmite was produced by Shandong Aluminum Plant and had a solid content of 62.0 wt %;
[0044] The aluminum sol has an aluminum oxide content of 21.5% by weight and is produced by the Qilu Branch of Sinopec Catalyst Co., Ltd.
[0045] Phosphoric acid was produced by Beijing Chemical Plant with analytical grade and mass concentration of 85%;
[0046] Sulfuric acid, produced by Beijing Chemical Plant, of analytical grade, with a mass concentration of 98%;
[0047] Hydrochloric acid, produced by Beijing Chemical Plant, of analytical grade, with a mass concentration of 36%;
[0048] The composition of the samples was determined by X-ray fluorescence spectroscopy (XRF);
[0049] The relative crystallinity of the samples was determined by X-ray powder diffraction (XRD) method:
[0050] SAPO-34 molecular sieve standard sample, produced by Sinopec Catalyst Co., Ltd. Nanjing Branch,
[0051] Analysis method for relative crystallinity of SAPO-34 molecular sieve: Taking the crystallinity of the standard sample as 100%, selecting the diffraction peaks at 2θ=9.6° and 20.8° in the XRD spectrum to fit the peak area, and obtaining the relative crystallinity of the sample by the ratio of the sum of the peak areas of the two diffraction peaks of the synthetic sample to the sum of the two corresponding peak areas of the standard sample;
[0052] The crystallinity of the residue Y-type molecular sieve was analyzed by Q / SH 361 711-2017 method.
[0053] Preparation Example 1
[0054] Example 1
[0055] (1) 12.46 g of residue 1# was activated by passing 100% by volume steam at 550°C for 3 h.
[0056] (2) slurrying the activated residue in 89.33 g of deionized water, adding 15 g of phosphoric acid, with a pH value of 1.9, and hydrothermally activating at 90° C. for 8 h to obtain a secondary activated residue slurry;
[0057] (3) adding 7.18 g of pseudo-boehmite, 11.84 g of phosphoric acid and 14.19 g of ethylenediamine to the above-mentioned secondary activated residue slurry to prepare a mixed solution;
[0058] (4) After the mixed solution was aged at 30° C. for 8 h, the temperature was raised for hydrothermal crystallization at a heating rate of 5° C. / min. After the temperature was raised to 170° C., crystallization was carried out for 28 h to obtain a crystallized solution;
[0059] (5) The crystallization liquid is cooled, washed, filtered and dried to obtain SAPO-34 molecular sieve.
[0060] Example 2
[0061] (1) 10.56 g of the residue 1# was activated by passing 100% by volume steam at 650°C for 3 h.
[0062] (2) the rubber residue after primary activation was slurried in 86.72 g of deionized water, 2 g of hydrochloric acid and 20 g of phosphoric acid were added, the pH value was 0.8, and hydrothermal activation was performed at 90° C. for 8 h to obtain a slurry of rubber residue after secondary activation;
[0063] (3) adding 7.74 g of pseudo-boehmite, 6 g of phosphoric acid and 18.98 g of triethylamine to the above-mentioned secondary activated residue slurry to prepare a mixed solution;
[0064] (4) After the mixed solution was aged at room temperature (30° C., the same below) for 10 h, the temperature was raised for hydrothermal crystallization at a heating rate of 2° C. / min to 170° C., and crystallization was performed for 32 h to obtain a crystallized solution;
[0065] (5) The crystallization liquid is cooled, washed, filtered and dried to obtain SAPO-34 molecular sieve.
[0066] Example 3
[0067] (1) 13.06 g of slag 1# was activated by passing 100 vol% steam at 600° C. for 3 h;
[0068] (2) the activated residue was slurried in 96.31 g of deionized water, 2 g of sulfuric acid and 15 g of phosphoric acid were added, the pH value was 0.8, and hydrothermal activation was performed at 90° C. for 8 h to obtain a dispersion of the residue after secondary activation;
[0069] (3) adding 7.56 g of pseudo-boehmite, 6.09 g of phosphoric acid and 12.01 g of isopropylamine to the above-mentioned secondary activated residue dispersion to prepare a mixed solution;
[0070] (4) After the mixed solution was aged at room temperature for 8 hours, the temperature was raised for hydrothermal crystallization at a heating rate of 3°C / min to 190°C and then crystallized for 24 hours to obtain a crystallized solution;
[0071] (5) The crystallization liquid is cooled, washed, filtered and dried to obtain SAPO-34 molecular sieve.
[0072] Example 4
[0073] (1) 21.1 g of the residue 2# was activated by passing 100% by volume steam at 600° C. for 3 h;
[0074] (2) the rubber residue after primary activation was slurried in 95.12 g of deionized water, 2 g of sulfuric acid and 15 g of phosphoric acid were added, the pH value was 1.2, and hydrothermal activation was performed at 90° C. for 8 h to obtain a dispersion of the rubber residue after secondary activation;
[0075] (3) adding 0.68 g of pseudo-boehmite, 6.09 g of phosphoric acid and 12.01 g of isopropylamine to the above-mentioned secondary activated residue dispersion to prepare a mixed solution;
[0076] (4) After the mixed solution was aged at room temperature for 8 hours, the temperature was raised for hydrothermal crystallization at a heating rate of 3°C / min to 190°C and then crystallized for 24 hours to obtain a crystallized solution;
[0077] (5) The crystallization liquid is cooled, washed, filtered and dried to obtain SAPO-34 molecular sieve.
[0078] Example 5
[0079] (1) 11.15 g of the residue 3# was activated by passing 100% by volume of water vapor at 600° C. for 3 h to obtain the residue after primary activation;
[0080] (2) the rubber residue after primary activation was slurried in 95.36 g of deionized water, 2 g of sulfuric acid and 15 g of phosphoric acid were added, the pH value was 0.9, and hydrothermal activation was performed at 90° C. for 8 h to obtain a dispersion of the rubber residue after secondary activation;
[0081] (3) adding 10.39 g of pseudo-boehmite, 6.09 g of phosphoric acid and 12.01 g of isopropylamine to the above-mentioned secondary activated residue dispersion to prepare a mixed solution;
[0082] (4) After the mixed solution is aged at room temperature for 8 hours, the temperature is raised for hydrothermal crystallization at a heating rate of 3° C. / min to 190° C. and then crystallized for 24 hours to obtain a crystallized solution;
[0083] (5) The crystallization liquid is cooled, washed, filtered and dried to obtain SAPO-34 molecular sieve.
[0084] Comparative Example 1
[0085] (1) 12.46 g of the residue 1# was added to 91.83 g of deionized water and beaten for 3 h to obtain a residue slurry;
[0086] (2) Add 7.18 g of pseudo-boehmite, 26.84 g of phosphoric acid and 14.19 g of ethylenediamine to the above-mentioned slurry to prepare a mixed solution.
[0087] (3) After the mixed solution was aged at room temperature for 8 hours, the temperature was raised for hydrothermal crystallization at a heating rate of 5°C / min to 170°C and then crystallized for 28 hours to obtain a crystallized solution.
[0088] (4) The crystallized liquid is cooled, washed, filtered and dried to obtain DB-1.
[0089] Comparative Example 2
[0090] 21.1 g of the residue 2# was calcined at 800°C for 3h to obtain an activated residue. The aluminum source, phosphorus source and template agent were added according to the ratio of Example 4, and the residue was aged and crystallized. After cooling, washing, filtering and drying, the product DB-2 was obtained.
[0091] Comparative Example 3
[0092] 11.15g of slag 3# and sodium hydroxide were mixed evenly at a mass ratio of 1:1.1, and calcined at 700°C for 3h to obtain activated slag, which was washed with deionized water. The product contained 5.5 wt% Na2O, 32.9 wt% Al2O3, 55.7 wt% SiO2, and 5.2 wt% RE2O3. Phosphorus source and aluminum source were supplemented according to the ratio of Example 5, template agent was added, and after aging and crystallization, cooling, washing, filtering, and drying, DB-3 was obtained.
[0093] The properties of the samples of the above examples and comparative examples are shown in Table 1.
[0094] Table 1 Crystallinity analysis of samples
[0095] Sample source Relative crystallinity, % Example 1 89.5 Example 2 84.3 Example 3 85.1 Example 4 86.7 Example 5 84.9 Comparative Example 1 12.1 Comparative Example 2 13.4 Comparative Example 3 14.9
[0096] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0097] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0098] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for synthesizing SAPO-34 molecular sieve using residue produced by catalytic cracking catalyst production, comprising the following steps: (1) subjecting the adhesive residue to a primary activation with high-temperature steam to obtain an activated adhesive residue; (2) adding an inorganic acid to the rubber residue after the primary activation to perform a secondary hydrothermal activation to obtain a rubber residue slurry after the secondary activation; (3) adding an aluminum source, an optional silicon source, a phosphorus source and a template agent to the slurry after secondary activation to obtain a mixed solution; (4) After the mixed solution is stirred and aged at room temperature, the temperature is raised for hydrothermal crystallization to obtain a crystallized solution; (5) The crystallized liquid is cooled, washed, filtered and dried.
2. The method according to claim 1, characterized in that Based on the dry weight of the slag, the slag contains 0-9 wt% Na2O, 20-60 wt% Al2O3, 20-60 wt% SiO2, and 0-15 wt% RE2O3. Preferably, the slag Y-type molecular sieve has a relative crystallinity of less than 10% and / or a micropore specific surface area of less than 100 m 2 / g; In one embodiment, the catalytic cracking catalyst residue is a molecular sieve modified residue, and the molecular sieve modification includes steam treatment and / or treatment with gas phase silicon tetrachloride, washing and optional exchange.
3. The method according to claim 1, characterized in that The temperature of the high-temperature steam for one activation is 500-700° C., the activation time is 2-4 hours, and the steam is 100% by volume steam.
4. The method according to claim 1, characterized in that The inorganic acid in step (2) is one or a mixture of phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid.
5. According to claim 1, it is characterized in that: The pH value of the mixture formed by adding inorganic acid to the slurry after the primary activation is 0.1-2, the temperature of the secondary activation is 80-120° C., and the time is 1-24 hours; the solid content of the slurry after the secondary activation is preferably 5-25% by weight.
6. The method according to claim 1, characterized in that The molar ratio of Al2O3, H3PO4, SiO2, template and H2O in the mixed solution of step (3) is 1:1.5-2.5:0-1.5:1-5:30-100; wherein Al2O3 is the molar number of the aluminum element in the mixed solution converted into Al2O3, H3PO4 is the molar number of the phosphorus element in the mixed solution converted into H3PO4, and SiO2 is the molar number of the silicon element in the mixed solution converted into SiO2. Preferably, H3PO4:Al2O3 is 1.8-2.2:1, SiO2:Al2O3 is 0.6-1.0:1, template:Al2O3 is 1.5-3.5:1, H2O:Al2O3 is 40-60:1; the ratios are molar ratios; Preferably, the silicon and aluminum introduced by the slag account for 1 to 30 weight % of the total amount of phosphorus, silicon and aluminum in the mixed solution, calculated as oxides, wherein silicon is calculated as SiO2, aluminum is calculated as Al2O3, and phosphorus is calculated as P2O5.
7. The method according to claim 1, characterized in that The silicon source in step (3) is one or more of silica sol, silica gel, and water glass; The aluminum source in step (3) is one or more of pseudo-boehmite, boehmite, alumina, aluminum hydroxide, aluminum sol or soluble aluminum salt, preferably pseudo-boehmite; The phosphorus source in step (3) is at least one of phosphoric acid, ammonium phosphate, phosphite or soluble metal phosphate; the phosphorus source is, for example, phosphoric acid with a mass fraction of 75-85%; The template agent is one or more of tetraethylammonium hydroxide, triethylamine, diethylamine or morpholine, preferably triethylamine.
8. The method according to claim 1, characterized in that In step (4), the aging time is 0 to 20 hours, preferably 8 to 15 hours; the room temperature is 10 to 30°C; after the aging is completed, the heating rate to the hydrothermal crystallization temperature is preferably 2 to 5°C / min.
9. The method according to claim 1, characterized in that: The pH value of the aged product in step (4) is 2-9.
10. The method according to claim 1 or 7, characterized in that: The temperature of hydrothermal crystallization is 150-250°C and the time is 16-48h; Preferably, the temperature of the hydrothermal crystallization is 160-220° C., and the time of the hydrothermal crystallization is 24-48 hours.
11. The method according to claim 1, characterized in that: After the hydrothermal crystallization is completed, the obtained crystallization liquid (mixed colloid) is cooled, filtered and washed to obtain SAPO-34 molecular sieve. In one embodiment, the washing is: washing with water until the pH value of the washed water is 7-8.
Citation Information
Patent Citations
Method for preparing SAPO-34 molecular sieve by using crystallized residual liquid of SAPO-34 molecular sieve
CN101555021A
Preparation method of ZSM-5 molecular sieve
CN102442686A
Efficient utilization method for fluidized catalytic cracking (FCC) catalyst glue refuse
CN104261425A
Catalytic cracking catalyst as well as preparation method and application thereof
CN114425398A
Nano Y-type molecular sieve taking glue residue as raw material as well as preparation method and application of nano Y-type molecular sieve
CN114620740A
Cited By
Method for preparing A-type molecular sieve from FCC (fluid catalytic cracking) catalyst waste rubber residues
CN119750605A