Preparation method and application of oxygen-enriched defect NaV8O20.nH2O aqueous zinc ion battery positive electrode material
By introducing oxygen vacancy defects into vanadium-based oxides and performing heat treatment, an oxygen-rich defective NaV8O20·nH2O aqueous zinc ion battery cathode material was prepared, which solved the problems of structural instability and poor conductivity of vanadium-based oxides during the charge and discharge process. It achieves high structural stability and charge-discharge specific capacity, and improves the rate and cycle performance of zinc-ion batteries.
Patent Information
- Application Number
- CN202410700046.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-01
AI Technical Summary
Existing vanadium-based oxide aqueous zinc-ion battery cathode materials have unstable structures, low ion diffusion coefficients, and poor conductivity during the charge and discharge process, resulting in limited practical applications. Single cation pre-embedding or oxygen vacancy defect designs are difficult to achieve ideal electrochemical performance. , especially in terms of zinc storage capacity and rate performance.
The preparation method of the oxygen-deficient NaV8O20·nH2O aqueous zinc-ion battery cathode material is adopted. The vanadium pentoxide powder is hydrothermally reacted in deionized water, and disodium ethylenediaminetetraacetate is added to introduce oxygen vacancy defects, followed by heat treatment. , adjust the layer spacing of the material and the valence state of vanadium, and improve the electrochemical performance.
The prepared oxygen-rich defect NaV8O20·nH2O material has high structural stability and charge-discharge specific capacity, shows good rate and cycle performance, and improves the electrochemical performance of zinc-ion batteries.
Smart Images

Figure BDA0004870792140000071 
Figure HDA0004870792150000011 
Figure HDA0004870792150000012
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of preparation of aqueous zinc ion positive electrode materials, in particular to an oxygen-rich defective NaV8O 20 Preparation method and application of nH2O aqueous zinc ion battery cathode material. Background Art
[0002] Aqueous zinc-ion batteries have attracted more and more attention due to their low cost and abundant positive electrode materials. Aqueous zinc-ion batteries are an ideal choice for large-scale energy storage applications. The positive electrode materials of zinc-ion batteries play a decisive role in the cost, safety, and cycle life of the battery. At present, the positive electrode materials of aqueous zinc-ion batteries widely favored by researchers mainly include: manganese-based oxides, vanadium oxides, Prussian blue homologues and other special materials. Among them, vanadium-based oxides are an ideal positive electrode energy storage material for zinc-ion batteries because of their high theoretical specific capacity, abundant resources, good safety, high energy density and environmental friendliness.
[0003] Vanadium pentoxide has the advantages of low cost, easy preparation, abundant sources, and good safety performance. It is a very promising cathode material for the next generation of zinc-ion batteries. However, its practical application is limited by its poor cycle stability, low ion diffusion coefficient, and poor conductivity. In order to improve the V2O5 during the charge and discharge process due to Zn 2+ In order to improve the zinc ion storage performance by reducing the structural instability caused by ion deintercalation, many modification studies have been conducted, including the composite of conductive materials, the preparation of amorphous V2O5, the introduction of water molecules and guest ions, and the synthesis of mixed-valence vanadium oxides.
[0004] As an important alkali metal, Na + Has a larger ionic radius and smaller mass. + Pre-embedding can improve the structural stability of vanadium oxide, improve its conductivity and electrochemical properties, and realize Zn 2 + Rapid and reversible insertion / extraction reaction. +It can act as a "pillar" to maintain the main structure during the zinc ion insertion and extraction process, and can increase the ion diffusion rate and electronic conductivity. However, cation pre-embedding often has a mass effect that is prone to partial capacity loss, and cation pre-embedded vanadium oxide is usually only stable when the capacity retention rate is about 50% of the theoretical capacity (about 250mAhg-1). Therefore, it is difficult to obtain vanadium-based aqueous zinc-ion battery positive electrode materials with ideal electrochemical properties through a single defect design method of cation pre-embedding, especially in terms of zinc storage capacity and rate performance. In addition, the oxygen vacancy defect design demonstrates its high efficiency and superiority in improving the electrochemical performance of vanadium oxide, especially the zinc storage capacity. The oxygen vacancy defects in the structure of vanadium-based materials are beneficial to increase its electronic conductivity and improve Zn 2+ Reversible insertion / extraction ion diffusion kinetics and enhanced pseudocapacitance effect of materials. At present, there are many studies on improving the performance of vanadium oxides through single cation pre-embedding strategy or oxygen vacancy defect design, but there are very few studies on the synergistic interaction between the two. Du et al. (Oxygen-vacancy and phosphate coordination triggered strain engineering of vanadium oxide for high-performance aqueous zinc ion storage."Nano Energy 89(2021):106477) synthesized (Na,Mn)V8O 20 nH2O material, further introduced oxygen vacancies on the surface of the material through chemical treatment, and studied the zinc storage performance of the material; however, there are problems in this study such as cumbersome preparation method and low specific capacity. Summary of the invention
[0005] In view of the above shortcomings, the present invention provides an oxygen-rich defective NaV8O 20 · Preparation method of nH2O aqueous zinc ion battery positive electrode material, the preparation process is simple, the prepared oxygen-rich defect NaV8O 20 nH2O aqueous zinc ion battery cathode material has the advantages of high structural stability and charge-discharge specific capacity. The specific technical solution is as follows:
[0006] An oxygen-rich defect NaV8O 20 A method for preparing a positive electrode material for an nH2O aqueous zinc ion battery comprises the following steps:
[0007] (1) dispersing vanadium pentoxide powder in deionized water, adding hydrogen peroxide dropwise and stirring; then adding deionized water solution of disodium ethylenediaminetetraacetic acid to obtain a mixed solution;
[0008] (2) subjecting the mixed solution to a hydrothermal reaction at 140 to 180° C. for 10 to 20 hours; after the reaction, centrifugation and freeze drying are performed to obtain a primary product;
[0009] (3) The primary product obtained in step (2) is heat treated at 180-220° C. for 0.5-2 h to obtain oxygen-rich defective NaV8O 20 nH2O material.
[0010] Preferably, the above oxygen-rich defect NaV8O 20 · A method for preparing a positive electrode material for an nH2O aqueous zinc ion battery, wherein in step (1), the ratio of vanadium pentoxide powder, deionized water, and hydrogen peroxide is 1 g: 17.26 ml: 4.64 ml.
[0011] Preferably, the above oxygen-rich defect NaV8O 20 · A method for preparing a positive electrode material for an nH2O aqueous zinc ion battery, wherein the molar ratio of disodium ethylenediaminetetraacetate to vanadium pentoxide is 0.05 to 0.35:1.
[0012] Preferably, the above oxygen-rich defect NaV8O 20 · A method for preparing a positive electrode material for an nH2O aqueous zinc ion battery, wherein the molar ratio of disodium ethylenediaminetetraacetate to vanadium pentoxide is 0.25:1.
[0013] Preferably, the above oxygen-rich defect NaV8O 20 · A method for preparing a positive electrode material for an nH2O aqueous zinc ion battery, wherein in step (2), a hydrothermal reaction is carried out at 160°C for 12 hours; and in step (3), a heat treatment is carried out at 200°C for 1 hour.
[0014] An oxygen-rich defect NaV8O 20 nH2O aqueous zinc ion battery positive electrode material, composed of the above-mentioned oxygen-rich defect NaV8O 20 The nH2O aqueous zinc ion battery positive electrode material is prepared by the preparation method.
[0015] The above oxygen-rich defect NaV8O 20 Application of nH2O aqueous zinc ion battery cathode material in aqueous zinc ion batteries.
[0016] Preferably, in the above application, the aqueous zinc ion battery comprises the oxygen-rich defect NaV8O 20 The electrode sheet is prepared from nH2O material, and the preparation method of the electrode sheet comprises: 20 nH2O material, conductive agent and binder are mixed with solvent, then coated on the current collector and dried to obtain an electrode sheet.
[0017] Preferably, in the above application, the conductive agent is Super P, the binder is polyvinylidene fluoride, NaV8O 20 The mass ratio of nH2O material, conductive agent and binder is 7:2:1, the current collector is a stainless steel mesh, and the solvent is N-methyl-2-pyrrolidone.
[0018] Preferably, in the above application, the electrode sheet, the counter electrode, the separator and the ZnSO4 electrolyte are assembled into a battery.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. Oxygen-rich defect NaV8O of the present invention 20 The preparation method of nH2O aqueous zinc ion battery positive electrode material has simple preparation process and mild reaction conditions. The prepared oxygen-rich defect NaV8O 20 As the positive electrode material of aqueous zinc-ion batteries, nH2O material has high structural stability and charge-discharge specific capacity, and exhibits good rate and cycle performance.
[0021] 2. Oxygen-rich defect NaV8O of the present invention 20 In the preparation method of the positive electrode material of nH2O aqueous zinc ion battery, disodium ethylenediaminetetraacetate is used as the sodium source. The ethylenediaminetetraacetic acid ion in disodium ethylenediaminetetraacetate has a carbon-carbon double bond and has weak reducibility, which can realize the embedding of sodium ions in vanadium oxide and the generation of oxygen vacancy defects. The subsequent heat treatment can adjust the interlayer spacing and valence state of vanadium in the material, thereby further improving the NaV8O 20 ·Electrical properties of nH2O aqueous zinc-ion battery cathode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0023] Figure 1 NaV8O prepared in Examples 1 to 4 and Comparative Example 1 20 XRD pattern of nH2O cathode material.
[0024] Figure 2 The oxygen-rich NaV8O prepared in Example 3 20 SEM image of nH2O cathode material.
[0025] Figure 3 NaV8O prepared in Example 3 and Comparative Example 1 20XPS spectrum of nH2O cathode material.
[0026] Figure 4 NaV8O prepared in Example 3 and Comparative Example 1 20 EPR diagram of nH2O cathode material.
[0027] Figure 5 NaV8O prepared in Examples 1 to 4 and Comparative Example 1 20 ·Characterization diagram of the cycling performance of nH2O cathode material.
[0028] Figure 6 NaV8O prepared in Examples 1 to 4 and Comparative Example 1 20 Battery rate performance diagram of nH2O cathode material. DETAILED DESCRIPTION
[0029] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the protection scope of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the present invention, etc. can be purchased from the market or can be prepared by existing methods.
[0030] Example 1
[0031] An oxygen-rich defect NaV8O 20 A method for preparing a positive electrode material for an nH2O aqueous zinc ion battery comprises the following steps:
[0032] (1) 0.248 g of vanadium pentoxide powder was dispersed in 4.28 ml of deionized water, and 1.15 ml of hydrogen peroxide was added dropwise and stirred for 20 min; then 45 ml of disodium ethylenediaminetetraacetic acid deionized water solution was added and stirred for 30 min. The molar ratio of disodium ethylenediaminetetraacetic acid to vanadium pentoxide was 0.05:1 (Na + :V molar ratio is 5%) to obtain a mixed solution;
[0033] (2) transferring the mixed solution to a high pressure reactor and subjecting it to a hydrothermal reaction at 160° C. for 12 h; after the reaction, centrifugally freeze-drying the mixture to obtain a primary product;
[0034] (3) The primary product obtained in step (2) was heat treated at 200°C for 1 h to obtain oxygen-rich defect NaV8O 20 nH2O material.
[0035] The prepared oxygen-rich defect NaV8O 20nH2O material for sample electrode preparation and half-cell assembly: oxygen-rich defect NaV8O 20 nH2O material, conductive agent Super P and binder PVDF were mixed in a ratio of 7:2:1, and an appropriate amount of organic solvent N-methyl-2-pyrrolidone was added to grind evenly, and then evenly coated on a stainless steel mesh and vacuum dried to prepare an electrode sheet. The electrode sheet, counter electrode (zinc sheet), diaphragm (glass fiber porous membrane) and 2.5 mol / L ZnSO4 electrolyte were assembled into a button cell.
[0036] Example 2
[0037] An oxygen-rich defect NaV8O 20 A method for preparing a positive electrode material for an nH2O aqueous zinc ion battery comprises the following steps:
[0038] (1) 0.248 g of vanadium pentoxide powder was dispersed in 4.28 ml of deionized water, and 1.15 ml of hydrogen peroxide was added dropwise and stirred for 20 min; then 45 ml of disodium ethylenediaminetetraacetic acid deionized water solution was added and stirred for 30 min. The molar ratio of disodium ethylenediaminetetraacetic acid to vanadium pentoxide was 0.15:1 (Na + :V molar ratio is 15%) to obtain a mixed solution;
[0039] (2) transferring the mixed solution to a high pressure reactor and subjecting it to a hydrothermal reaction at 160° C. for 12 h; after the reaction, centrifugally freeze-drying the mixture to obtain a primary product;
[0040] (3) The primary product obtained in step (2) was heat treated at 200°C for 1 h to obtain oxygen-rich defect NaV8O 20 nH2O material.
[0041] The prepared oxygen-rich defect NaV8O 20 nH2O material for sample electrode preparation and half-cell assembly: oxygen-rich defect NaV8O 20 nH2O material, conductive agent Super P and binder PVDF were mixed in a ratio of 7:2:1, and an appropriate amount of organic solvent N-methyl-2-pyrrolidone was added to grind evenly, and then evenly coated on a stainless steel mesh and vacuum dried to prepare an electrode sheet. The electrode sheet, counter electrode (zinc sheet), diaphragm (glass fiber porous membrane) and 2.5 mol / L ZnSO4 electrolyte were assembled into a button cell.
[0042] Example 3
[0043] An oxygen-rich defect NaV8O 20 A method for preparing a positive electrode material for an nH2O aqueous zinc ion battery comprises the following steps:
[0044] (1) 0.248 g of vanadium pentoxide powder was dispersed in 4.28 ml of deionized water, and 1.15 ml of hydrogen peroxide was added dropwise and stirred for 20 min; then 45 ml of disodium ethylenediaminetetraacetic acid deionized water solution was added and stirred for 30 min. The molar ratio of disodium ethylenediaminetetraacetic acid to vanadium pentoxide was 0.25:1 (Na + :V molar ratio is 25%) to obtain a mixed solution;
[0045] (2) transferring the mixed solution to a high pressure reactor and subjecting it to a hydrothermal reaction at 160° C. for 12 h; after the reaction, centrifugally freeze-drying the mixture to obtain a primary product;
[0046] (3) The primary product obtained in step (2) was heat treated at 200°C for 1 h to obtain oxygen-rich defect NaV8O 20 nH2O material.
[0047] The prepared oxygen-rich defect NaV8O 20 nH2O material for sample electrode preparation and half-cell assembly: oxygen-rich defect NaV8O 20 nH2O material, conductive agent Super P and binder PVDF were mixed in a ratio of 7:2:1, and an appropriate amount of organic solvent N-methyl-2-pyrrolidone was added to grind evenly, and then evenly coated on a stainless steel mesh and vacuum dried to prepare an electrode sheet. The electrode sheet, counter electrode (zinc sheet), diaphragm (glass fiber porous membrane) and 2.5 mol / L ZnSO4 electrolyte were assembled into a button cell.
[0048] Example 4
[0049] An oxygen-rich defect NaV8O 20 A method for preparing a positive electrode material for an nH2O aqueous zinc ion battery comprises the following steps:
[0050] (1) 0.248 g of vanadium pentoxide powder was dispersed in 4.28 ml of deionized water, and 1.15 ml of hydrogen peroxide was added dropwise and stirred for 20 min; then 45 ml of disodium ethylenediaminetetraacetic acid deionized water solution was added and stirred for 30 min. The molar ratio of disodium ethylenediaminetetraacetic acid to vanadium pentoxide was 0.35:1 (Na + :V molar ratio is 35%) to obtain a mixed solution;
[0051] (2) transferring the mixed solution to a high pressure reactor and subjecting it to a hydrothermal reaction at 160° C. for 12 h; after the reaction, centrifugally freeze-drying the mixture to obtain a primary product;
[0052] (3) The primary product obtained in step (2) was heat treated at 200°C for 1 h to obtain oxygen-rich defect NaV8O 20 nH2O material.
[0053] The prepared oxygen-rich defect NaV8O 20 nH2O material for sample electrode preparation and half-cell assembly: oxygen-rich defect NaV8O 20 nH2O material, conductive agent Super P and binder PVDF were mixed in a ratio of 7:2:1, and an appropriate amount of organic solvent N-methyl-2-pyrrolidone was added to grind evenly, and then evenly coated on a stainless steel mesh and vacuum dried to prepare an electrode sheet. The electrode sheet, counter electrode (zinc sheet), diaphragm (glass fiber porous membrane) and 2.5 mol / L ZnSO4 electrolyte were assembled into a button cell.
[0054] Comparative Example 1
[0055] A NaV8O 20 A method for preparing a positive electrode material for an nH2O aqueous zinc ion battery comprises the following steps:
[0056] (1) Disperse 0.248 g of vanadium pentoxide powder in 4.28 ml of deionized water, add 1.15 ml of hydrogen peroxide and stir for 20 min; then add 45 ml of sodium chloride aqueous solution and continue stirring for 30 min. The molar ratio of sodium chloride to vanadium pentoxide is 0.5:1 (Na + :V molar ratio is 25%) to obtain a mixed solution;
[0057] (2) transferring the mixed solution to a high pressure reactor and subjecting it to a hydrothermal reaction at 160° C. for 12 h; after the reaction, centrifugally freeze-drying the mixture to obtain a primary product;
[0058] (3) The initial product obtained in step (2) was heat treated at 200°C for 1 h to obtain NaV8O 20 nH2O material.
[0059] The prepared oxygen-rich defect NaV8O 20 nH2O material for sample electrode preparation and half-cell assembly: NaV8O 20 nH2O material, conductive agent Super P and binder PVDF were mixed in a ratio of 7:2:1, and an appropriate amount of organic solvent N-methyl-2-pyrrolidone was added to grind evenly, and then evenly coated on a stainless steel mesh and vacuum dried to prepare an electrode sheet. The electrode sheet, counter electrode (zinc sheet), diaphragm (glass fiber porous membrane) and 2.5 mol / L ZnSO4 electrolyte were assembled into a button cell.
[0060] Comparative Example 2
[0061] An oxygen-rich defect NaV8O 20 A method for preparing a positive electrode material for an nH2O aqueous zinc ion battery comprises the following steps:
[0062] (1) 0.248 g of vanadium pentoxide powder was dispersed in 4.28 ml of deionized water, and 1.15 ml of hydrogen peroxide was added dropwise and stirred for 20 min; then 45 ml of disodium ethylenediaminetetraacetic acid deionized water solution was added and stirred for 30 min. The molar ratio of disodium ethylenediaminetetraacetic acid to vanadium pentoxide was 0.25:1 (Na + :V molar ratio is 25%) to obtain a mixed solution;
[0063] (2) The mixed solution was transferred to a high pressure reactor and subjected to a hydrothermal reaction at 160°C for 12 h. After the reaction, the mixture was centrifuged and freeze-dried to obtain NaV8O 20 nH2O material.
[0064] The prepared NaV8O 20 nH2O material for sample electrode preparation and half-cell assembly: oxygen-rich defect NaV8O 20 nH2O material, conductive agent Super P and binder PVDF were mixed in a ratio of 7:2:1, and an appropriate amount of organic solvent N-methyl-2-pyrrolidone was added to grind evenly, and then evenly coated on a stainless steel mesh and vacuum dried to prepare an electrode sheet. The electrode sheet, counter electrode (zinc sheet), diaphragm (glass fiber porous membrane) and 2.5 mol / L ZnSO4 electrolyte were assembled into a button cell.
[0065] NaV8O prepared in Examples 1 to 4 and Comparative Example 1 20 · XRD spectrum of nH2O material Figure 1 As shown in the figure, it can be seen that the material prepared by the present invention is NaV8O 20 ·nH2O.
[0066] Figure 2 The oxygen-rich NaV8O prepared in Example 3 20 SEM image of nH2O positive electrode material. It can be seen from the figure that the oxygen-rich NaV8O prepared by the present invention 20 The morphology of nH2O material is an irregular structure composed of small pieces with a size of several microns and a fluffy surface. SEM-EDS shows that the Na, V, and O elements in the sample are evenly distributed.
[0067] Figure 3 NaV8O prepared in Example 3 and Comparative Example 1 20 XPS graph of nH2O positive electrode material. It can be seen from the graph that there is an obvious sodium element signal peak in the product sample prepared by the present invention. 20 nH2O sample and oxygen-rich defect NaV8O of Example 3 20 ·V in nH2O samples 4+The molar ratios of V in the total V element are 11.98% and 33.40%, respectively, and the average valence of V is +4.88 and +4.67, respectively. 20 ·V in nH2O samples 4+ The content of vanadium increases and the average valence state of vanadium decreases, indicating that the use of EDTA-2Na as a sodium source in the synthesis process can successfully introduce oxygen vacancy defects.
[0068] Figure 4 Oxygen-rich defect NaV8O prepared in Example 3 and Comparative Example 1 20 nH2O cathode material and NaV8O 20 EPR diagram of nH2O positive electrode material. It can be seen from the figure that the oxygen-rich NaV8O prepared in Example 3 of the present invention 20 The EPR signal with a g value of ∼1.96 in the nH2O sample is obvious, which is attributed to the presence of oxygen vacancy defects, indicating the successful introduction of oxygen vacancies into the sample structure.
[0069] The constant current charge and discharge performance of the battery was tested using a BTS-5V / 10mA charge and discharge tester from Shenzhen Xinwei Company. The charge and discharge voltage range was 0.3 to 1.6V, and the current density of the cycle performance test was 1.0A / g. The cycle performance test results of the samples of Examples 1 to 4 and Comparative Example 1 are shown in FIG. Figure 5 At a current density of 1.0 A / g, the initial discharge specific capacities of Examples 1 to 4 and Comparative Example 1 were 130.4 mAh g -1 、173.1mAhg -1 、339.2mAhg -1 、165.6mAhg -1 、109.4mAhg -1 After 200 cycles, the discharge capacity is 142.8 mAh g -1 、247.0mAhg -1 、282.1mAhg -1 、229.6mAhg -1 、155.3mAhg -1 .
[0070] The constant current charge and discharge performance of the battery was tested using a BTS-5V / 10mA charge and discharge tester from Shenzhen Xinwei Company. The charge and discharge voltage range was 0.3 to 1.6V, and the current density of the cycle performance test was 0.2 to 4.0A / g. The rate performance test results of the samples of Example 3 and Comparative Example 1 are shown in Figure 2. Figure 6 As shown, the discharge specific capacity of the sample of Example 3 at 0.2A / g, 0.5A / g, 1.0A / g, 2.0A / g, 3.0A / g, and 4.0A / g is 395.0mAhg -1、364.0mAhg -1 、336.0mAhg -1 、300.4mAh g -1 、266.7mAhg -1 、234.2mAhg -1 The sample of comparative example 1 has a discharge capacity of 360.6 mAh g at 0.2 A / g, 0.5 A / g, 1.0 A / g, 2.0 A / g, 3.0 A / g, and 4.0 A / g, respectively. -1 、260.7Ahg -1 、171.9mAhg -1 、76.8mAhg -1 , 40.3mAh g -1 、21.0mAhg -1 The discharge specific capacity of Comparative Example 2 is shown in Table 1. It can be seen from the table that heat treatment of the material can improve the discharge specific capacity and show a good rate.
[0071] Table 1 Specific capacity of Example 3 and Comparative Example 2 at different current densities
[0072]
[0073] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. An oxygen-rich defect NaV8O 20 · A method for preparing a positive electrode material for nH2O aqueous zinc ion battery, characterized in that: The following steps are involved: (1) dispersing vanadium pentoxide powder in deionized water, adding hydrogen peroxide dropwise and stirring; then adding deionized water solution of disodium ethylenediaminetetraacetic acid to obtain a mixed solution; (2) subjecting the mixed solution to a hydrothermal reaction at 140 to 180° C. for 10 to 20 hours; after the reaction, centrifugation and freeze drying are performed to obtain a primary product; (3) The primary product obtained in step (2) is heat treated at 180-220° C. for 0.5-2 h to obtain oxygen-rich defective NaV8O 20 nH2O material.
2. The oxygen-rich defect NaV8O according to claim 1 20 · A method for preparing a positive electrode material for nH2O aqueous zinc ion battery, characterized in that: In the step (1), the ratio of vanadium pentoxide powder, deionized water and hydrogen peroxide is 1 g: 17.26 ml: 4.64 ml.
3. The oxygen-rich defect NaV8O according to claim 1 20 · A method for preparing a positive electrode material for nH2O aqueous zinc ion battery, characterized in that: The molar ratio of disodium ethylenediaminetetraacetate to vanadium pentoxide is 0.05-0.35:
1.
4. The oxygen-rich defect NaV8O according to claim 3 20 · A method for preparing a positive electrode material for nH2O aqueous zinc ion battery, characterized in that: The molar ratio of disodium ethylenediaminetetraacetate to vanadium pentoxide is 0.25:
1.
5. The oxygen-rich defect NaV8O according to claim 1 20 · A method for preparing a positive electrode material for nH2O aqueous zinc ion battery, characterized in that: In the step (2), the hydrothermal reaction is carried out at 160° C. for 12 hours; and in the step (3), the heat treatment is carried out at 200° C. for 1 hour.
6. An oxygen-rich defect NaV8O 20 nH2O aqueous zinc ion battery positive electrode material, characterized in that: The oxygen-rich defect NaV8O according to any one of claims 1 to 5 20 The nH2O aqueous zinc ion battery positive electrode material is prepared by the preparation method.
7. The oxygen-rich defect NaV8O according to claim 6 20 Application of nH2O aqueous zinc ion battery cathode material in aqueous zinc ion batteries.
8. The use according to claim 7, characterized in that: The aqueous zinc ion battery includes the oxygen-rich defect NaV8O 20 The electrode sheet is prepared from nH2O material, and the preparation method of the electrode sheet comprises: 20 nH2O material, conductive agent and binder are mixed with solvent, then coated on the current collector and dried to obtain an electrode sheet.
9. The use according to claim 8, characterized in that: The conductive agent is Super P, the binder is polyvinylidene fluoride, NaV8O 20 The mass ratio of nH2O material, conductive agent and binder is 7:2:1, the current collector is a stainless steel mesh, and the solvent is N-methyl-2-pyrrolidone.
10. The use according to claim 8, characterized in that: The electrode sheet, the counter electrode, the separator and the ZnSO4 electrolyte are assembled into a battery.
Citation Information
Cited By
Graphene-sodium hydrogen vanadate hydrate heterostructure material rich in oxygen vacancies, preparation method and application of graphene-sodium hydrogen vanadate hydrate heterostructure material
CN121215718A
Modified positive electrode structure, zinc-vanadium battery, and manufacturing methods thereof
EP4749711A1